N-doped Cu nanoparticle catalyst for zinc-carbon dioxide battery as well as preparation method and application of N-doped Cu nanoparticle catalyst

Synthesis of N-doped Cu nanoparticle catalysts through CO2 laser technology solved the problems of low catalytic efficiency and poor stability of cathode electrocatalysts in zinc-carbon dioxide batteries, and achieved efficient carbon dioxide reduction reaction and excellent electrocatalytic performance, demonstrating the zinc - Application potential in carbon dioxide batteries.

CN118899451APending Publication Date: 2024-11-05BOHAI UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410928924.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The cathode electrocatalysts of existing zinc-carbon dioxide batteries have low catalytic efficiency and poor stability, which affects the kinetics and selectivity of carbon dioxide reduction reaction.

Method used

The N-doped Cu nanoparticle catalyst was synthesized by CO2 laser technology. Cu2O was formed by adding NaOH and ascorbic acid to the copper source solution, and then the N-doped Cu-HDA-X catalyst was induced to induced the synthesis of the N-doped Cu-HDA-X catalyst to regulate electrons on the catalyst surface. Environment and stress to improve the adsorption of reaction intermediates and electron transfer efficiency.

Benefits of technology

An efficient carbon dioxide reduction reaction was achieved, which significantly improved the selectivity and electrocatalytic activity of C2 products, improved the discharge power density and charge and discharge stability of zinc-carbon dioxide batteries, and demonstrated its potential in practical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118899451A_ABST
    Figure CN118899451A_ABST
Patent Text Reader

Abstract

The invention belongs to a catalyst for a battery, and relates to an N-doped Cu nanoparticle catalyst for a zinc-carbon dioxide battery as well as a preparation method and application of the N-doped Cu nanoparticle catalyst. According to the N-doped Cu nanoparticle catalyst, adsorption of a reaction intermediate can be regulated and controlled by adjusting the electronic environment and surface stress of the surface of the catalyst, so that the selectivity and activity of eCO2RR are improved, electron transfer in the catalysis process can be further improved, and the selectivity of a specific C2 product can be improved; by regulating and controlling the doping amount of hexadecylamine (HDA), the synthesized Cu-HDA-1. 25 catalyst has a rod-like structure, can further improve electron transfer in the catalysis process, and is beneficial to ion diffusion and catalytic reaction. The performance of the catalyst is superior to that of a traditional catalyst, the preparation method is simple, the reaction speed is high, energy consumption is low, and the catalyst can be applied to a zinc-carbon dioxide battery cathode catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to battery catalysts, and relates to an N-doped Cu nanoparticle catalyst for zinc-carbon dioxide batteries, a preparation method and an application thereof, and specifically relates to a CO catalyst for zinc-carbon dioxide batteries. 2 N-doped Cu nanoparticle catalyst synthesized by laser technology, preparation method and application thereof. Background Art

[0002] Against the backdrop of accelerating global energy consumption, electricity, as a sustainable and eco-friendly new energy source, is gradually gaining attention. Unlike traditional fossil energy, it does not produce large amounts of carbon dioxide and other harmful gases, and causes less pollution to the environment. At the same time, the renewability of electricity also makes it a reliable energy option. It can be generated through renewable energy sources such as solar energy and wind energy, thereby reducing dependence on limited resources. In addition, with the continuous advancement of technology, the storage and transmission efficiency of electricity is also constantly improving, making its application more extensive and convenient. Therefore, the research and development of energy storage equipment and technological innovation of electricity are imminent.

[0003] Rechargeable aqueous zinc-carbon dioxide batteries (ZCBs) are a type of battery that combines the cathode CO 2 The new fuel cell that can release CO2 and release electricity provides an effective method and strategy to address current energy and environmental issues. Compared with traditional solid-state lithium batteries, the advantages of aqueous ZCB are high theoretical energy density, abundant raw materials, and high safety. These excellent properties make aqueous ZCB have potential application prospects in "energy conservation and emission reduction" and "carbon fixation and energy release". Existing cathode electrocatalysts have low catalytic efficiency and poor stability; therefore, it is necessary to develop efficient and stable cathode electrocatalysts for electrocatalytic carbon dioxide reduction (eCO 2 RR) reaction is crucial to the promotion of water system ZCB.

[0004] eCO 2 RR can CO 2 Converted into organic compounds with higher energy density, storing electrical energy in the form of chemical energy. 2 RR is a highly complex process involving multiple electron and proton transfer processes, which can form complex reaction intermediates and lead to slow reaction kinetics. In essence, copper (Cu) has a moderate adsorption strength for carbon monoxide (CO) molecules, and CO molecules can be further reduced to C with higher value through CC coupling reaction on its surface. 2+ products, thereby producing hydrocarbons and oxygen-containing compounds; and the doping of nitrogen atoms can change the electronic structure of the Cu surface, regulate the adsorption of reaction intermediates by adjusting the catalyst surface stress, thereby increasing the eCO 2In addition, the doping of nitrogen atoms can not only regulate the binding energy of the reaction intermediates, but also accelerate the eCO 2 Therefore, the heteroatom doping strategy was used for CO 2 The catalytic system for the conversion of eCO 2 RR has important prospects.

[0005] However, currently, Cu-based composite catalytic materials are usually prepared by high-temperature pyrolysis, and the obtained materials often agglomerate, which is not conducive to the exposure of active sites and affects the electrocatalytic performance. 2 Laser induced synthesis technology is a cutting-edge material preparation technology that cleverly uses CO 2 Lasers can precisely project laser energy to a designated location, providing powerful energy support for metal reduction. This technology not only has high reaction efficiency, but also precise position control, does not require additional catalysts, effectively reduces production costs and reduces environmental pollution. At present, it has been widely used in the preparation of metal nanomaterials, showing great application potential in the fields of energy and environment.

[0006] Therefore, the present invention develops a CO for zinc-carbon dioxide battery 2 The method of synthesizing N-doped Cu nanoparticle catalysts using laser technology has important practical significance. Summary of the invention

[0007] In view of the above technical problems, the present invention provides an N-doped Cu nanoparticle catalyst for zinc-carbon dioxide batteries and a preparation method and application thereof. The catalyst of the present invention has better performance than traditional catalysts, a simple preparation method, a fast reaction speed, and low energy consumption. The catalyst can be used in zinc-carbon dioxide battery cathode catalysts.

[0008] In order to achieve the above object, the present invention provides the following technical solutions.

[0009] A method for preparing an N-doped Cu nanoparticle catalyst for a zinc-carbon dioxide battery comprises the following steps: Step 1: Dissolve the copper source in deionized (DI) water, stir at 55±10℃ for 30 min, add 2 mol / L NaOH solution, heat at 55±10℃ until the color turns brown, add 0.6 mol / L ascorbic acid solution, stir for 30 min, age, and dry in vacuum at room temperature to obtain Cu 2 O; Step 2: Cu 2O and copper source were dissolved in deionized water 1 to form solution A, 1,3,5-trimethylbenzenecarboxylic acid and hexadecylamine (HDA) were dissolved in deionized water 2 and ethanol mixed solvent to form solution B, which was then poured into solution A under vigorous stirring; 1 mol L -1 of KOH, stirred for 10 min, aged; collected by centrifugation, and dried in vacuo to obtain a catalyst precursor; Step 3: Grind the catalyst precursor in step 2 into powder and spread it evenly on a PI film with a thickness of 100 mm. 2 The laser marking machine has a laser power of 8 W and a scanning speed of 150 mm s -1 Under air atmosphere, CO 2 Laser induction was performed twice, and then the mixture was ground evenly, washed twice with distilled water, dried with air blast, and ground into powder to obtain a Cu-HDA-X catalyst, i.e., an N-doped Cu nanoparticle catalyst.

[0010] Furthermore, in steps 1 and 2, the copper source is one of copper chloride, copper sulfate, copper carbonate or copper acetate.

[0011] Furthermore, in step 1, the mass ratio of copper source: sodium hydroxide: ascorbic acid is 0.682:3.2:4.228.

[0012] Furthermore, in step 1, the ratio of copper source to deionized water is 0.682 g:400 mL.

[0013] Furthermore, in step 1, the aging time is 3±2 h.

[0014] Furthermore, in step 1, the drying temperature is 25±10° C. and the drying time is 10±2 h.

[0015] Furthermore, in step 2, Cu 2 O: The mass ratio of copper source: trimesic acid: hexadecylamine is 0.2:0.426:0.263:1.25.

[0016] Furthermore, in step 2, Cu 2 The dosage ratio of O to deionized water 1 is 0.426 g:50 mL.

[0017] Furthermore, in step 2, the volume ratio of deionized water 2: ethanol: potassium hydroxide is 45:5:1.

[0018] Furthermore, in step 2, the aging time is 10±2 h.

[0019] Furthermore, in step 2, the vacuum drying temperature is 25±10° C., and the vacuum drying time is 10-12 h.

[0020] Furthermore, in step 3, the blast drying temperature is 80±10° C., and the blast drying time is 10-12 h.

[0021] The method is used to prepare an N-doped Cu nanoparticle catalyst.

[0022] Application of the N-doped Cu nanoparticle catalyst in a zinc-carbon dioxide battery cathode catalyst.

[0023] The N-doped Cu nanoparticle catalyst is used as a carbon dioxide reduction reaction catalyst.

[0024] Compared with the prior art, the beneficial effects of the present invention are as follows.

[0025] (1) N-doped Cu nanoparticle catalysts can regulate the adsorption of reaction intermediates by adjusting the electronic environment and surface stress of the catalyst surface, thereby improving the eCO 2 The selectivity and activity of RR can further improve the electron transfer in the catalytic process and help to increase the specific C 2 Product selectivity.

[0026] (2) The present invention utilizes CO 2 Laser induction, novel method, simple preparation process, compared with the slow and energy-consuming traditional high-temperature pyrolysis method, the reaction speed is fast, energy consumption is low, and the Cu nanoparticles have good dispersion. By adjusting the doping amount of hexadecylamine (HDA), the synthesized Cu-HDA-1.25 catalyst has a rod-like structure, which can further improve the electron transfer in the catalytic process and is beneficial to ion diffusion and catalytic reaction.

[0027] (3) The Cu-HDA-1.25 catalyst of the present invention is used in eCO 2 The Cu-HDA-1.25 catalyst was used as a Zn-CO2 cathode catalyst, showing excellent performance. The rechargeable Zn-CO2 battery assembled based on Cu-HDA-1.25 has obvious advantages over other recently reported electrocatalysts, with a charge-discharge rate of 37.3 mA cm -2 The discharge current density was 29.5 mW cm -2 The maximum discharge power density and excellent charge-discharge stability of this electrocatalyst demonstrate the potential of this electrocatalyst in eCO 2 Potential of RR in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a process flow chart of the present invention.

[0029] Figure 2This is the SEM image of Cu-HDA-1.25 of Example 1 of the present invention.

[0030] Figure 3 This is the Faraday efficiency diagram of Cu-HDA-1.25 in Example 1 of the present invention; the electrolyte solution is: 1 mol L - 1 KOH.

[0031] Figure 4 The Cu-HDA-X produced by the present invention and the comparative example is 2 H 4 Faraday efficiency diagram; the electrolyte solution is: 1 mol L -1 KOH.

[0032] Figure 5 This is a stability test diagram of Cu-HDA-1.25 at a potential of -1.0 V (vs. RHE) in Example 1 of the present invention.

[0033] Figure 6 The total current density diagram of the embodiment of the present invention and the comparative example Cu-HDA-X; the electrolyte solution is: 1 molL -1 KOH.

[0034] Figure 7 The current density diagram of the embodiment of the present invention and the comparative example Cu-HDA-X; the electrolyte solution is: 1 molL -1 KOH.

[0035] Figure 8 Schematic diagram of a reversible aqueous zinc-carbon dioxide battery.

[0036] Fig. 9 The discharge polarization curve and the corresponding power density curve of Cu-HDA-1.25 in Example 1 of the present invention; the scanning rate is: 10 mV s -1 .

[0037] Fig.10 This is a graph comparing the cathode performance of zinc-carbon dioxide batteries using Cu-HDA-1.25 of Example 1 of the present invention and several existing electrocatalysts.

[0038] Fig.11 This is a discharge curve diagram of Cu-HDA-1.25 at different current densities in Example 1 of the present invention.

[0039] Fig.12 The Cu-HDA-1.25 cathode of Example 1 of the present invention is at 5.0 mV s -1 Charge-discharge cycle curves at different current densities.

[0040] Fig.13The XRD diagrams of Cu-HDA-X of the embodiments of the present invention and the comparative examples are shown in FIG.

[0041] Fig.14 This is the SEM image of Cu-HDA-0 of comparative example 1 of the present invention.

[0042] Fig.15 This is the Faraday efficiency diagram of Cu-HDA-0 in comparative example 1 of the present invention; the electrolyte solution is: 1 mol L -1 KOH.

[0043] Fig.16 This is the SEM image of Cu-HDA-0.625, comparative example 2 of the present invention.

[0044] Fig.17 This is the Faraday efficiency diagram of Cu-HDA-0.625 of comparative example 2 of the present invention; the electrolyte solution is: 1 mol L - 1 KOH.

[0045] Fig.18 This is the SEM image of Cu-HDA-2.5 of comparative example 3 of the present invention.

[0046] Fig.19 This is the Faraday efficiency diagram of Cu-HDA-2.5 of comparative example 3 of the present invention; the electrolyte solution is: 1 mol L - 1 KOH. DETAILED DESCRIPTION

[0047] In order to make those skilled in the art better understand the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. These embodiments should be understood to be only used to illustrate the present invention and not to limit the protection scope of the present invention. After reading the contents recorded in the present invention, all other embodiments obtained after various changes or modifications made to the present invention based on the technical solution and embodiments of the present invention also fall within the scope of protection of the claims of the present invention.

[0048] A method for preparing an N-doped Cu nanoparticle catalyst for a zinc-carbon dioxide battery comprises the following steps: Step 1: Dissolve the copper source in deionized (DI) water, stir at 55±10℃ for 30 min, add 2mol / L NaOH solution, heat at 55±10℃ until the color turns brown, add 0.6mol / L ascorbic acid solution, stir for 30 min, age, and dry in vacuum at room temperature to obtain Cu 2 O; Step 2: Cu 2O and copper source were dissolved in deionized water 1 to form solution A, 1,3,5-trimethylbenzenecarboxylic acid and hexadecylamine (HDA) were dissolved in deionized water 2 and ethanol mixed solvent to form solution B, which was then poured into solution A under vigorous stirring; 1 mol L -1 of KOH, stirred for 10 min, aged; collected by centrifugation, and dried in vacuo to obtain a catalyst precursor; Step 3: Grind the catalyst precursor in step 2 into powder and spread it evenly on a PI film with a thickness of 100 mm. 2 The laser marking machine has a laser power of 8 W and a scanning speed of 150 mm s -1 Under air atmosphere, CO 2 Laser induction was performed twice, and then the mixture was ground evenly, washed twice with distilled water, dried with air blast, and ground into powder to obtain a Cu-HDA-X catalyst, i.e., an N-doped Cu nanoparticle catalyst.

[0049] Furthermore, in steps 1 and 2, the copper source is one of copper chloride, copper sulfate, copper carbonate or copper acetate.

[0050] Furthermore, in step 1, the mass ratio of copper source: sodium hydroxide: ascorbic acid is 0.682:3.2:4.228.

[0051] Furthermore, in step 1, the ratio of copper source to deionized water is 0.682 g:400 mL.

[0052] Furthermore, in step 1, the aging time is 3±2 h.

[0053] Furthermore, in step 1, the drying temperature is 25±10° C. and the drying time is 10±2 h.

[0054] Furthermore, in step 2, Cu 2 O: The mass ratio of copper source: trimesic acid: hexadecylamine is 0.2:0.426:0.263:1.25.

[0055] Furthermore, in step 2, Cu 2 The dosage ratio of O to deionized water 1 is 0.426 g:50 mL.

[0056] Furthermore, in step 2, the volume ratio of deionized water 2: ethanol: potassium hydroxide is 45:5:1.

[0057] Furthermore, in step 2, the aging time is 10±2 h.

[0058] Furthermore, in step 2, the vacuum drying temperature is 25±10° C., and the vacuum drying time is 10-12 h.

[0059] Furthermore, in step 3, the blast drying temperature is 80±10° C., and the blast drying time is 10-12 h.

[0060] The present invention uses a scanning electron microscope (SEM, Hitachi S-4800) to characterize the electrocatalyst morphology. Powder X-ray diffraction (XRD, D8 ADVANCE) is used to characterize the crystal structure. 2 Laser cutting system (SC-CO 2 -B30, total power of 30 W, laser wavelength of 10.6 µm) was purchased from Shanghai Suochang Optoelectronic Equipment Co., Ltd.

[0061] All electrochemical tests were performed using a CHI 760D electrochemical workstation (Shanghai Chenhua). A customized flow-type electrolyzer (Wuhan Gaoshi Ruilian) was used to separate the anode and cathode compartments with an anion exchange membrane. 2 RR performance test. Carbon paper with gas diffusion layer (GDL) loaded with catalyst material was used as the working electrode, and Hg / HgO electrode and a platinum sheet were used as the reference electrode and counter electrode, respectively. To prepare the working electrode, carbon paper (CP) was cut into rectangular sheets (2.5 cm x 1 cm), and the catalyst was ultrasonically dispersed in a solution (V 水 :V 异丙醇 :V Nafion =4:1:0.025) to obtain a uniform suspension (7.5 mg mL -1 ). Subsequently, 200 μL of the suspension was dropped onto the carbon paper surface (electrode area 2 cm x 0.5 cm) and allowed to dry naturally. The eCO was tested using chronoamperometry at room temperature. 2 RR, all test potentials are converted to potentials relative to the reversible hydrogen electrode (RHE) by the formula: E (vs.RHE) = E (vs.Hg / HgO) + 0.095 V+0.059 pH.

[0062] During the test, CO was fed into the 2 The gas was heated at 24 mL min -1 The gas diffusion electrode (GDE) was injected at a flow rate of 1.0 mol L-1 and the electrolyte (1.0 mol L-1) was circulated at a flow rate of 120 rpm using a peristaltic pump (Cole-Parmer). - 1 KOH).

[0063] Example 1.

[0064] 1) 0.682 g of copper chloride was dissolved in 400 mL of DI water, stirred at 55±10℃ for 30 min, 40 mL of a solution containing 3.2 g of NaOH was added, heated at 55±10℃ until the color turned brown, 40 mL of a 0.6 mol / L ascorbic acid solution was added, stirred for 30 min, and aged for 3 h. The CuCl solution was dried under vacuum at 25℃ for 12 h to obtain 2 O; 2) 200 mg Cu 2 O and 0.426 g of copper chloride were dissolved in 50 mL of DI water to form solution A, 1,3,5-trimethylolpropane (0.263 g), 1.25 g of hexadecylamine were dissolved in 45 mL of DI water and 5 mL of ethanol mixed solvent to form solution B, which was then poured into solution A under vigorous stirring. 1 mL of 1 mol L -1 of KOH, stirred for 10 min, aged for 10 h, collected by centrifugation, and vacuum dried at 25 °C for 12 h to obtain a catalyst precursor; 3) After the catalyst precursor is ground into powder, it is evenly spread on a PI film with a thickness of 100 mm and heated with CO 2 The laser marking machine has a laser power of 8 W and a scanning speed of 150 mm s -1 Under air atmosphere, CO 2 The laser was induced twice, and then ground evenly, washed twice with distilled water, dried at 80°C for 10 h, and ground into powder to obtain Cu-HDA-1.25 catalyst.

[0065] The scanning electron microscope image of the Cu-HDA-1.25 catalyst prepared in Example 1 of the present invention is as follows: Figure 2 As shown, it can be clearly seen that the metal nanoparticles grow on the rod-like structure.

[0066] The Faraday efficiency diagram of the Cu-HDA-1.25 catalyst prepared in Example 1 of the present invention is as follows Figure 3 As shown in the figure, when the potential is -0.9 V, the C 2 The product has the highest Faraday efficiency of 75.5%. 2 The product is C 2 H 4 , and its Faraday efficiency is 60.4%.

[0067] The present invention (Example 1, Comparative Examples 1, 2 and 3) Cu-HDA-X produces C 2 H 4 The Faraday efficiency is Figure 4 As shown, the Cu-HDA-1.25 electrode has a C 2The product has the highest Faradaic efficiency of 75.5% at a potential of -0.9 V.

[0068] The stability test diagram of the Cu-HDA-1.25 catalyst prepared in Example 1 of the present invention is as follows Figure 5 As shown, Cu-HDA-1.25 at a potential of -0.9 V is -1 eCO can be efficiently produced in KOH 2 RR and maintained for more than 14 h, indicating that Cu-HDA-1.25 has good catalytic stability.

[0069] The total current density of Cu-HDA-X of the present invention (Example 1, Comparative Examples 1, 2 and 3) is as follows Figure 6 As shown in Figure 2, the total current density of Cu-HDA-1.25 is the highest, which is 240 mA cm at −1.0 V. -2 .

[0070] The present invention (Example 1, Comparative Examples 1, 2 and 3) Cu-HDA-X produces C 2 H 4 The Faraday efficiency is Figure 7 As shown, Cu-HDA-1.25 has a 2 The product has the highest partial current density, which is 180.24 mA cm at a potential of -1.0 V. -2 .

[0071] The Cu-HDA-1.25 prepared in Example 1 was used as the cathode material to assemble a zinc-carbon dioxide battery. -1 KOH as cathode electrolyte, 6.0 mol L -1 KOH and 0.2 mol L -1 Zn(AC) 2 As the anode electrolyte, its schematic diagram is as follows Figure 8 shown.

[0072] The discharge polarization curve and the corresponding power density curve of Cu-HDA-1.25 prepared in Example 1 of the present invention are as follows: Fig. 9 As shown in the figure, Cu-HDA-1.25 has a discharge current density of 37.3 mA cm -2 The maximum discharge power density is 29.5 mW cm -2 .

[0073] The performance of Cu-HDA-1.25 prepared in Example 1 of the present invention is compared with several electrocatalysts reported recently as cathodes for zinc-carbon dioxide batteries. Fig.10 As shown in the figure, it can be seen that Cu-HDA-1.25 has excellent discharge current density and discharge power density compared with other electrocatalysts.

[0074] The discharge curves of Cu-HDA-1.25 prepared in Example 1 of the present invention at different current densities are as follows Fig.11 As shown, during battery discharge, C 2 The Faradaic efficiency of the product is always above 70%, indicating that CO 2 Convert to C 2 The product is dominant.

[0075] The charge-discharge cycle curve of Cu-HDA-1.25 prepared in Example 1 of the present invention is as follows: Fig.12 As shown, at 5.0 mA cm -2 The charge and discharge cycle stability of zinc-carbon dioxide battery can reach 40 h at the current density.

[0076] Comparative example 1.

[0077] 1) 0.682 g of copper chloride was dissolved in 400 mL of DI water, stirred at 55±10℃ for 30 min, 40 mL of a solution containing 3.2 g of NaOH was added, heated at 55±10℃ until the color turned brown, 40 mL of a 0.6 mol / L ascorbic acid solution was added, stirred for 30 min, and aged for 3 h. The CuCl solution was dried under vacuum at 25℃ for 12 h to obtain 2 O; 2) 200 mg Cu 2 O and 0.426 g of copper chloride were dissolved in 50 mL of DI water to form solution A, and 1,3,5-trimethylolpropane (0.263 g) was dissolved in 45 mL of DI water and 5 mL of ethanol mixed solvent to form solution B, which was then poured into solution A under vigorous stirring. 1 mL of 1 mol L -1 of KOH, stirred for 10 min, aged for 10 h, collected by centrifugation, and vacuum dried at 25 °C for 12 h to obtain a catalyst precursor; 3) After the catalyst precursor is ground into powder, it is evenly spread on a PI film with a thickness of 100 mm and heated with CO 2 The laser marking machine has a laser power of 8 W and a scanning speed of 150 mm s -1 Under air atmosphere, CO 2 Laser induction was performed twice, and then the mixture was ground evenly, washed twice with distilled water, dried at 80 °C for 10 h, and ground into powder to obtain Cu-HDA-0 catalyst.

[0078] The XRD patterns of Cu-HDA-X of the present invention (Example 1, Comparative Examples 1, 2 and 3) are as follows: Fig.13As shown in the XRD patterns, Cu-HDA-0, Cu-HDA-0.625, Cu-HDA-1.25 and Cu-HDA-2.5 exhibit good crystallinity. The Cu-HDA-0 catalyst can clearly observe the diffraction peaks at 36.4°, 42.3° and 61.3°, which correspond to the Cu 2 O (111), (200) and (220) planes, indicating the formation of Cu 2 O (PDF 05-0667). Diffraction peaks at 43.3°, 50.4° and 74.1° can be clearly observed for Cu-HDA-0.625, Cu-HDA-1.25 and Cu-HDA-2.5 catalysts, which correspond to the Cu (111), Cu (200) and Cu (220) crystal planes of metallic Cu, indicating the formation of metallic Cu (PDF 04-0836). However, the position of the XRD diffraction peak gradually moves to a higher angle with the increase of HDA, and no obvious alloy phase is produced, indicating that N doping will cause the expansion of the Cu substrate lattice to produce compressive strain, thereby changing the electronic structure of the Cu surface.

[0079] The scanning electron microscope image of the Cu-HDA-0 catalyst prepared in Comparative Example 1 of the present invention is as follows: Fig.14 As shown, a clear cubic morphology is presented.

[0080] The Faraday efficiency of Cu-HDA-0 catalyst is shown in the figure Fig.15 As shown in the figure, when the potential is -0.9 V, the C 2 The Faraday efficiency of the product is 34.8%. 2 The product is C 2 H 4 , and its Faradaic efficiency is 25.6%.

[0081] Comparative example 2.

[0082] 1) 0.682 g of copper chloride was dissolved in 400 mL of DI water, stirred at 55±10℃ for 30 min, 40 mL of a solution containing 3.2 g of NaOH was added, heated at 55±10℃ until the color turned brown, 40 mL of a 0.6 mol / L ascorbic acid solution was added, stirred for 30 min, and aged for 3 h. The CuCl solution was dried under vacuum at 25℃ for 12 h to obtain 2 O; 2) 200 mg Cu 2O and 0.426 g of copper chloride were dissolved in 50 mL of DI water to form solution A, 1,3,5-trimethylolpropane (0.263 g), 0.625 g of hexadecylamine were dissolved in 45 mL of DI water and 5 mL of ethanol mixed solvent to form solution B, which was then poured into solution A under vigorous stirring. 1 mL of 1 mol L -1 of KOH, stirred for 10 min, aged for 10 h, collected by centrifugation, and dried under vacuum at 25 °C for 12 h to obtain a catalyst precursor; 3) After the catalyst precursor is ground into powder, it is evenly spread on a PI film with a thickness of 100 mm and heated with CO 2 The laser marking machine has a laser power of 8 W and a scanning speed of 150 mm s -1 Under air atmosphere, CO 2 Laser induction was performed twice, and then the mixture was ground evenly, washed twice with distilled water, dried at 80°C for 10 h, and ground into powder to obtain Cu-HDA-0.625 catalyst.

[0083] The scanning electron microscope image of the Cu-HDA-0.625 catalyst prepared in Comparative Example 2 of the present invention is as follows: Fig.16 As shown, it can be observed that the metal nanoparticles grow on the rod-like structures, but the rod-like structures are stuck together.

[0084] The Faraday efficiency of Cu-HDA-0.625 catalyst is shown in the figure Fig.17 As shown in the figure, when the potential is -0.9 V, the C 2 The Faraday efficiency of the product is 55.9%. 2 The product is C 2 H 4 , and its Faraday efficiency is 34.8%.

[0085] Comparative example 3.

[0086] 1) 0.682 g of copper chloride was dissolved in 400 mL of DI water, stirred at 55±10℃ for 30 min, 40 mL of a solution containing 3.2 g of NaOH was added, heated at 55±10℃ until the color turned brown, 40 mL of a 0.6 mol / L ascorbic acid solution was added, stirred for 30 min, and aged for 3 h. The CuCl solution was dried under vacuum at 25℃ for 12 h to obtain 2 O; 2) 200 mg Cu 2O and 0.426 g of copper chloride were dissolved in 50 mL of DI water to form solution A, 1,3,5-trimethylolpropane (0.263 g), 2.5 g of hexadecylamine were dissolved in 45 mL of DI water and 5 mL of ethanol mixed solvent to form solution B, which was then poured into solution A under vigorous stirring. 1 mL of 1 mol L -1 of KOH, stirred for 10 min, aged for 10 h, collected by centrifugation, and vacuum dried at 25 °C for 12 h to obtain a catalyst precursor; 3) After the catalyst precursor is ground into powder, it is evenly spread on a PI film with a thickness of 100 mm and heated with CO 2 The laser marking machine has a laser power of 8 W and a scanning speed of 150 mm s -1 Under air atmosphere, CO 2 The laser was induced twice, and then ground evenly, washed twice with distilled water, dried at 80°C for 10 h, and ground into powder to obtain Cu-HDA-2.5 catalyst.

[0087] The scanning electron microscope image of the Cu-HDA-2.5 catalyst prepared in Comparative Example 3 of the present invention is as follows: Fig.18 When the amount of HAD added was 2.5 g, the catalyst was piled up, which was not conducive to the transmission of substances and the penetration of electrolyte.

[0088] The Faraday efficiency of Cu-HDA-2.5 catalyst is shown in the figure Fig.19 As shown in the figure, when the potential is -0.9 V, the C 2 The Faraday efficiency of the product is 65.4%. 2 The product is C 2 H 4 , and its Faraday efficiency is 53.1%.

[0089] In summary, the present invention develops an N-doped Cu nanoparticle catalyst for zinc-carbon dioxide batteries and a preparation method and application thereof; CO 2 Laser-synthesized N-doped Cu nanoparticles for efficient electrocatalytic reduction of CO 2 C 2 The product can be used to prepare cathode electrocatalysts for zinc-carbon dioxide batteries. Cu-HDA-1.25 at 1.0 mol L -1 In KOH, the Faradaic efficiency at -0.9 V vs. RHE is 75.5%, where C 2 H 4 The Faraday efficiency is 60.4%. J c 180.24 mA cm -2Rechargeable Zn-CO2 battery based on Cu-HDA-1.25 assembled at 37.3 mA cm -2 The discharge current density was 29.5 mW cm -2 The maximum discharge power density and excellent charge-discharge stability of this electrocatalyst demonstrate the potential of this electrocatalyst in eCO 2 Therefore, the novel synthesis method proposed in the present invention is to use CO 2 The method of synthesizing electrocatalysts with laser technology has the advantages of being fast and simple. The synthesized Cu-HDA-1.25 catalyst provides ideas for the design and preparation of high-performance zinc-carbon dioxide batteries. The method is simple to synthesize and preliminary results show that the prepared catalyst is a promising eCO 2 RR electrocatalysts for metal-air batteries, fuel cells and electrocatalysis.

Claims

1. A method for preparing an N-doped Cu nanoparticle catalyst for a zinc-carbon dioxide battery, characterized in that: The steps include: Step 1, the copper source is dissolved in deionized water, stirred at 55±10°C for 30 min, 2 mol / L NaOH solution is added, heated at 55±10°C until the color changes to brown, 0.6 mol / L ascorbic acid solution is added, stirred for 30 min, aged, and vacuum dried at room temperature to obtain Cu2O; Step 2: Cu2O and copper source are dissolved in deionized water 1 to form solution A, 1,3,5-trimethylbenzenecarboxylic acid and hexadecylamine are dissolved in deionized water 2 and ethanol mixed solvent to form solution B, which is then poured into solution A under vigorous stirring; 1 molL -1 of KOH, stirred for 10 min, aged; collected by centrifugation, and dried in vacuo to obtain a catalyst precursor; Step 3: Grind the catalyst precursor of step 2 into powder, spread it evenly on a PI film with a thickness of 100 mm, and mark it with a CO2 laser with a laser power of 8 W and a scanning speed of 150 mm s. -1 Under the same conditions, CO2 laser induction was carried out twice in an air atmosphere, and then the mixture was evenly ground, washed twice with distilled water, dried with air blast, and ground into powder to obtain a Cu-HDA-X catalyst, i.e., an N-doped Cu nanoparticle catalyst.

2. The preparation method according to claim 1, characterized in that: In steps 1 and 2, the copper source is one of copper chloride, copper sulfate, copper carbonate or copper acetate.

3. The preparation method according to claim 1, characterized in that: In the step 1, the mass ratio of copper source: sodium hydroxide: ascorbic acid is 0.682:3.2:4.228; the amount ratio of copper source: deionized water is 0.682 g:400 mL.

4. The preparation method according to claim 1, characterized in that: In step 1, the aging time is 3±2 h; the drying temperature is 25±10° C., and the drying time is 10±2 h.

5. The preparation method according to claim 1, characterized in that: In the step 2, the mass ratio of Cu2O: copper source: trimesic acid: hexadecylamine is 0.2: 0.426: 0.263: 1.25; the amount ratio of Cu2O to deionized water 1 is 0.426 g: 50 mL.

6. The preparation method according to claim 1, characterized in that: In the step 2, the volume ratio of deionized water 2: ethanol: potassium hydroxide is 45:5:

1.

7. The preparation method according to claim 1, characterized in that: In step 2, the aging time is 10±2 h; the vacuum drying temperature is 25±10° C., and the vacuum drying time is 10-12 h.

8. The preparation method according to claim 1, characterized in that: In the step 3, the blast drying temperature is 80±10° C., and the blast drying time is 10-12 h.

9. An N-doped Cu nanoparticle catalyst prepared by the method according to any one of claims 1 to 8.

10. Use of the N-doped Cu nanoparticle catalyst prepared by the method according to any one of claims 1 to 8 in a cathode catalyst for a zinc-carbon dioxide battery.

Citation Information

Cited By

  • Nanometer flower-shaped electrocatalyst synthesized based on pulse CO2 laser induction as well as preparation method and application of nanometer flower-shaped electrocatalyst

    CN121575441A

  • Nanoflower-like electrocatalysts synthesized based on pulsed CO2 laser-induced synthesis, their preparation methods, and applications.

    CN121575441B