Silicon carbide substrate and method for producing same
By doping and annealing the N-type silicon carbide substrate, the semi-insulating silicon carbide region is formed, which solves the problem of high production cost of semi-insulating silicon carbide wafers, improves the matching with the gallium nitride epitaxial layer and semiconductors performance of the device.
Patent Information
- Application Number
- CN202410538774.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-05
- Filing Date
- 2024-04-30
- Publication Date
- 2024-11-05
AI Technical Summary
The existing semi-insulated silicon carbide wafers are costly, which makes it difficult to meet the high resistance requirements when it is used to grow the substrate of the gallium nitride epitaxial layer, and is prone to leakage or short circuit problems, and the cost is high, which affects the semiconductor device. Production efficiency and quality.
By performing a doping process on the N-type silicon carbide substrate, a semi-insulating silicon carbide region extending from the surface to a certain depth is formed, and annealing process is carried out to reduce production costs and improve the matching between the silicon carbide substrate and the epitaxial layer. sex.
It is achieved to improve the high resistivity of the silicon carbide substrate while maintaining low costs, reduce the production cost of semiconductor devices, and improve the quality and performance of the device.
Smart Images

Figure CN118899331A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a silicon carbide substrate and a method for manufacturing the same. Background Art
[0002] Silicon carbide wafers are third-generation semiconductor materials. According to their electrical properties, silicon carbide wafers can be divided into low-resistance N-type silicon carbide wafers and high-resistance semi-insulating silicon carbide wafers. Generally speaking, N-type silicon carbide wafers have lower production costs, but they do not meet the requirements of high-resistance substrates, and components installed on them are prone to leakage or short circuit problems. Semi-insulating silicon carbide wafers have a resistance of more than 10 5 ohm cm resistivity, and is often used as a substrate for growing gallium nitride epitaxial layers. Gallium nitride is a third-generation semiconductor material. Because of its high operating frequency, it is very suitable for chargers, 5G base stations, 5G communication equipment, etc. Compared with silicon components, gallium nitride components can conduct electrons more efficiently and can withstand higher electric fields than silicon components. However, due to the high production cost of semi-insulating silicon carbide wafers, many manufacturers are committed to developing methods to reduce their production costs. Summary of the invention
[0003] The present invention provides a silicon carbide substrate and a method for manufacturing the same, the main advantage of which is that the matching between the silicon carbide substrate and the epitaxial layer above it can be improved while maintaining the low cost of the silicon carbide substrate. In this way, not only can the production cost of semiconductor devices be reduced, but also the quality and performance of semiconductor devices can be improved.
[0004] At least one embodiment of the present invention provides a silicon carbide substrate, which includes an N-type silicon carbide substrate having a first surface and a second surface opposite to the first surface. The N-type silicon carbide substrate includes a semi-insulating silicon carbide region and an N-type silicon carbide region. The semi-insulating silicon carbide region extends from the first surface to a depth into the N-type silicon carbide substrate. The semi-insulating silicon carbide region includes nitrogen and a first dopant. The first dopant includes at least one of a VB group element, a VIIA group element, argon and silicon. The N-type silicon carbide region is adjacent to the semi-insulating silicon carbide region and includes nitrogen.
[0005] At least one embodiment of the present invention provides a method for manufacturing a silicon carbide substrate, comprising the following steps. An N-type silicon carbide substrate is provided, which has a first surface and a second surface opposite to the first surface. A doping process is performed on the first surface of the N-type silicon carbide substrate to form a semi-insulating silicon carbide region in the N-type silicon carbide substrate extending from the first surface to a depth into the N-type silicon carbide substrate. The semi-insulating silicon carbide region includes nitrogen and a first dopant. The first dopant includes at least one of a VB group element, a VIIA group element, argon and silicon. An area of the N-type silicon carbide substrate that has not been subjected to the doping process includes an N-type silicon carbide region. The N-type silicon carbide region includes nitrogen. An annealing process is performed on the semi-insulating silicon carbide region.
[0006] Based on the above, the first surface of the N-type silicon carbide substrate with lower production cost can be converted into a semi-insulating silicon carbide region with high resistivity, thereby reducing the cost of producing semi-insulating silicon carbide. In some embodiments, the first surface can be optimized by an annealing process, thereby improving the epitaxy quality of a subsequent epitaxial process. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] Figures 1A to 1E is a cross-sectional schematic diagram of a method for manufacturing a silicon carbide substrate according to an embodiment of the present invention;
[0008] Figure 2 is a cross-sectional schematic diagram of a silicon carbide substrate according to another embodiment of the present invention;
[0009] Figure 3A is a flow chart of a method for manufacturing a silicon carbide substrate according to an embodiment of the present invention;
[0010] Figure 3B is a flow chart of a method for manufacturing a silicon carbide substrate according to another embodiment of the present invention. DETAILED DESCRIPTION
[0011] Figures 1A to 1E is a cross-sectional schematic diagram of a method for manufacturing a silicon carbide substrate 10 according to an embodiment of the present invention. Figure 1A , an N-type silicon carbide substrate 100 is provided. The N-type silicon carbide substrate 100 is, for example, a wafer, and has a first surface 102 and a second surface 104 opposite to the first surface 102. In some embodiments, the first surface 102 of the N-type silicon carbide substrate 100 is a silicon surface and has a relatively low surface roughness Ra, thus facilitating the subsequent formation of an epitaxial layer on the first surface 102. In some embodiments, the surface roughness Ra of the first surface 102 is less than 1 nanometer, preferably less than 0.1 nanometer. The second surface 104 of the N-type silicon carbide substrate 100 is a carbon surface.
[0012] In some embodiments, the N-type silicon carbide substrate 100 contains nitrogen. For example, the method for manufacturing the N-type silicon carbide substrate 100 includes the following steps. First, silicon carbide powder is placed at the bottom of a crystal growth furnace, and silicon carbide seeds are placed at the top of the crystal growth furnace. Then, the silicon carbide powder is sublimated in a high-temperature and closed crystal growth furnace. After the silicon carbide vapor condenses, it adheres to the silicon carbide seeds, thereby obtaining a silicon carbide ingot. Then, the silicon carbide ingot is subjected to a series of cutting processes and grinding processes to obtain a plurality of silicon carbide wafers (i.e., the N-type silicon carbide substrate 100). In this embodiment, the crystal growth furnace contains nitrogen (for example, the silicon carbide powder contains nitrogen or a gas containing nitrogen is applied to the crystal growth furnace), so the N-type silicon carbide substrate 100 obtained in the end contains nitrogen.
[0013] In some embodiments, the concentration of nitrogen in the N-type silicon carbide substrate 100 is 10 17 cm -3 Up to 10 20 cm -3 In some embodiments, the thickness T of the N-type silicon carbide substrate 100 is about 200 microns to 1000 microns. In some embodiments, the N-type silicon carbide substrate 100 includes 4H silicon carbide or 6H silicon carbide. In some embodiments, the resistivity of the N-type silicon carbide substrate 100 is 1.5×10 -2 ohm cm to 2.5×10 -2 ohm cm.
[0014] Please refer to Figure 1B , a doping process IP is performed on the first surface 102 of the N-type silicon carbide substrate 100 to form a semi-insulating silicon carbide region 110 in the N-type silicon carbide substrate 100 extending from the first surface 102 into the N-type silicon carbide substrate 100 to a depth (for example, less than or equal to 1 micron). The aforementioned depth may also be referred to as the thickness T1 of the semi-insulating silicon carbide region 110. The doping process IP implants a first dopant into the N-type silicon carbide substrate 100, so that the portion of the N-type silicon carbide substrate 100 close to the first surface 102 is modified into a semi-insulating silicon carbide region 110 with a higher resistivity. The region of the N-type silicon carbide substrate 100 that is not subjected to the doping process IP includes an N-type silicon carbide region 120. In some embodiments, the first dopant includes at least one of a VB group element (for example, niobium, vanadium, etc.), a VIIA group element (for example, fluorine, etc.), argon, and silicon. In some embodiments, the concentration of nitrogen in the N-type silicon carbide region 120 is 10 17 cm -3 Up to 10 20 cm -3 .
[0015] The concentration of the first dopant in the semi-insulating silicon carbide region 110 is greater than the concentration of nitrogen in the semi-insulating silicon carbide region 110. In some embodiments, the energy used in the doping process IP is 10 keV to 2500 keV. The doping dose of the first dopant is 10 12 Up to 5×10 15 cm -2 In some embodiments, the concentration of the first dopant in the semi-insulating silicon carbide region 110 increases closer to the first surface 102 . In some embodiments, when the first dopant includes silicon, the silicon concentration of the semi-insulating silicon carbide region 110 may be higher than the silicon concentration of the N-type silicon carbide region 120 .
[0016] Please refer to Figure 1C , an annealing process AP is performed on the semi-insulating silicon carbide region 120 or on the entire N-type silicon carbide substrate 100. The annealing process AP can be performed by high-temperature furnace annealing, laser annealing, microwave annealing, rapid annealing or other suitable methods. In some embodiments, the N-type silicon carbide substrate 100 is heated to 800°C to 2000°C (preferably 800°C to 1600°C) in a high-temperature furnace and maintained for 15 minutes to 60 minutes (preferably 20 minutes to 40 minutes). In some embodiments, the semi-insulating silicon carbide region 120 is heated by laser, and the laser can heat up to a higher temperature (for example, 1000°C to 2000°C) more quickly, so the time required for the annealing process AP can be shortened (for example, less than 10 minutes). In a preferred embodiment, the annealing process AP is a rapid annealing process, the temperature of which is 800 to 1000 degrees, and the annealing time is within one minute.
[0017] Since the semi-insulating silicon carbide region 110 additionally includes the first dopant, the resistivity of the semi-insulating silicon carbide region 110 is reduced. In some embodiments, the resistivity of the semi-insulating silicon carbide region 110 is greater than 10 5 ohm cm, for example 10 5 ohm cm to 10 12 In some embodiments, the resistivity of the N-type silicon carbide region 120 is 1.5×10 -2 ohm cm to 2.5×10 -2 In some embodiments, the resistivity of the semi-insulating silicon carbide region 110 is 10 times that of the N-type silicon carbide region 120. 6 Up to 10 13 times.
[0018] In some embodiments, the thickness T1 of the semi-insulating silicon carbide region 110 is 0.035% to 0.5% of the total thickness of the N-type silicon carbide substrate (i.e., the thickness T1 plus the thickness T2). In some embodiments, the thickness T1 of the semi-insulating silicon carbide region 110 is less than or equal to 1 micron (preferably 350 nanometers to 400 nanometers), and the thickness T2 of the N-type silicon carbide region 120 is 200 to 1000 microns. It should be noted that the thicknesses of various elements in the drawings are for illustration only and are not shown in proportion.
[0019] In some embodiments, the micro-pipe density (MPD) in the semi-insulating silicon carbide region 110 is less than 1 cm -2 In some embodiments, the basal plane defect (BPD) in the semi-insulating silicon carbide region 110 is less than 500 cm -2 In some embodiments, the threading screw dislocation (TSD) in the semi-insulating silicon carbide region 110 is less than 100 cm -2 .
[0020] Please refer to Figure 1D , forming a semi-insulating silicon carbide epitaxial layer 200 contacting the first surface 102. In the present embodiment, the semi-insulating silicon carbide region 110 formed by the doping process has a better lattice matching with the semi-insulating silicon carbide epitaxial layer 200 located thereon. Therefore, an optimized epitaxial quality can be obtained. For example, the lattice constant of the semi-insulating silicon carbide region 110 formed by the doping process is close to the lattice constant of the semi-insulating silicon carbide epitaxial layer 200 located thereon, thereby improving the epitaxial quality.
[0021] In some embodiments, the semi-insulating silicon carbide epitaxial layer 200 also includes nitrogen and the first dopant. However, the concentration of nitrogen in the semi-insulating silicon carbide region 110 is greater than the concentration of nitrogen in the semi-insulating silicon carbide epitaxial layer 200. In some embodiments, the concentration of the first dopant in the semi-insulating silicon carbide region 110 is greater than the concentration of nitrogen in the semi-insulating silicon carbide region 110 and the concentration of nitrogen in the semi-insulating silicon carbide epitaxial layer 200.
[0022] Please refer to Figure 1E A semiconductor epitaxial layer 300 is directly formed on a side of the semi-insulating silicon carbide epitaxial layer 200 opposite to the N-type silicon carbide substrate 100 , thereby obtaining a silicon carbide substrate 10 .
[0023] In some embodiments, the material of the semiconductor epitaxial layer 300 includes a nitride containing at least one of aluminum and gallium, such as AlInGaN, AlN, AlGaN, GaN, etc.
[0024] In some embodiments, the thickness t of the semiconductor epitaxial layer 300 is greater than 4 micrometers, preferably greater than 10 micrometers, such as 10 micrometers to 20 micrometers.
[0025] In some embodiments, the semiconductor epitaxial layer 300 includes a second dopant. In some embodiments, the second dopant includes, for example, at least one of C, Fe, Co, Mn, Cr, V, and Ni. In some embodiments, the concentration of the second dopant in the semiconductor epitaxial layer 300 is greater than 10 16 cm -3 , for example, 10 16 cm -3 Up to 10 18 cm -3 In some embodiments, the resistivity of the semiconductor epitaxial layer 300 is greater than 10 5 ohm cm, for example 10 5 ohm cm to 10 12 In some embodiments, the semiconductor epitaxial layer 300 formed by the epitaxial process has excellent crystallinity. For example, the half-width of the (002) plane of the semiconductor epitaxial layer 300 detected by an X-ray diffractometer is less than 220 arcsec.
[0026] Figure 2 FIG. 1 is a cross-sectional schematic diagram of a silicon carbide substrate 20 according to another embodiment of the present invention. It must be noted that: Figure 2 The implementation examples are used Figures 1A to 1E The component numbers and partial contents of the embodiments are the same, wherein the same or similar numbers are used to represent the same or similar components, and the description of the same technical contents is omitted. The description of the omitted parts can be referred to the aforementioned embodiments, and will not be repeated here.
[0027] Figure 2 The silicon carbide substrate 20 and Figure 1E The difference between the silicon carbide substrate 10 and the silicon carbide substrate 10 is that the silicon carbide substrate 20 does not include the semi-insulating silicon carbide epitaxial layer 200. In the silicon carbide substrate 20, the semiconductor epitaxial layer 300 is directly formed on the semi-insulating silicon carbide region 110 of the N-type silicon carbide substrate 100 (ie, on the first surface 102).
[0028] In this embodiment, the semi-insulating silicon carbide region 110 formed by the doping process has better lattice matching with the semiconductor epitaxial layer 300 located thereon. Therefore, an optimized epitaxial quality can be obtained. For example, the lattice constant of the semi-insulating silicon carbide region 110 formed by the doping process is close to the lattice constant of the semiconductor epitaxial layer 300 located thereon, thereby improving the epitaxial quality.
[0029] In addition, compared with the embodiment in which a semi-insulating silicon carbide epitaxial layer 200 is additionally formed on the N-type silicon carbide substrate 100, Figure 2 The silicon carbide substrate 20 has a lower production cost.
[0030] Figure 3A is a flow chart of a method for manufacturing a silicon carbide substrate according to an embodiment of the present invention. Figure 3A Step S1 and Figure 1A , providing an N-type silicon carbide substrate 100. Please refer to Figure 3A Step S2 and Figure 1B , a doping process IP is performed on the first surface 110a of the N-type silicon carbide substrate 100 to define a semi-insulating silicon carbide region 120 and an N-type silicon carbide region 110 in the N-type silicon carbide substrate 100. Please refer to Figure 3A Step S3 is the same as Figure 1C , an annealing process AP is performed on the N-type silicon carbide substrate 100. Please refer to Figure 3A Step S4 is the same as Figure 1D , forming a semi-insulating silicon carbide epitaxial layer 200 on the semi-insulating silicon carbide region 110. Please refer to Figure 3A Step S5 and Figure 1E , a semiconductor epitaxial layer 300 is formed on the semi-insulating silicon carbide epitaxial layer 200 .
[0031] Figure 3B is a flow chart of a method for manufacturing a silicon carbide substrate according to another embodiment of the present invention. Figure 3A The process shown in Figure 3B Specifically, after the annealing process AP is performed on the N-type silicon carbide substrate 100 (eg, Figure 3B Step S3 is the same as Figure 1C As shown), a semiconductor epitaxial layer 300 is formed on the semi-insulating silicon carbide region 110, as shown Figure 3B Step S4-1 and Figure 2 shown.
[0032] The silicon carbide substrate of the present invention is described in detail below through examples. However, the following examples are not intended to limit the present invention.
[0033] Example 1
[0034] An N-type silicon carbide substrate with a thickness of 322 microns is provided, wherein the resistivity of the N-type silicon carbide substrate is 2×10 -2 The silicon surface of the N-type silicon carbide substrate is doped with silicon, the dopant is 100 keV, and the doping dose is 5×10 15 cm -2After forming a semi-insulating silicon carbide region with a depth of 350nm in the N-type silicon carbide substrate by doping, a rapid annealing process is performed on the N-type silicon carbide substrate at a temperature of 800°C and an annealing time of one minute. The resistivity of the semi-insulating silicon carbide region obtained is 5.7×10 7 ohm cm.
[0035] Example 2
[0036] An N-type silicon carbide substrate with a thickness of 322 microns is provided, wherein the resistivity of the N-type silicon carbide substrate is 2×10 -2 The silicon surface of the N-type silicon carbide substrate is doped with silicon, the dopant is 100 keV, and the doping dose is 5×10 15 cm -2 After forming a semi-insulating silicon carbide region with a depth of 400nm in the N-type silicon carbide substrate by doping, a rapid annealing process is performed on the N-type silicon carbide substrate at a temperature of 1000°C and an annealing time of one minute. The resistivity of the semi-insulating silicon carbide region obtained is 1.54×10 8 ohm cm.
[0037] In summary, in an embodiment of the present invention, a portion of an N-type silicon carbide substrate is modified into a semi-insulating silicon carbide region by a doping process. Since the semi-insulating silicon carbide region has a high lattice matching with the epitaxial layer to be formed thereon, the quality of the epitaxial layer can be improved. In addition, compared with directly manufacturing a whole piece of semi-insulating silicon carbide substrate, forming a semi-insulating silicon carbide region in an N-type silicon carbide substrate by the method of an embodiment of the present invention has a lower production cost.
Claims
1. A silicon carbide substrate, characterized in that: include: An N-type silicon carbide substrate having a first surface and a second surface opposite to the first surface, wherein the N-type silicon carbide substrate comprises: a semi-insulating silicon carbide region extending from the first surface into the N-type silicon carbide substrate to a depth, the semi-insulating silicon carbide region comprising nitrogen and a first dopant, the first dopant comprising at least one of a VB group element, a VIIA group element, argon and silicon; and The N-type silicon carbide region is adjacent to the semi-insulating silicon carbide region and includes nitrogen. 2 . The silicon carbide substrate according to claim 1 , wherein the first dopant comprises at least one of niobium, vanadium, fluorine, argon, and silicon.
3. The silicon carbide substrate according to claim 1, further comprising: A semi-insulating silicon carbide epitaxial layer, contacting the first surface; as well as The semiconductor epitaxial layer contacts a side of the semi-insulating silicon carbide epitaxial layer opposite to the N-type silicon carbide substrate. 4 . The silicon carbide substrate according to claim 3 , wherein the semi-insulating silicon carbide epitaxial layer includes nitrogen, and a concentration of nitrogen in the semi-insulating silicon carbide region is greater than a concentration of nitrogen in the semi-insulating silicon carbide epitaxial layer. 5 . The silicon carbide substrate according to claim 1 , wherein a concentration of the first dopant in the semi-insulating silicon carbide region is greater than a concentration of nitrogen in the semi-insulating silicon carbide region. The silicon carbide substrate according to claim 1 , wherein the first surface is a silicon surface, and a roughness Ra of the first surface is less than 1 nanometer. 7 . The silicon carbide substrate according to claim 1 , wherein a thickness of the semi-insulating silicon carbide region is 0.035% to 0.5% of a total thickness of the N-type silicon carbide substrate. 8 . The silicon carbide substrate according to claim 7 , wherein the thickness of the semi-insulating silicon carbide region is less than or equal to 1 micrometer, and the thickness of the N-type silicon carbide region is 200 to 1000 micrometers.
9. The silicon carbide substrate according to claim 1, wherein the resistivity of the semi-insulating silicon carbide region is 10 times that of the N-type silicon carbide region. 6 Up to 10 13 times.
10. The silicon carbide substrate according to claim 9, wherein the resistivity of the semi-insulating silicon carbide region is greater than 10 5 ohm cm, and the resistivity of the N-type silicon carbide region is 1.5×10 -2 ohm cm to 2.5×10 -2 ohm cm.
11. A method for manufacturing a silicon carbide substrate, characterized in that: include: Providing an N-type silicon carbide substrate, the N-type silicon carbide substrate having a first surface and a second surface opposite to the first surface; Performing a doping process on the first surface of the N-type silicon carbide substrate to form a semi-insulating silicon carbide region in the N-type silicon carbide substrate extending from the first surface into the N-type silicon carbide substrate to a depth, wherein the semi-insulating silicon carbide region includes nitrogen and a first dopant, the first dopant includes at least one of a VB group element, a VIIA group element, argon, and silicon, and wherein a region of the N-type silicon carbide substrate that is not subjected to the doping process includes an N-type silicon carbide region, and the N-type silicon carbide region includes nitrogen; and An annealing process is performed on the semi-insulating silicon carbide region.
12. The manufacturing method according to claim 11, further comprising: directly forming a semi-insulating silicon carbide epitaxial layer on the first surface; as well as A semiconductor epitaxial layer is directly formed on a side of the semi-insulating silicon carbide epitaxial layer opposite to the N-type silicon carbide substrate.
13. The manufacturing method according to claim 11, further comprising: A semiconductor epitaxial layer is directly formed on the first surface.