High-efficiency PERC battery based on surface passivation and preparation process thereof

By adopting double-layer passivation technology and high-transparent indium tin oxide film in solar cells, the problem of poor passivation effect on the back is solved, the photoelectric conversion efficiency and battery stability are improved, the surface reflectivity is reduced, and the battery is improved. Performance at high temperatures.

CN118899347APending Publication Date: 2024-11-05CECEP SOLAR ENERGY TECH (ZHENJIANG) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410944286.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing solar cells have poor passivation effect on the back, resulting in low light absorption and insufficient battery efficiency. There is a deep energy-level trap capture effect in the local thinning area, affecting the conversion efficiency.

Method used

The passivation layer is adopted by double-layer passivation technology, including the bottom alumina passivation layer and the top fluorine-doped alumina passivation layer, and a highly transparent tin-oxide indium film is formed on the surface. The passivation layer is improved by sol-gel method and heat treatment. quality and stability.

Benefits of technology

It improves the photoelectric conversion efficiency, reduces carrier recombination, enhances the long-term stability and durability of the battery, reduces the surface reflectivity, and improves the performance of the battery in high temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899347A_ABST
    Figure CN118899347A_ABST
Patent Text Reader

Abstract

The surface passivation-based high-efficiency PERC battery comprises a silicon substrate, a phosphorus layer emitter and a front surface silicon nitride passivation layer are sequentially arranged on the front surface of the silicon substrate, and a front surface metal silver electrode is arranged in the front surface silicon nitride passivation layer; double passivation layers are sequentially arranged on the back surface of the silicon substrate, the bottom layer of the double passivation layers is an aluminum oxide passivation layer, and the outer layer of the double passivation layers is a fluorine-doped aluminum oxide passivation layer; and indium tin oxide films fixed by a sol-gel method are arranged on the surfaces of the double-layer passivation layer and the silicon nitride passivation layer. Compared with an existing PERC cell, the mode of double-layer passivation and the high-transparency indium tin oxide thin film is introduced in the scheme, the photoelectric conversion efficiency can be improved, and recombination of carriers on the surface can be reduced. And heat treatment after fluorination treatment can stabilize the structure of the passivation layer and enhance the long-term stability and durability of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This article relates to a high-efficiency PERC cell based on surface passivation and its preparation process. Background Art

[0002] The photovoltaic industry is experiencing rapid growth as demand for renewable energy increases. Currently, most commercially used solar cells use crystalline silicon as the base material. In order to increase conversion efficiency and reduce manufacturing costs, new designs and technologies need to be developed to improve existing solar cell structures.

[0003] Higher light absorption can be achieved by local thinning of the back side, and the back field performance can be improved by doping, thereby further improving the conversion efficiency. However, due to the presence of the back metal contact, good back passivation effect is usually not obtained. In addition, due to the defects at the interface between the local thinning area and the unprocessed area, deep energy level trap capture effect is prone to occur in the local thinning area.

[0004] The development of surface passivation technology is key to improving the performance of solar cells, especially in suppressing the recombination of surface electron holes. Aluminum oxide (Al2O3) and other materials such as silicon nitride (SiNx) have been widely used as passivation layers. These materials can effectively reduce the surface defect density, but there is room for further improvement in passivation quality and efficiency. Summary of the invention

[0005] In order to solve the above problems, this solution provides a high-efficiency PERC cell structure based on double-layer passivation to further improve light utilization, and proposes a preparation process for this cell structure.

[0006] A high-efficiency PERC cell based on surface passivation comprises a silicon substrate, wherein a phosphorus layer emitter and a front surface silicon nitride passivation layer are sequentially arranged on the front side of the silicon substrate, and a front surface metal silver electrode is arranged in the front surface silicon nitride passivation layer; a double-layer passivation layer is sequentially arranged on the back side of the silicon substrate, wherein the bottom layer of the double-layer passivation layer is an aluminum oxide passivation layer, and the outer layer is a fluorine-doped aluminum oxide passivation layer; and an indium tin oxide film fixed by a sol-gel method is arranged on the surfaces of the double-layer passivation layer and the silicon nitride passivation layer.

[0007] A preparation process of a high-efficiency PERC cell based on surface passivation comprises the following steps:

[0008] S1: Preparation of silicon substrate

[0009] Clean the silicon substrate, remove the dirt and oxide layer on the surface, and obtain the surface concave shape by etching on the back of the silicon substrate;

[0010] S2: Preparation of the bottom passivation layer on the reverse side

[0011] Depositing an aluminum oxide passivation layer on the back side of the silicon substrate with a surface depression shape by chemical vapor deposition or atomic layer deposition;

[0012] S3: Fluorination treatment

[0013] Performing fluorination treatment on the aluminum oxide passivation layer, and performing heat treatment after the fluorination is completed to stabilize the structure of the fluorine-doped aluminum oxide passivation layer;

[0014] S4. Front side processing of silicon substrate

[0015] A front surface silicon nitride passivation layer is provided on the front surface of the silicon substrate;

[0016] S5. Preparation of Indium Tin Oxide Thin Film

[0017] The indium tin oxide precursor solution is coated on the passivated silicon substrate by a sol-gel method, a preliminary heat treatment is performed at a certain temperature to evaporate the solvent and solidify the sol layer, and a final sintering is performed at a higher temperature to form a uniform and highly conductive indium tin oxide film;

[0018] S6: Electrode Formation

[0019] Metal grid lines are formed on the indium tin oxide film using a screen printing technique, followed by an annealing process to improve contact.

[0020] Double passivation layer - A double passivation layer is applied on the back of the cell. The bottom layer uses a traditional aluminum oxide (Al2O3) layer to achieve good passivation effect, and the top layer uses a new fluorine-doped aluminum oxide (Al2O3:F) layer to further improve the surface passivation quality.

[0021] Double passivation layer design:

[0022] First layer: Aluminum oxide passivation layer (Al2O3)

[0023] Material selection: Choose a high purity aluminum source and an oxidant, such as high concentration oxygen or ozone.

[0024] Process steps: A uniform and dense aluminum oxide layer is formed on the surface of the silicon substrate by chemical vapor deposition (CVD) or atomic layer deposition (ALD) technology. CVD or ALD technology can achieve precise thickness control and high-quality passivation effect.

[0025] Second layer: Fluorine-doped aluminum oxide passivation layer (Al2O3:F)

[0026] Material selection: On the basis of the aluminum oxide layer, the passivation quality is further improved by doping with fluorine. The fluorine source can be hydrogen fluoride (HF) or ammonium fluoride (NH4F).

[0027] Process steps:

[0028] After the first layer of aluminum oxide is formed, a fluorination treatment is performed, and fluorine element can be introduced into the aluminum oxide layer by an immersion method or a CVD method.

[0029] The chemical stability and passivation effect of the passivation layer are ensured by precisely controlling the fluorine doping concentration and processing time.

[0030] Processing steps:

[0031] Substrate cleaning: First, the silicon substrate is thoroughly cleaned to remove oil, oxide layer and other contaminants on the surface to ensure good bonding between the subsequent passivation layer and the silicon substrate.

[0032] The first passivation layer is formed:

[0033] Set the process parameters of CVD or ALD, such as temperature, pressure, gas flow, etc.

[0034] Under controlled conditions, a uniform aluminum oxide layer is formed on the surface of the silicon substrate.

[0035] Fluoridation treatment:

[0036] The first aluminum oxide layer is subjected to fluorination treatment, and the fluorine doping concentration can be controlled by adjusting the concentration of HF or NH4F and the treatment time.

[0037] Interlayer passivation effect test:

[0038] The quality and thickness of the passivation layer were tested by X-ray photoelectron spectroscopy (XPS) and scanning electron microscopy (SEM).

[0039] Final passivation layer formation:

[0040] After the fluorination treatment, post-treatment such as heat treatment is performed to stabilize the structure of the fluorine-doped layer.

[0041] Performance evaluation:

[0042] The surface passivation effect of the double passivation layer was evaluated, and parameters such as the dark current density (J0) and saturation current density (Jsc) of the battery were tested.

[0043] Furthermore, in S2, an aluminum oxide passivation layer is deposited by chemical vapor deposition, wherein the deposition process is as follows:

[0044] S21, using organic solvents and ultrasonic cleaning to remove grease, dust and other impurities on the back of the silicon substrate;

[0045] S22, selecting argon or nitrogen as a carrier gas, selecting a mixed gas of an aluminum compound and oxygen as a reaction gas, and introducing them into the container;

[0046] S23. After the introduction, a chemical reaction occurs on the surface of the silicon substrate to generate aluminum oxide. After the deposition is completed, the temperature inside the container is lowered, the reaction gas is exhausted, and nitrogen is introduced for atmosphere replacement.

[0047] High light transmittance contact material - Select materials with high light transmittance and good electrical conductivity as the front contact material of the battery to reduce light absorption loss.

[0048] Among them, the transparent material with high light transmittance is indium tin oxide, which has high light transmittance and high electrical conductivity.

[0049] Preparation method: Sol-gel method:

[0050] Preparation of metal organic compound solutions containing indium and tin, usually using alkoxides or acetates as precursors.

[0051] A uniform precursor film is formed through a sol-gel reaction, and then heat-treated at high temperature to obtain an ITO thin film.

[0052] This approach allows for fine control over the film's composition and microstructure.

[0053] Furthermore, the preparation of the indium tin oxide precursor solution in S5 includes the following steps: preparing tin acetate Sn(Ac)4 and indium acetate In(Ac)3 as raw materials, and selecting an organic solvent as the solvent; adding a certain amount of acetic acid or sodium acetate, adjusting the pH value to between 2-5, adding sodium hydroxide or ammonium hydroxide as a catalyst to promote the polymerization reaction, and aging at room temperature to form a uniform sol.

[0054] Furthermore, the organic solvent is selected from ethanol, isopropanol or acetone.

[0055] In S3, fluorine element is introduced by immersion method or CVD method to complete the fluorination reaction.

[0056] In S4, after the front side of the silicon substrate is cleaned, it is oxidized in oxygen at a certain temperature to form a silicon dioxide protective layer, and then a phosphorus-containing substance is used as a diffusion source, and is deposited on the front area of ​​the silicon substrate at a temperature of 800-1100 degrees Celsius. After the deposition is completed, rapid thermal annealing is performed to activate the phosphorus atoms to form an n-type doped area; after cleaning, a front surface silicon nitride passivation layer is attached. The reaction temperature is 800-1100 degrees Celsius, and a silicon dioxide protective layer is formed on the front side of the silicon substrate. After the entire n-type doped area is formed, the silicon substrate is cleaned again, and then a front surface silicon nitride passivation layer is attached, and the attachment temperature is controlled at 300°C to 400°C.

[0057] In order to maintain the distribution of fluorine atoms in the alumina lattice for a certain period of time, after the preparation of the reverse bottom passivation layer and the fluorine-doped alumina passivation layer, a heat treatment is performed to maintain stability, and the heat treatment temperature is 400-600 degrees Celsius.

[0058] Beneficial effects:

[0059] Compared with existing PERC cells, the introduction of double-layer passivation and highly transparent indium tin oxide film in this solution can improve the photoelectric conversion efficiency and reduce the recombination of carriers on the surface. In addition, the heat treatment after fluorination can stabilize the passivation layer structure and enhance the long-term stability and durability of the cell.

[0060] Compared with ordinary batteries, the surface passivation layer can effectively isolate moisture and impurities in the air, reducing the negative impact on battery performance. The life span is also improved to a certain extent, and the aluminum oxide layer deposited on the back and the silicon nitride layer on the front have excellent thermal resistance, which helps the battery to operate stably in high temperature environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] Figure 1 It is a preparation flow chart of high-efficiency PERC cells based on surface passivation. DETAILED DESCRIPTION

[0062] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with embodiments and drawings. The embodiments are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.

[0063] Embodiment 1:

[0064] A high-efficiency PERC cell based on surface passivation comprises a silicon substrate, wherein a phosphorus layer emitter and a front surface silicon nitride passivation layer are sequentially arranged on the front side of the silicon substrate, and a front surface metal silver electrode is arranged in the front surface silicon nitride passivation layer; a double-layer passivation layer is sequentially arranged on the back side of the silicon substrate, wherein the bottom layer of the double-layer passivation layer is an aluminum oxide passivation layer, and the outer layer is a fluorine-doped aluminum oxide passivation layer; and an indium tin oxide film fixed by a sol-gel method is arranged on the surfaces of the double-layer passivation layer and the silicon nitride passivation layer.

[0065] Specifically, the high-efficiency PERC cell based on surface passivation provided in the embodiment of the present application can effectively reduce light reflection and avoid waste of photons by setting a double passivation layer on the back of the silicon substrate, thereby increasing the light absorption capacity of the cell, allowing more photons to be absorbed and converted into current, thereby improving the conversion efficiency of the cell and solving the problem of high surface reflectivity of existing cells.

[0066] The thickness of the silicon nitride passivation layer on the front surface is less than or equal to 5 microns. The thickness of the double-layer passivation layer is greater than or equal to 30 microns. The area of ​​the metal silver electrode on the front surface is less than or equal to 5% of the surface area of ​​the silicon substrate.

[0067] The oxygen / aluminum ratio of the aluminum oxide passivation layer is 1.0 to 1.1. The fluorine content of the fluorine-doped aluminum oxide passivation layer is less than or equal to 10%. The thickness of the indium tin oxide film is less than or equal to 5 microns.

[0068] Accordingly, the embodiment of the present application also provides a preparation process of a high-efficiency PERC cell based on surface passivation, comprising the following steps:

[0069] S1: Preparation of silicon substrate: Clean the silicon substrate, remove the dirt and oxide layer on the surface, and obtain the surface concave shape by etching on the back of the silicon substrate;

[0070] S2: Deposit an aluminum oxide passivation layer by chemical vapor deposition, wherein the deposition process is as follows:

[0071] Use organic solvents and ultrasonic cleaning to remove grease, dust and other impurities on the back of the silicon substrate; select argon as the carrier gas, and select a mixed gas containing aluminum compounds and oxygen as the reaction gas, and introduce it into the container; after introduction, a chemical reaction occurs on the surface of the silicon substrate to generate aluminum oxide, and after deposition is completed; lower the temperature inside the container, exhaust the reaction gas, and introduce nitrogen for atmosphere replacement.

[0072] S3: Fluorination treatment is performed on the aluminum oxide passivation layer, and after the fluorination is completed, heat treatment is performed to stabilize the structure of the fluorine-doped aluminum oxide passivation layer;

[0073] S4, front surface treatment of the silicon substrate: a front surface silicon nitride passivation layer is provided on the front surface of the silicon substrate;

[0074] S5. Preparation of indium tin oxide thin film: Use the sol-gel method to coat the indium tin oxide precursor solution on the passivated silicon substrate, perform preliminary heat treatment at a certain temperature to evaporate the solvent and solidify the sol layer, and finally sinter at a higher temperature to form a uniform, highly conductive indium tin oxide thin film.

[0075] S6: Electrode formation Metal grid lines are formed on the indium tin oxide film using a screen printing technique, followed by an annealing process to improve contact.

[0076] The high-efficiency PERC cell based on surface passivation provided in the embodiment of the present application can effectively reduce light reflection by setting a double passivation layer on the back of the silicon substrate, thereby avoiding waste of photons and increasing the light absorption capacity of the cell, so that more photons are absorbed and converted into current, thereby improving the conversion efficiency of the cell and solving the problem of high surface reflectivity of existing cells.

[0077] Compared with traditional monocrystalline silicon solar cells, the PERC cell using double-layer passivation technology in Example 1 can increase the cell efficiency to 25% to 28%. The contact resistance is reduced to below 1 milliohm square. The reflectivity of the front surface of the cell is reduced to less than about 3%, and the temperature coefficient of the cell is reduced to -0.3% / °C. And in the extremely high temperature test, the ambient temperature is set to 80-90 degrees Celsius and the relative humidity is 85%. After 1000 hours of continuous power generation, the efficiency attenuation is 0.75%, the power attenuation is 7%, and the open circuit voltage (Voc) decrease rate is 10mV / °C. It can be seen that the high temperature tolerance of the product has been significantly improved.

[0078] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A high-efficiency PERC cell based on surface passivation, characterized in that: The invention comprises a silicon substrate, wherein a phosphorus layer emitter and a front surface silicon nitride passivation layer are sequentially arranged on the front side of the silicon substrate, and a front surface metal silver electrode is arranged in the front surface silicon nitride passivation layer; a double-layer passivation layer is sequentially arranged on the back side of the silicon substrate, wherein the bottom layer of the double-layer passivation layer is an aluminum oxide passivation layer, and the outer layer is a fluorine-doped aluminum oxide passivation layer; The surfaces of the double-layer passivation layer and the silicon nitride passivation layer are provided with an indium tin oxide film fixed by a sol-gel method.

2. A preparation process for a high-efficiency PERC cell based on surface passivation, characterized in that: The following steps are involved: S1: Preparation of silicon substrate Clean the silicon substrate, remove the dirt and oxide layer on the surface, and obtain the surface concave shape by etching on the back of the silicon substrate; S2: Preparation of the bottom passivation layer on the reverse side Depositing an aluminum oxide passivation layer on the back side of the silicon substrate with a surface depression shape by chemical vapor deposition or atomic layer deposition; S3: Fluorination treatment Performing fluorination treatment on the aluminum oxide passivation layer, and performing heat treatment after the fluorination is completed to stabilize the structure of the fluorine-doped aluminum oxide passivation layer; S4. Front side processing of silicon substrate A front surface silicon nitride passivation layer is provided on the front surface of the silicon substrate; S5. Preparation of Indium Tin Oxide Thin Film The indium tin oxide precursor solution is coated on the passivated silicon substrate by a sol-gel method, a preliminary heat treatment is performed at a certain temperature to evaporate the solvent and solidify the sol layer, and a final sintering is performed at a higher temperature to form a uniform and highly conductive indium tin oxide film; S6: Electrode Formation Metal grid lines are formed on the indium tin oxide film using a screen printing technique, followed by an annealing process to improve contact.

3. The preparation process of a high-efficiency PERC cell based on surface passivation according to claim 2, characterized in that: In S2, an aluminum oxide passivation layer is deposited by chemical vapor deposition, wherein the deposition process is as follows: S21, using organic solvents and ultrasonic cleaning to remove grease, dust and other impurities on the back of the silicon substrate; S22, selecting argon or nitrogen as a carrier gas, selecting a mixed gas of an aluminum compound and oxygen as a reaction gas, and introducing them into the container; S23. After the introduction, a chemical reaction occurs on the surface of the silicon substrate to generate aluminum oxide. After the deposition is completed, the temperature inside the container is lowered, the reaction gas is exhausted, and nitrogen is introduced for atmosphere replacement.

4. A preparation process for a high-efficiency PERC cell based on surface passivation according to any one of claims 2 to 3, characterized in that: The preparation of the indium tin oxide precursor solution in S5 includes the following steps: preparing tin acetate Sn(Ac)4 and indium acetate In(Ac)3 as raw materials, and selecting an organic solvent as the solvent; adding a certain amount of acetic acid or sodium acetate, adjusting the pH value to between 2-5, adding sodium hydroxide or ammonium hydroxide as a catalyst to promote the polymerization reaction, and aging at room temperature to form a uniform sol.

5. The preparation process of a high-efficiency PERC cell based on surface passivation according to claim 4, characterized in that: The organic solvent is ethanol, isopropanol or acetone.

6. The process for preparing a high-efficiency PERC cell based on surface passivation according to claim 2, characterized in that: After the preparation of the reverse bottom passivation layer and the fluorine-doped aluminum oxide passivation layer is completed, heat treatment is performed to maintain stability, and the heat treatment temperature is 400-600 degrees Celsius.

7. The process for preparing a high-efficiency PERC cell based on surface passivation according to claim 2, characterized in that: In S3, fluorine element is introduced by immersion method or CVD method to complete the fluorination reaction.

8. The process for preparing a high-efficiency PERC cell based on surface passivation according to claim 2, characterized in that: In S4, after the front side of the silicon substrate is cleaned, it is oxidized in oxygen at a certain temperature to form a silicon dioxide protective layer, and then a phosphorus-containing substance is used as a diffusion source and deposited on the front side area of ​​the silicon substrate at a temperature of 800-1100 degrees Celsius. After the deposition is completed, rapid thermal annealing is performed to activate the phosphorus atoms to form an n-type doped area; after cleaning, a silicon nitride passivation layer is attached to the front surface.

9. The process for preparing a high-efficiency PERC cell based on surface passivation according to claim 8, characterized in that: The reaction temperature is 800-1100 degrees Celsius, and a silicon dioxide protective layer is formed on the front side of the silicon substrate.

10. The process for preparing a high-efficiency PERC cell based on surface passivation according to claim 8, characterized in that: After the entire n-type doped region is formed, the silicon substrate is cleaned again, and then a front surface silicon nitride passivation layer is attached, and the attachment temperature is controlled at 300°C to 400°C.