Composite positive electrode material containing long / short-range conductive agent as well as preparation method and application of composite positive electrode material

By using long/short range conductive agents in lithium cobalt oxide positive electrode materials to form a conductive network, the problem of low conductivity of LiCoO2 materials in high power scenarios is solved, and the rate performance and structural stability are significantly improved.

CN118899440AActive Publication Date: 2024-11-05INST OF ELECTRICAL ENG CHINESE ACAD OF SCI

Patent Information

Application Number
CN202410642259.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-23
Publication Date
2024-11-05
Estimated Expiration
2044-05-23

AI Technical Summary

Technical Problem

Lithium cobalt oxide (LiCoO2) positive electrode material exhibits poor electron and ionic conductivity in high power scenarios, and is prone to side reactions with the electrolyte during charging and discharging, affecting its rate performance.

Method used

Using composite positive electrode materials containing long/short-range conductive agents, the positive electrode active particles are connected through physical adsorption to form a conductive network, and the positive electrode active particles are filled with zero-dimensional short-range conductive agents and one-dimensional long-range conductive agents (such as carbon black and gas-phase-grown carbon fibers) The gaps between them form a conductive network and improve the conductivity of electrons and ions.

Benefits of technology

The electron and ion conductivity of the positive electrode material is significantly improved, structural stability and rate performance are improved, better electron and ion transmission is achieved, and the cycle life of the electrode is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899440A_ABST
    Figure CN118899440A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium ion batteries, and particularly relates to a composite positive electrode material containing a long / short-range conductive agent as well as a preparation method and application of the composite positive electrode material. The material comprises positive active particles, a zero-dimensional short-range conductive agent which is connected with the adjacent positive active particles through a physical adsorption effect, and a one-dimensional long-range conductive agent which is connected with the positive active particles through a physical adsorption effect, gaps among the positive active particles are filled with a conductive network formed by a zero-dimensional short-range conductive agent and a one-dimensional long-range conductive agent; the zero-dimensional short-range conductive agent has a nano spherical structure; the one-dimensional long-range conductive agent has a one-dimensional linear structure. The positive electrode active material has a long-range / short-range composite conductive network which can be tightly filled among active particles, so that the electronic and ionic conductivity and structural stability of the positive electrode active material are remarkably improved, and excellent rate capability is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a composite positive electrode material containing a long / short range conductive agent, and a preparation method and application thereof. Background Art

[0002] Lithium cobalt oxide (LiCoO2) is a commercially mature cathode material with a theoretical specific capacity of up to 270 mAh g -1 , and has achieved great success in consumer electronics such as laptops, mobile phones, and mobile power supplies. However, LiCoO2 materials only exert about half of their theoretical specific capacity in the safe cutoff voltage range of 3.0 to 4.2 V, and their poor electronic and ionic conductivity limits their application in high-power scenarios. For example, at room temperature, the electronic conductivity of LiCoO2 materials is as low as 5×10 -8 S cm -1 , which is much lower than the electronic conductivity of NCM 811 material, which is 4.1×10 -3 S cm -1 ; and the ionic conductivity of LiCoO2 material is only 2.3×10 -7 S cm -1 , while NCM 811 material reaches 6.3×10 -3 S cm -1 .

[0003] Therefore, whether in terms of electronic conductivity or ionic conductivity, LiCoO2 material exhibits poor rate performance among existing positive electrode materials. At the same time, during the charge and discharge cycle, the surface of LiCoO2 material easily undergoes side reactions with the electrolyte to form impurities such as Li2CO3 and LiOH with low conductivity, further affecting the rate performance of LiCoO2 positive electrode material. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a composite positive electrode material containing a long / short range conductive agent and a preparation method and application thereof, which can significantly improve the electronic and ionic conductivity and structural stability of the positive electrode active material, thereby achieving excellent rate performance.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] The present invention provides a composite positive electrode material containing a long / short-range conductive agent, comprising: positive electrode active particles, a zero-dimensional short-range conductive agent connecting adjacent positive electrode active particles by physical adsorption, and a one-dimensional long-range conductive agent connecting positive electrode active particles by physical adsorption, wherein the gaps between the positive electrode active particles are filled with a conductive network formed by the zero-dimensional short-range conductive agent and the one-dimensional long-range conductive agent;

[0007] The zero-dimensional short-range conductive agent has a nano-spherical structure;

[0008] The one-dimensional long-range conductive agent has a one-dimensional linear structure.

[0009] Preferably, the zero-dimensional short-range conductive agent includes one or more of carbon black, conductive graphite and Ketjen black.

[0010] Preferably, the one-dimensional long-range conductive agent comprises vapor-grown carbon fibers and / or carbon nanotubes; the aspect ratio L / D of the vapor-grown carbon fibers is ≥30:1, and the aspect ratio L / D of the carbon nanotubes is ≥1000:1.

[0011] Preferably, the positive electrode active particles include one or more of lithium cobalt oxide ternary material, lithium iron phosphate ternary material, lithium nickel oxide ternary material, nickel cobalt manganese ternary material and nickel cobalt aluminum ternary material.

[0012] Preferably, the mass ratio of the one-dimensional long-range conductive agent to the zero-dimensional short-range conductive agent is (1-4):(1-4).

[0013] The present invention also provides a method for preparing the composite positive electrode material containing the long / short range conductive agent described in the above technical solution, comprising the following steps:

[0014] The one-dimensional long-range conductive agent, the zero-dimensional short-range conductive agent and the organic solvent are mixed, and water bath ultrasonication is performed to obtain a conductive agent dispersion liquid;

[0015] The conductive agent dispersion and positive electrode active particles are mixed and ball milled to obtain the composite positive electrode material containing the long / short range conductive agent.

[0016] Preferably, the temperature of the water bath ultrasound is ≤20°C; the time of the water bath ultrasound is 5 to 60 minutes; and the power of the water bath ultrasound is 450 to 600W.

[0017] Preferably, the ball-to-material ratio of the ball mill is 1:1-20; the rotation speed of the ball mill is 100-500 rpm; and the time of the ball mill is 30-720 min.

[0018] The present invention also provides the use of the composite positive electrode material containing the long / short-range conductive agent described in the above technical solution or the composite positive electrode material containing the long / short-range conductive agent prepared by the preparation method described in the above technical solution in a lithium ion battery.

[0019] The present invention also provides a lithium-ion battery comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the active material in the positive electrode is the composite positive electrode material containing a long / short-range conductive agent as described in the above technical solution or the composite positive electrode material containing a long / short-range conductive agent prepared by the preparation method as described in the above technical solution.

[0020] The present invention provides a composite positive electrode material containing a long / short-range conductive agent, including: positive electrode active particles, a zero-dimensional short-range conductive agent connecting adjacent positive electrode active particles by physical adsorption, and a one-dimensional long-range conductive agent connecting positive electrode active particles by physical adsorption, wherein the gaps between the positive electrode active particles are filled with a conductive network formed by the zero-dimensional short-range conductive agent and the one-dimensional long-range conductive agent; the zero-dimensional short-range conductive agent has a nano-spherical structure; the one-dimensional long-range conductive agent has a one-dimensional linear structure. In the present invention, the long-range / short-range conductive network not only provides "point-to-point contact" electronic conduction between adjacent active material particles, but also provides "point-to-line contact" electronic conduction between multiple active material particles in a local area. On the one hand, this microstructure can alleviate the volume strain accompanying the charge and discharge process, effectively improve the capacity loss caused by the loss of electrical contact of the active material particles, and on the other hand, a conductive network with a stable structure and large-area rapid conductivity is introduced into the entire electrode, which can achieve better rate performance at the entire electrode scale. The present invention ingeniously designs a long-range / short-range composite conductive path for disorderly stacked positive electrode active particles, improves the rapid transmission of electrons and ions on the surface of irregularly distributed positive electrode active particles, and makes them have high electronic and ionic conductivity.

[0021] The present invention also provides a method for preparing the above-mentioned composite positive electrode material containing long / short-range conductive agents. The present invention obtains a uniformly dispersed electrode slurry through ultrasound and ball milling. The obtained electrode material has a long-range / short-range composite conductive network that can be tightly filled between active particles, significantly improving the electronic and ionic conductivity and structural stability of the positive electrode active material, and achieving excellent rate performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Schematic diagram of the microstructure of the electrode formed by the composite positive electrode material in Example 1 and Comparative Examples 1-2, wherein (a) is treated with a short-range conductive agent, (b) is treated with a long-range conductive agent, and (c) is treated with a long-range / short-range conductive agent;

[0023] Figure 2 SEM images of LiCoO2 particles, VGCF, and LiCoO2 / VGCF-CNTs-super C electrodes in Example 6, including (a) LiCoO2 particles, (b) VGCF, (c) surface morphology of LiCoO2 / VGCF-CNTs-super C electrode, (d) cross-sectional morphology of LiCoO2 / VGCF-CNTs-super C electrode, (e) local magnified view of LiCoO2 / VGCF-CNTs-super C electrode, and (f) four elements Co, O, C, and F;

[0024] Figure 3The cyclic voltammetry curves of the batteries obtained in Application Example 1 and Comparative Application Example 1 are (a) a LiCoO2 electrode containing only a short-range conductive agent, and (b) a LiCoO2 / VGCF-CNTs-super C composite electrode containing a long-range conductive agent and a short-range conductive agent;

[0025] Figure 4 The impedance comparison diagram of the battery obtained in Application Example 1 and Comparative Application Example 1, wherein (a) the LiCoO2 electrode containing only a short-range conductive agent, and (b) the LiCoO2 / VGCF-CNTs-super C composite electrode containing a long-range conductive agent and a short-range conductive agent;

[0026] Figure 5 CV curves of the battery obtained in Application Example 1 corresponding to different cut-off voltage intervals;

[0027] Figure 6 Comparison of the cycling performance of LiCoO2 cathode at different pretreatment temperatures and VGCF ratios;

[0028] Figure 7 This is the effect of different pretreatment temperatures and VGCF ratios on the rate performance of LiCoO2 cathode;

[0029] Figure 8 This is a graph showing the effect of different conductive agents and binder types on the rate performance of LiCoO2 positive electrode;

[0030] Fig. 9 This is a graph showing the effect of different separator types on the rate performance of LiCoO2 cathode;

[0031] Fig.10 This is the effect of different electrode surface modification layer thicknesses on the rate performance of LiCoO2 positive electrode;

[0032] Fig.11 The effect of different VGCF:CNTs ratios on the positive electrode rate performance;

[0033] Fig.12 This is the surface morphology of the LiCoO2 / VGCF-CNTs-super C electrode prepared in Example 6 on the Al foil surface. DETAILED DESCRIPTION

[0034] The present invention provides a composite positive electrode material containing a long / short-range conductive agent, comprising: positive electrode active particles, a zero-dimensional short-range conductive agent connecting adjacent positive electrode active particles by physical adsorption, and a one-dimensional long-range conductive agent connecting positive electrode active particles by physical adsorption, wherein the gaps between the positive electrode active particles are filled with a conductive network formed by the zero-dimensional short-range conductive agent and the one-dimensional long-range conductive agent;

[0035] The zero-dimensional short-range conductive agent has a nano-spherical structure;

[0036] The one-dimensional long-range conductive agent has a one-dimensional linear structure.

[0037] Unless otherwise specified, the present invention has no special requirements on the sources of the raw materials used, and commercially available products known to those skilled in the art may be used.

[0038] The composite positive electrode material containing long / short-range conductive agent provided by the present invention comprises: positive electrode active particles; the gaps between the positive electrode active particles are filled with a conductive network formed by a zero-dimensional short-range conductive agent and a one-dimensional long-range conductive agent. In the present invention, the positive electrode active particles preferably include one or more of lithium cobalt oxide ternary materials, lithium iron phosphate ternary materials, lithium nickel oxide ternary materials, nickel cobalt manganese ternary materials and nickel cobalt aluminum ternary materials, and more preferably lithium cobalt oxide ternary materials; the particle size of the positive electrode active particles is preferably 100nm to 100μm, more preferably 100nm to 50μm; the positive electrode active particles include large-size particles and small-size particles, wherein the particle size of the large-size particles is preferably >50μm and ≤100μm, and the particle size of the small-size particles is preferably 100nm to 50μm; the volume ratio of the large-size particles to the small-size particles is preferably 1:1.

[0039] The composite positive electrode material containing a long / short-range conductive agent provided by the present invention comprises: a zero-dimensional short-range conductive agent connecting adjacent positive electrode active particles by physical adsorption; the zero-dimensional short-range conductive agent has a nano-spherical structure. In the present invention, the zero-dimensional short-range conductive agent preferably comprises one or more of carbon black, conductive graphite and Ketjen black, more preferably carbon black or Ketjen black; the carbon black is preferably Super C 45; the particle size of the zero-dimensional short-range conductive agent is preferably 0.05 to 15 μm, more preferably 50 to 100 nm.

[0040] The composite positive electrode material containing a long / short-range conductive agent provided by the present invention comprises: a one-dimensional long-range conductive agent connecting positive electrode active particles by physical adsorption; the one-dimensional long-range conductive agent has a one-dimensional linear structure. In the present invention, the one-dimensional long-range conductive agent preferably comprises vapor-grown carbon fiber VGCF and / or carbon nanotubes CNTs, more preferably vapor-grown carbon fiber; the aspect ratio of the vapor-grown carbon fiber is preferably L / D≥30:1, and the aspect ratio of the carbon nanotube is preferably L / D≥1000:1.

[0041] In the present invention, VGCF and CNTs have a one-dimensional linear structure, which can usually wrap around the active material particles to form a point-line contact, forming a uniform point-line connection conductive network inside the electrode. VGCF and CNTs also have a large aspect ratio. Even if the active material undergoes irreversible deformation, the gaps formed between its particles can be reconnected by VGCF and CNTs to ensure that the electron transmission path will not be interrupted. At the same time, the entire electrode benefits from the high strength of VGCF and CNTs materials, which increases the bonding force between the active material particles and will not fall off seriously due to deformation. In addition, VGCF and CNTs have a special hollow structure, which can store a large amount of electrolyte inside, which is conducive to the rapid transmission of lithium ions around and shortens the ion transmission path. In summary, the electrode containing a long-range conductive agent can exhibit high-rate charge and discharge performance.

[0042] In the present invention, the mass ratio of the positive electrode active particles and the zero-dimensional short-range conductive agent is preferably (70-95):(1-10), and more preferably (70-85):(4-10); the mass ratio of the one-dimensional long-range conductive agent and the zero-dimensional short-range conductive agent is preferably (1-4):(1-4), and more preferably (2-3):(2-3).

[0043] The present invention also provides a method for preparing the composite positive electrode material containing the long / short range conductive agent described in the above technical solution, comprising the following steps:

[0044] The one-dimensional long-range conductive agent, the zero-dimensional short-range conductive agent and the organic solvent are mixed, and water bath ultrasonication is performed to obtain a conductive agent dispersion liquid;

[0045] The conductive agent dispersion and positive electrode active particles are mixed and ball milled to obtain the composite positive electrode material containing the long / short range conductive agent.

[0046] The invention mixes a one-dimensional long-range conductive agent, a zero-dimensional short-range conductive agent and an organic solvent, and performs water bath ultrasound to obtain a conductive agent dispersion.

[0047] In the present invention, the organic solvent is preferably N-methylpyrrolidone (NMP); the mass ratio of the sum of the zero-dimensional short-range conductive agent and the one-dimensional long-range conductive agent to the organic solvent is preferably (0.1-4):(1-6), more preferably 0.2:4.

[0048] In the present invention, the temperature of the water bath ultrasound is preferably ≤20°C, more preferably 10-15°C; the time of the water bath ultrasound is preferably 5-60min, more preferably 20min; the power of the water bath ultrasound is preferably 450-600W, more preferably 500-550W.

[0049] After obtaining the conductive agent dispersion, the present invention mixes the conductive agent dispersion and positive electrode active particles and performs ball milling to obtain the composite positive electrode material containing the long / short range conductive agent.

[0050] When the positive electrode active particles are lithium cobalt oxide ternary materials, before mixing the conductive agent dispersion and the positive electrode active particles, the present invention preferably also includes: preheating the positive electrode active particles; the preheating treatment is preferably carried out in a mixed atmosphere of argon and oxygen; the volume ratio of argon and oxygen is preferably (100-95): (0.5-5), more preferably 98:2; the temperature of the preheating treatment is preferably 550-600°C, more preferably 550°C or 600°C, and most preferably 550°C; the holding time of the preheating treatment is preferably 2h; the heating rate to the preheating treatment temperature is preferably 5°C / min. The present invention compensates for the lack of lattice oxygen in commercial LiCoO2 through preheating treatment, and other types of positive electrode active materials generally do not use a preheating treatment step.

[0051] In the present invention, the mixing of the conductive agent dispersion and the positive electrode active particles is preferably carried out under the condition of magnetic stirring; the rotation speed of the magnetic stirring is preferably 100-800 rpm, more preferably 250-550 rpm; the time of the magnetic stirring is preferably 5-240 min, more preferably 60 min.

[0052] In the present invention, the ball-to-material ratio of the ball mill is preferably 1:1-20, more preferably 1:5-10; the rotation speed of the ball mill is preferably 100-500rpm, more preferably 200-300rpm; the ball milling time is preferably 30-720min, more preferably 60-120min; the ball milling is preferably carried out in an agate tank; the grinding balls used in the ball mill are preferably stainless steel balls and / or agate balls, more preferably agate balls; the grinding balls used in the ball mill preferably include grinding balls with a diameter of 10mm and grinding balls with a diameter of 5mm; the mass ratio of the grinding balls with a diameter of 10mm and the grinding balls with a diameter of 5mm is preferably 1:1.

[0053] The VGCF and CNTs used in the present invention have the same disadvantages as traditional conductive agents, that is, nano-sized materials are not easy to disperse due to electrostatic effects. The present invention adopts ultrasonic-ball milling technology to successfully prepare electrode slurry with uniform dispersion of conductive agent through high-speed shearing, solving the dispersion problem.

[0054] After the ball milling, the present invention preferably further comprises: drying the slurry obtained by the ball milling to obtain a composite positive electrode material containing a long / short range conductive agent. In the present invention, the drying temperature is preferably 80 to 150° C., more preferably 100 to 120° C.; the drying time is preferably 2 to 24 hours, more preferably 6 to 12 hours.

[0055] Compared with the existing positive electrode modification technology, the beneficial effect achieved by the present invention is that different types of conductive agents are directly added during the ball milling process to change the problem of poor conductivity of the positive electrode material. Compared with using complex modification methods such as doping, coating, sintering and other methods to modify the positive electrode material to improve its electron / ion transmission performance, the preparation method provided by the present invention is more conducive to the batch preparation of positive electrode materials and the improvement of rate performance.

[0056] The present invention also provides the use of the composite positive electrode material containing the long / short-range conductive agent described in the above technical solution or the composite positive electrode material containing the long / short-range conductive agent prepared by the preparation method described in the above technical solution in a lithium ion battery.

[0057] The present invention also provides a lithium-ion battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the active material in the positive electrode is a composite positive electrode material containing a long / short-range conductive agent; the composite positive electrode material containing a long / short-range conductive agent is the composite positive electrode material containing a long / short-range conductive agent described in the above technical scheme or the composite positive electrode material containing a long / short-range conductive agent prepared by the preparation method described in the above technical scheme.

[0058] In the present invention, the method for preparing the positive electrode preferably comprises the following steps:

[0059] The one-dimensional long-range conductive agent, the zero-dimensional short-range conductive agent and a solution containing a binder are mixed, and water bath ultrasonication is performed to obtain a conductive agent dispersion;

[0060] The conductive agent dispersion and the positive electrode active particles are mixed and ball-milled, and the obtained ball-milled slurry is coated on the surface of the Al foil current collector, first dried, and then pressed and second dried.

[0061] In the present invention, the method for preparing the solution containing the binder is preferably: mixing the binder and the organic solvent, and sequentially performing water bath ultrasound or magnetic stirring to obtain a solution containing the binder; the binder is preferably polyvinylidene fluoride (PVDF); the model of the polyvinylidene fluoride (PVDF) is preferably HSV900 or 5310; the organic solvent is preferably N-methylpyrrolidone (NMP); the mass of the binder is preferably 2-5% of the mass of the organic solvent, more preferably 2.5%; the temperature of the water bath ultrasound is preferably ≤ 20℃, more preferably 10-15℃; the power of the water bath ultrasound is preferably 450-600W, more preferably 500-550W; the time of the water bath ultrasound is preferably 5-30min, more preferably 10-20min; the temperature of the magnetic stirring is preferably 10-50℃, more preferably 10-20℃; the rate of the magnetic stirring is preferably 200-700rpm, more preferably 300-400rpm; the time of the magnetic stirring is preferably 5-60min, more preferably 20min. In the present invention, the binder can swell in the solution to form a polymer chain, which plays a role in linking the composite positive electrode material containing the long / short-range conductive agent and the current collector.

[0062] In the present invention, the process of mixing a one-dimensional long-range conductive agent, a zero-dimensional short-range conductive agent and a solution containing a binder, performing water bath ultrasound, and the process of mixing the conductive agent dispersion and positive electrode active particles and performing ball milling are consistent with the process in the preparation method of the composite positive electrode material containing long / short-range conductive agents, and will not be repeated here.

[0063] In the present invention, the temperature of the first drying is preferably 100°C, the time is preferably 6 hours, and the first drying is preferably air-blast drying; the pressing pressure is preferably 16 MPa, and the time is preferably 10 seconds; the temperature of the second drying is preferably 100°C, the time is preferably 6 hours, and the second drying is preferably carried out in a vacuum drying oven.

[0064] In the present invention, the loading amount of the composite positive electrode material containing the long / short range conductive agent in the positive electrode is preferably 2 to 10 mg·cm -2 , more preferably 3 to 4 mg·cm -2 .

[0065] The composite positive electrode material containing long / short-range conductive agents provided by the present invention can ensure good electrical contact between different active particles inside the positive electrode, and the assembled button battery has low charge transfer impedance and excellent rate performance.

[0066] The present invention preferably further comprises: depositing gold (Au) on the positive electrode by magnetron sputtering; the deposition time is preferably 5 to 15 seconds, more preferably 5 seconds, 10 seconds or 15 seconds, and most preferably 15 seconds. The present invention has no special limitation on the magnetron sputtering process, and the magnetron sputtering process known in the art can be used.

[0067] In the present invention, the negative electrode is preferably a metal lithium sheet; the diaphragm is preferably a polypropylene (PP) diaphragm or a cellulose diaphragm, more preferably a polypropylene (PP) diaphragm; the thickness of the diaphragm is preferably 3μm, 5.5μm or 12μm, more preferably 5.5μm; the electrolyte is preferably a LiPF6 solution; the solvent used for the LiPF6 solution is a mixture of ethylene carbonate EC, dimethyl carbonate DMC and diethyl carbonate DEC; the volume ratio of ethylene carbonate EC, dimethyl carbonate DMC and diethyl carbonate DE is preferably 1:1:1; the concentration of the LiPF6 solution is preferably 1.2mol / L.

[0068] The technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention, but they should not be construed as limiting the protection scope of the present invention.

[0069] Example 1

[0070] 0.1 g PVDF was dissolved in 4 g NMP solvent and ultrasonically treated at 500 W power for 10 min in a 10°C water bath to obtain a uniformly dispersed solution containing the binder;

[0071] 0.1 g of short-range conductive agent carbon black (Super C 45, particle size of 50-100 nm) and 0.1 g of long-range conductive agent VGCF (L / D ≥ 1000:1) were added to the binder-containing solution, and ultrasonication was continued at 500 W power for 20 min in a 10° C. water bath to obtain a conductive agent dispersion;

[0072] 0.7 g of commercial LiCoO2 positive electrode particles were directly added to the above conductive agent dispersion, magnetically stirred at 500 rpm for 60 min, and then transferred to an agate ball mill and ball milled for 120 min, with a ball-to-material ratio of 1:10; the ball mill speed was 300 rpm, and the grinding balls used were agate balls, with diameters of 10 mm and 5 mm in two sizes, with a mass ratio of 1:1, to obtain a uniform slurry;

[0073] The uniformly dispersed slurry is coated on aluminum foil and dried at 100° C. for 6 h to obtain an electrode sheet loaded with a composite positive electrode material containing a long / short range conductive agent.

[0074] Example 2

[0075] The difference from Example 1 is that the LiCoO2 positive electrode particles are preheated, and an Ar / O2 mixed atmosphere with a volume ratio of 98:2 is selected. The temperature is increased to 550°C and 600°C, respectively, with a step size of 5°C / min, and each is kept warm for 2 h to compensate for the lack of lattice oxygen in commercial LiCoO2. The rest of the content is consistent with Example 1.

[0076] Example 3

[0077] The difference from Example 2 is that the mass ratios of the long-range conductive agent VGCF and the short-range conductive agent carbon black (Super C 45) are adjusted to VGCF:Super C=0.15g:0.05g, 0.05g:0.15g, 0.2g:0g, respectively. The composite positive electrode material samples obtained by the three ratios are marked as VGCF-1, VGCF-2, and VGCF-3, respectively. The rest of the content is consistent with Example 2.

[0078] Example 4

[0079] The difference from Example 2 is that the short-range conductive agent carbon black (Super C 45) is replaced by Ketjen black (KB), and the rest of the contents are consistent with Example 2.

[0080] Example 5

[0081] The difference from Example 2 is that the binder is changed from traditional PVDF (model HSV900) to model 5310, and the rest of the contents are consistent with Example 2.

[0082] Example 6

[0083] The difference from Example 2 is that the long-range conductive agent VGCF is replaced by part of CNTs, and the mass ratio of the long-range conductive agent to the short-range conductive agent is VGCF:CNTs:KB=0.12g:0.03g:0.05g, 0.075g:0.075g:0.05g, 0.03g:0.12g:0.05g, and the rest of the content is consistent with Example 2.

[0084] Comparative Example 1

[0085] The difference from Example 1 is that no long-range conductive agent is used, only a short-range conductive agent is used, and the rest of the contents are consistent with Example 1, thereby obtaining a composite positive electrode material containing a short-range conductive agent.

[0086] Comparative Example 2

[0087] The difference from Example 1 is that no short-range conductive agent is used, only a long-range conductive agent is used, and the rest of the contents are consistent with Example 1, thereby obtaining a composite positive electrode material containing a long-range conductive agent.

[0088] Application Example 1

[0089] The slurry obtained in Example 1 was uniformly coated on an aluminum foil current collector, and dried under 100° C. for 6 h. After completely removing the NMP solvent, it was cut into a disc positive electrode with a diameter of 11 mm. It was treated at a pressure of 16 MPa for 10 s using a hydraulic device, and then weighed and placed in a vacuum drying oven at 100° C. for 6 h to obtain an electrode sheet, which was then directly transferred to a glove box for standby use;

[0090] The above-mentioned electrode sheet was used as the positive electrode, the metal lithium sheet was used as the counter electrode and the reference electrode, the traditional polypropylene separator PP (thickness of 12 μm) was used as the separator, and 1.2 mol / L LiPF6 solution (the solvent was a mixture of ethylene carbonate EC, dimethyl carbonate DMC and diethyl carbonate DEC, with a volume ratio of 1:1:1) was used as the electrolyte to assemble a CR 2025 button battery in a glove box.

[0091] Application Example 2

[0092] The difference from Application Example 1 is that the composite positive electrode material containing the long / short range conductive agent prepared in Example 1 is replaced by the composite positive electrode material prepared in Example 2, and the rest of the contents are consistent with Application Example 1.

[0093] Application Example 3

[0094] The difference from Application Example 1 is that the composite positive electrode material containing the long / short range conductive agent prepared in Example 1 is replaced by the composite positive electrode material prepared in Example 3, and the rest of the contents are consistent with Application Example 1.

[0095] Application Example 4

[0096] The difference from Application Example 2 is that the separator is changed to a cellulose separator with thicknesses of 5.5 μm and 3 μm respectively, and the rest of the contents are consistent with Application Example 2.

[0097] Application Example 5

[0098] The difference from Application Example 2 is that an Au modification layer is deposited on the surface of the electrode sheet, and the deposition time is designed to be 5s, 10s, and 15s respectively. The rest of the content is consistent with Application Example 2.

[0099] Comparative application example 1

[0100] The difference from Application Example 1 is that the composite positive electrode material containing long / short-range conductive agent prepared in Example 1 is replaced by the composite positive electrode material containing short-range conductive agent prepared in Comparative Example 1, and the rest of the contents are consistent with Application Example 1.

[0101] Performance Testing

[0102] (1) Electron microscopy was performed on the electrodes formed by the composite positive electrode materials in Example 1 and Comparative Examples 1-2. The results are as follows: Figure 1As shown, among them, (a) short-range conductive agent treatment, (b) long-range conductive agent treatment, and (c) long-range / short-range conductive agent treatment.

[0103] Figure 1 The structural schematic diagrams of three positive electrode materials are given. Figure 1 (a) Zero-dimensional spherical particles are dispersed around LiCoO2 particles. Figure 1 (b) shows a one-dimensional linear conductive agent wrapped around the LiCoO2 particles. Figure 1 (c) shows that the two conductive agents, zero-dimensional and one-dimensional, are evenly distributed in the pores of LiCoO2 particles, forming a uniform conductive network. Figure 1 The electrode structure shown in (c) is an ideal electrode structure, which is conducive to the rapid transmission of electrons between different LiCoO2 particles.

[0104] (2) The LiCoO2 particles, VGDF one-dimensional material, and LiCoO2 / VGCF-CNTs-super C electrode in Example 6 were analyzed and tested using a scanning electron microscope. The results are as follows: Figure 2 As shown, (a) LiCoO2 particles, (b) VGCF, (c) surface morphology of LiCoO2 / VGCF-CNTs-super C electrode, (d) cross-sectional morphology of LiCoO2 / VGCF-CNTs-super C electrode, (e) local enlarged view of LiCoO2 / VGCF-CNTs-super C electrode, (f) uniform distribution of the four elements Co, O, C, and F in the composite electrode.

[0105] Depend on Figure 2 It can be seen that after mixing conductive materials of different dimensions, they can be combined with LiCoO2 particles to form a three-dimensional conductive system. "Point-point" contact and "point-line" contact are formed between two or more adjacent LiCoO2 particles. Compared with traditional conductive agents, which can only provide electron conduction in local areas, this three-dimensional conductive system can quickly transmit electrons.

[0106] (3) The batteries obtained in Application Example 1 and Comparative Application Example 1 were transferred to a Xinwei charge and discharge tester for constant current charge and discharge test. The cut-off voltage was set to 3.0-4.4 V, the test temperature was room temperature 25 °C, and the rate performance test was performed at different current densities, which were set in sequence from 0.1 to 10 A·g -1 The results are shown in Table 1. Figures 3 to 5 As shown, LiCoO2 and LiCoO2(L) in the figure are comparative application example 1 and application example 1 respectively.

[0107] Depend on Figure 3The CV curves shown in the figure show that the addition of the long-range conductive agent VGCF does not affect the chemical reactions of LiCoO2 during the process of lithium ion insertion and extraction, and the positions of the oxidation peak and reduction peak remain unchanged. After overcoming the large polarization in the first cycle of charge and discharge, the polarization degree of the second and third cycles of charge and discharge decreases and remains unchanged. In addition, Figure 4 The electrochemical impedance spectroscopy (EIS) shown in the figure more significantly shows the advantages of adding long-range conductive agents. Compared with LiCoO2 electrodes with only short-range conductive agents, LiCoO2 (L) has a smaller contact impedance of 3.8Ω, which is smaller than the contact impedance of LiCoO2 electrodes of 6.1Ω. By comparing the EIS spectra, we can directly observe the effect of long-range conductive agents on reducing electrode contact impedance. In order to give full play to the theoretical specific capacity of the LiCoO2 positive electrode, the cut-off voltage is increased, and the highest working voltage without causing side reactions is determined by measuring the CV curves corresponding to different cut-off voltage intervals. The results are shown in Figure 1. Figure 5 As shown, the high cutoff voltages are selected as 4.1V, 4.2V, 4.3V, 4.4V, and 4.5V in turn. It is observed that the CV curve corresponding to 4.3V is incomplete, indicating that the capacity of LiCoO2 is not fully utilized, and a new small peak appears at 4.5V, which may come from the decomposition of part of the electrolyte and the beginning of side reactions. Therefore, 3.0-4.4V is finally selected as the safe operating voltage range of the LiCoO2 electrode, which can maximize the lithium storage capacity of the active material while ensuring the normal operation of the battery.

[0108] (4) The effects of different preheating temperatures in Example 2 and different ratios of long-range conductive agent to short-range conductive agent in Example 3 on the cycling performance of LiCoO2 electrode are shown in the following table. Figure 6 Although LiCoO2 without preheating treatment has a high discharge capacity in the first 200 cycles, the discharge capacity decays rapidly from the 200th cycle, with an average decrease of 1.2 mA·h·g per cycle. -1 After the LiCoO2 electrode was preheated at 550℃ or 600℃, the missing lattice oxygen in LiCoO2 was supplemented, and LiCoO2 had a more stable structure. During the whole cycle, the discharge capacity decayed slowly, and the average discharge capacity decreased by 0.2mA·h·g per cycle. -1. At the same time, LiCoO2 preheated at 550°C was selected. In the preparation process of the electrode slurry, the mass ratios of LiCoO2:PVDF:VGCF:Super C were designed to be 0.7g:0.1g:0.2g:0g, 0.7g:0.1g:0.15g:0.05g, and 0.7g:0.1g:0.05g:0.15g, respectively. The samples with these three ratios were labeled VGCF-1, VGCF-2, and VGCF-3, respectively. After comparing their charge and discharge cycle performance, the high ratio of long-range conductive agent has excellent cycle performance. The mass ratio of LiCoO2:PVDF:VGCF:Super C is tentatively set to 0.7g:0.1g:0.15g:0.05g. At the same time, the rate performance of all LiCoO2 electrodes in Example 2 and Example 3 was compared, and the results are as follows. Figure 7 As shown. In 0.1~7.0A·g -1 Under increasing current density, the sample preheated at 550℃ and the mass ratio of LiCoO2:PVDF:VGCF:Super C are 0.7g:0.1g:0.15g:0.05g, which has excellent rate performance. -1 The corresponding reversible capacity under the condition of -1 , which is higher than the reversible capacity of the untreated LiCoO2 electrode at this current density of 49 mA·h·g -1 .

[0109] (5) In order to further improve the rate performance of LiCoO2 electrode, a new comparative experiment was designed based on the type of conductive agent and binder, corresponding to the samples of Example 4 and Example 5. In Example 4, the short-range conductive agent carbon black was replaced with Ketjen black (KB), and the corresponding mass ratio remained unchanged. The corresponding rate performance is as follows: Figure 8 As shown in the figure, it is observed that the type of short-range conductive agent has no significant effect on the rate performance of the LiCoO2 electrode. -1 No significant difference in discharge capacity was observed at current densities of 0.1 A·g -1 and 2.0A·g -1 At a current density of 1.34 Å, the reversible specific capacity of the samples using Super C45 and KB is 174 mA·h·g -1 and 104mA·h·g -1 .

[0110] (6) The effects of different separator types on the rate performance of LiCoO2 electrodes were compared. Fig. 9As shown, for the common PP membranes, three types of membranes, 3μm, 5.5μm, and 12μm, were selected, and cellulose membranes were also added. When using the same electrode material and the same test conditions, it was found that the ultra-thin 3μm PP membrane corresponds to a higher reversible specific capacity at low current density, but the membrane is not easy to spread and is easily broken due to electrostatic effects during stacking operations. With the increase of current density, it was found that the PP membrane with a thickness of 5.5μm exhibited better performance. The cellulose membrane and the 12μm P membrane have a larger thickness and a longer side of the ion shuttle path, and the corresponding rate performance has no advantage. After comprehensive consideration, a PP membrane with a thickness of 5.5μm was selected.

[0111] (7) In order to optimize the interface between the LiCoO2 electrode and the electrolyte, magnetron sputtering technology was used to deposit metal gold (Au) on the surface of the LiCoO2 electrode. The effects of different deposition times (0s, 5s, 10s, and 15s) on its rate performance were compared. The test results are shown in Figure 2. Fig.10 As shown, the results indicate that the effect of surface modification of Au on the rate performance of LiCoO2 electrode is not obvious, and the reversible specific capacity of the sample deposited for 15s is slightly increased. Considering the complexity of the magnetron sputtering process and the continuity of the entire electrode preparation, the LiCoO2 electrode / electrolyte interface is no longer optimized.

[0112] (8) Starting from optimizing the proportion of the conductive agent, based on the above optimization selection, the mass ratio of LiCoO2:PVDF:VGCF:SuperC is 0.7g:0.1g:0.15g:0.05g, and 0.15g of VGCF is further replaced by VGCF:CNTs=0.12g:0.03g, 0.075g:0.075g, 0.03g:0.12g, that is, the mass ratio of VGCF:CNTs is marked as 4:1, 2.5:2.5, and 1:4 respectively, and their effects on the rate performance of the LiCoO2 electrode are compared. The results are as follows Fig.11 As shown, the 1:4 sample corresponds to the best rate performance. For example, at the same 0.5 A g -1 At a current density of 1:4, the reversible specific capacity of the sample is 163 mA·h·g -1 , which is higher than the specific capacity of VGCF electrode alone by 150mA·h·g -1 .

[0113] (9) The rate performance of the LiCoO2 electrodes corresponding to different embodiments was tested. The batteries were assembled into button cells in the same manner as described above. The test results are shown in Table 1.

[0114] Table 1 Rate performance of LiCoO2 electrodes corresponding to different embodiments

[0115]

[0116]

[0117] As can be seen from Table 1, the type and proportion of the long-range conductive agent and short-range conductive agent selected by the preparation method and screening of the present invention can effectively improve the rate performance of the LiCoO2 electrode. In a preferred embodiment of the present invention, the mass ratio of the electrode composition LiCoO2: PVDF: VGCF: CNTs: Super C45 is finally selected to be 0.7:: 0.1: 0.03: 0.12: 0.05, which corresponds to the highest reversible specific capacity at different current densities. This is due to the long-range / short-range conductive network constructed inside the LiCoO2 electrode, which can provide good electrical contact at high current density, reducing the loss of electrical contact of the active material particles, and showing a high reversible specific capacity. The unmodified LiCoO2 electrode not only has a poor cycle life, but also its discharge specific capacity will decay rapidly at high current density.

[0118] (10) Fig.12 Surface morphology of the LiCoO2 / VGCF-CNTs-super C electrode prepared in Example 6 on the Al foil surface.

[0119] Depend on Fig.12 It can be seen that the three-dimensional conductive network used in the present invention has a good inhibitory effect on the agglomeration of LiCoO2 particles. The components within the entire electrode scale are evenly distributed, the separated LiCoO2 particles are evenly distributed on the entire electrode surface, and the particles are surrounded by conductive materials.

[0120] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention rather than all the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A composite cathode material containing a long / short range conductive agent, It is characterized in that include: Positive electrode active particles, a zero-dimensional short-range conductive agent connecting adjacent positive electrode active particles by physical adsorption, and a one-dimensional long-range conductive agent connecting the positive electrode active particles by physical adsorption, wherein the gaps between the positive electrode active particles are filled with a conductive network formed by the zero-dimensional short-range conductive agent and the one-dimensional long-range conductive agent; The zero-dimensional short-range conductive agent has a nano-spherical structure; The one-dimensional long-range conductive agent has a one-dimensional linear structure.

2. The composite positive electrode material containing a long / short range conductive agent according to claim 1, It is characterized in that The zero-dimensional short-range conductive agent includes one or more of carbon black, conductive graphite and Ketjen black.

3. The composite positive electrode material containing a long / short range conductive agent according to claim 1, It is characterized in that The one-dimensional long-range conductive agent includes vapor-grown carbon fibers and / or carbon nanotubes; the length-to-diameter ratio L / D of the vapor-grown carbon fibers is ≥30:1, and the length-to-diameter ratio L / D of the carbon nanotubes is ≥1000:

1.

4. The composite positive electrode material containing a long / short range conductive agent according to claim 1, It is characterized in that The positive electrode active particles include one or more of lithium cobalt oxide ternary materials, lithium iron phosphate ternary materials, lithium nickel oxide ternary materials, nickel cobalt manganese ternary materials and nickel cobalt aluminum ternary materials.

5. The composite positive electrode material containing a long / short range conductive agent according to claim 1, 2 or 3, It is characterized in that The mass ratio of the one-dimensional long-range conductive agent to the zero-dimensional short-range conductive agent is (1-4):(1-4).

6. A method for preparing a composite positive electrode material containing a long / short range conductive agent according to any one of claims 1 to 5, It is characterized in that The following steps are involved: A one-dimensional long-range conductive agent, a zero-dimensional short-range conductive agent and an organic solvent are mixed and subjected to water bath ultrasound to obtain a conductive agent dispersion; The conductive agent dispersion and positive electrode active particles are mixed and ball-milled to obtain the composite positive electrode material containing the long / short range conductive agent.

7. The preparation method according to claim 6, It is characterized in that The temperature of the water bath ultrasound is ≤20°C; the time of the water bath ultrasound is 5 to 60 minutes; and the power of the water bath ultrasound is 450 to 600W.

8. The preparation method according to claim 6, It is characterized in that The ball-to-material ratio of the ball mill is 1:1-20; the rotation speed of the ball mill is 100-500 rpm; and the time of the ball mill is 30-720 min.

9. Use of the composite positive electrode material containing a long / short-range conductive agent according to any one of claims 1 to 5 or the composite positive electrode material containing a long / short-range conductive agent prepared by the preparation method according to any one of claims 6 to 8 in a lithium-ion battery.

10. A lithium ion battery comprising a positive electrode, a negative electrode, a separator and an electrolyte, It is characterized in that The active material in the positive electrode is the composite positive electrode material containing a long / short range conductive agent as described in any one of claims 1 to 5 or the composite positive electrode material containing a long / short range conductive agent prepared by the preparation method as described in any one of claims 6 to 8.

Citation Information

Patent Citations

  • Composite conductive agent and dispersion method thereof as well as positive plate and lithium ion battery

    CN103531814A

  • Method for preparing lithium iron phosphate and lithium nickel cobalt manganese oxide composite cathode material

    CN104377353A

  • Modification method for improving electrochemical performance of lithium-rich manganese-based material

    CN107834061A

  • Composite material for positive electrode of lithium battery

    JP2009176721A

Cited By

  • Oil system homogenizing method of power type lithium primary battery positive electrode slurry