Electrolyte and secondary battery

By adjusting the electrolyte composition, especially by reducing ethylene carbonate and increasing propylene carbonate and fluoroethylene carbonate, and combining it with additives, the side reaction problem between the electrolyte and the positive electrode active material in high-energy-density batteries was solved, thereby improving battery cycle performance and gas production control.

CN118899533APending Publication Date: 2024-11-05ENVISION AESC JAPAN LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411172073.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing electrolytes are difficult to adapt to the high operating voltage of high-energy-density batteries, which leads to increased oxidation of the surface of the positive electrode active material, lattice collapse and release of oxygen, resulting in decreased battery cycle life and increased gas production. There is a lack of systematic solutions.

Method used

Adjusting the electrolyte composition reduces the use of ethylene carbonate, which has the worst oxidation resistance, and increases alternative components such as propylene carbonate and fluoroethylene carbonate. Adding 1,3-propanesulfonate lactone and ethylene sulfate as additives optimizes the electrolyte's conductivity and film-forming effect, and reduces side reactions.

Benefits of technology

By reducing side reactions between the electrolyte and the positive electrode active material under high operating voltage, the battery cycle life and gas generation issues are improved, while ensuring that the initial impedance of the battery does not deteriorate, and improving lithium-ion transport capacity and negative electrode interface protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005009589650000141
    Figure BDA0005009589650000141
  • Figure BDA0005009589650000142
    Figure BDA0005009589650000142
  • Figure BDA0005009589650000151
    Figure BDA0005009589650000151
Patent Text Reader

Abstract

The invention provides an electrolyte and a secondary battery, and belongs to the technical field of secondary batteries, the electrolyte comprises a lithium salt and a solvent, the solvent comprises ethylene carbonate, propylene carbonate, fluoroethylene carbonate and linear carbonate; the mass percentage of the ethylene carbonate relative to the solvent is 2%-10%, and the mass percentage of the sum of the propylene carbonate and the fluoroethylene carbonate relative to the solvent is 10%-30%. The electrolyte provided by the invention can be well matched with a battery with high working voltage, and effectively improves the problems of poor cycle performance and large cycle gas production of the battery while ensuring that the initial impedance of the battery is not deteriorated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of secondary batteries, and in particular to an electrolyte and a secondary battery. Background Art

[0002] Lithium-ion batteries are widely used in consumer electronics, electric vehicles and energy storage due to their long cycle life, high operating voltage, low self-discharge rate, no memory effect and environmental friendliness. In the above application areas, people have an increasing demand for battery life and are in urgent need of batteries with higher energy density.

[0003] In order to improve the energy density of batteries, the positive active materials of batteries are developing towards high energy density and high charging voltage. However, as the activity of positive active materials increases, the stability of positive active materials also becomes worse and worse, which is manifested in the increased oxidation of the surface of positive active materials. Existing electrolytes are difficult to adapt to secondary batteries with high working voltages. Under high voltage, electrolytes are prone to side reactions in positive active materials, causing the surface lattice of positive active materials to collapse and release oxygen, which in turn causes the battery cycle life to decrease and gas production to increase.

[0004] At present, the industry lacks a systematic understanding of the cyclic gas production of high energy density batteries, and the solutions are relatively scarce. It is urgent to develop electrolytes suitable for high energy density positive electrodes to effectively solve the above technical problems. Summary of the invention

[0005] In view of the above shortcomings of the prior art, the present invention provides an electrolyte and a secondary battery to improve the technical problem that the existing electrolyte is prone to side reactions with the positive electrode active material in high operating voltage batteries, resulting in a decrease in battery cycle life and worsening gas production while ensuring the conductive performance of the electrolyte.

[0006] To achieve the above-mentioned purpose and other related purposes, the present invention provides an electrolyte, which includes a lithium salt and a solvent, wherein the solvent includes ethylene carbonate, propylene carbonate, fluoroethylene carbonate and linear carbonate; the mass percentage of the ethylene carbonate relative to the solvent is 2% to 10%, and the mass percentage of the sum of the masses of the propylene carbonate and the fluoroethylene carbonate relative to the solvent is 10% to 30%.

[0007] In an example of the present invention, the mass percentage of the fluoroethylene carbonate relative to the solvent is 0.5% to 3%.

[0008] In an example of the present invention, the electrolyte further includes an additive, and the additive includes 1,3-propane sultone and vinyl sulfate.

[0009] In an example of the present invention, the mass percentage of the 1,3-propane sultone relative to the electrolyte is less than or equal to 0.5%, and the mass percentage of the vinyl sulfate relative to the electrolyte is greater than or equal to 0.8%.

[0010] In an example of the present invention, the mass percentage of the vinyl sulfate relative to the electrolyte is 0.8% to 1%.

[0011] In one example of the present invention, the linear carbonate includes one or more of dimethyl carbonate, diethyl carbonate or ethyl methyl carbonate.

[0012] The present invention also provides a secondary battery, which includes a positive electrode sheet, a negative electrode sheet, a separator, and the electrolyte described in any one of the above examples.

[0013] In an example of the present invention, the upper limit of the operating voltage of the secondary battery is above 4.15V.

[0014] In one example of the present invention, the negative electrode plate includes a negative electrode active material, the negative electrode active material includes a silicon material, and the mass percentage of the silicon material in the negative electrode active material is less than or equal to 5%; in the electrolyte, the mass percentage of the fluoroethylene carbonate relative to the solvent is 0.5% to 3%.

[0015] In one example of the present invention, the electrolyte also includes additives, and the additives include 1,3-propane sultone and vinyl sulfate; wherein the mass percentage of the 1,3-propane sultone relative to the electrolyte is less than or equal to 0.5%, and the mass percentage of the vinyl sulfate relative to the electrolyte is greater than or equal to 0.8%.

[0016] The electrolyte provided by the present invention adjusts the content of components in the electrolyte, and improves the oxidation resistance and electrochemical stability of the electrolyte by reducing the component with the worst oxidation resistance in the electrolyte (i.e., ethylene carbonate), so as to reduce the probability of the electrolyte having side reactions with the positive electrode active material at high voltage, thereby improving the gas production problem in the battery cycle process. At the same time, the electrolyte compensates for the decrease in dielectric constant and conductivity caused by the reduction of ethylene carbonate by optimizing the content of other alternative components (propylene carbonate, fluoroethylene carbonate), and ensures that the lithium ion transmission capacity of the electrolyte and the film-forming effect at the negative electrode interface do not deteriorate, thereby ensuring the cycle performance of the battery. The electrolyte can be well matched to batteries with high operating voltages, and while taking into account the protection that the initial impedance of the battery does not deteriorate, it effectively improves the problems of poor battery cycle performance and large cycle gas production. DETAILED DESCRIPTION

[0017] The following is an explanation of the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the features in the following embodiments and the embodiments can be combined with each other without conflict. It should also be understood that the terms used in the embodiments of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods for which specific conditions are not specified in the following examples are usually carried out under conventional conditions or according to the conditions recommended by the manufacturers.

[0018] For simplicity, only some numerical ranges are explicitly disclosed herein, and each point or single value between the end points of the range is included in the range. Therefore, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unspecified range. It should be noted that in the present invention, the content of each component in the electrolyte represents the mass percentage of the component relative to the solvent or the electrolyte.

[0019] The inventors have found that in current secondary batteries with high energy density positive electrodes (such as lithium-ion batteries with high nickel ternary positive electrode systems), a large amount of additives are generally added to the electrolyte used to stabilize the positive electrode interface to reduce the side reactions between the electrolyte and the positive electrode active material. However, the additives that can stabilize the positive electrode interface generally have high impedance characteristics, which will have a negative impact on the conductive properties of the electrolyte. Therefore, although the electrolyte used in the prior art can inhibit the battery's cycle gas production, it also causes the battery's DC resistance (DCR) and cycle capacity to decrease.

[0020] To this end, the present invention provides an electrolyte, which improves the oxidation resistance and electrochemical stability of the electrolyte by reducing the content of the ethylene carbonate component with the worst oxidation resistance in conventional solvents, thereby reducing the side reactions of the electrolyte with the positive electrode active material under high voltage and improving the gas production problem in the battery cycle process; at the same time, the electrolyte also appropriately increases the content of alternative components such as propylene carbonate and fluoroethylene carbonate to compensate for the decrease in dielectric constant and conductivity caused by the reduction in ethylene carbonate content, ensuring that the lithium ion transmission capacity of the electrolyte and the film-forming effect at the negative electrode interface do not deteriorate, and maintaining the cycle performance of the protected battery. Different from the existing method of adding a large amount of high-impedance additives to suppress battery gas production, this electrolyte does not need to use high-impedance additives to stabilize the interface of the positive electrode active material, so it can take into account both improving the battery cycle life and the cycle gas production problem in high-working voltage batteries, and ensure that the initial impedance of the battery does not deteriorate.

[0021] The electrolyte includes a lithium salt and a solvent, and the solvent includes ethylene carbonate (EC), propylene carbonate (PC), fluoroethylene carbonate (FEC) and linear carbonate.

[0022] The mass percentage of ethylene carbonate (EC) relative to the solvent is any value between 2% and 10%; for example, it can be 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%. A small amount of ethylene carbonate components added to the solvent can enhance the antioxidant capacity of the electrolyte at high temperature and high voltage, and at the same time can ensure the film-forming effect of the solid electrolyte interface film (SEI) of the electrolyte on the surface of the negative electrode. Among them, if the content of ethylene carbonate in the solvent is too high, it will reduce the antioxidant stability of the electrolyte, cause an increase in positive electrode side reactions, and worsen the cycle gas production of the battery; if the content of ethylene carbonate in the solvent is too low, it will reduce the conductivity of the electrolyte, affect the kinetic properties of the electrolyte, and lead to insufficient film formation of the SEI film on the surface of the negative electrode, so that the negative electrode will be co-embedded with the solvent during charge and discharge, resulting in the battery being unable to perform normal charge and discharge cycles, and the battery cycle gas production is also abnormal.

[0023] The sum of the mass of propylene carbonate (PC) and fluoroethylene carbonate (FEC) relative to the mass percentage of the solvent is any value between 10% and 30%; for example, it can be 10%, 13%, 15%, 17%, 20%, 23%, 25%, 27% or 30%. Propylene carbonate and fluoroethylene carbonate added appropriately in the solvent can serve as substitute components for ethylene carbonate, making up for the decrease in dielectric constant and conductivity caused by the reduction in ethylene carbonate content, and ensuring that the lithium ion transmission capacity of the electrolyte and the film-forming effect at the negative electrode interface are not deteriorated.

[0024] In some embodiments, the mass percentage of propylene carbonate relative to the solvent is any value between 7% and 27%, for example, it can be 7%, 10%, 13%, 15%, 17%, 20%, 23%, 25% or 27%. An appropriate amount of propylene carbonate in the solvent can ensure the conductivity of the electrolyte and reduce the risk of damage to the negative electrode. Among them, when the content of propylene carbonate in the solvent is too low, the dielectric constant of the electrolyte decreases, the conductivity decreases, and the charge and discharge cycle of the battery is negatively affected; when the content of propylene carbonate in the solvent is too high, the excess propylene carbonate is not only difficult to form a SEI film on the surface of the carbon negative electrode active material, but also continues to reduce and decompose with the surface of the carbon negative electrode active material under low voltage conditions, increasing the risk of the electrolyte depriving the negative electrode active material, affecting the cycle life and cycle gas production of the battery.

[0025] In some embodiments, the mass percentage of fluoroethylene carbonate relative to the solvent is any value between 0.5% and 3%, for example, it can be 0.5%, 0.7%, 1%, 1.2%, 1.4%, 1.5%, 1.7%, 2%, 2.2%, 2.4%, 2.5%, 2.7% or 3%. An appropriate amount of fluoroethylene carbonate in the solvent can take into account both the protection effect of the electrolyte on the negative electrode interface and the control of the battery's cyclic gas production. Among them, when the content of fluoroethylene carbonate in the solvent is too high, the excess fluoroethylene carbonate is easy to decompose at high temperature to produce hydrogen fluoride, which will cause the battery's cyclic gas production to increase; when the content of fluoroethylene carbonate in the solvent is too low, too little fluoroethylene carbonate cannot play the role of negative electrode film formation to protect the negative electrode, which is easy to cause propylene carbonate to embed into the carbon negative electrode active material, destroying the battery's cyclic stability.

[0026] In some embodiments, the electrolyte further includes additives, including 1,3-propane sultone (PS) and dithiothreitol (DTD). The additives help to form a stable SEI interface film at the negative electrode interface, which can further enhance the film-forming effect of the electrolyte at the negative electrode interface, enhance the protective effect on the negative electrode interface, and improve the charge and discharge cycle performance of the battery.

[0027] In some embodiments, the mass percentage of 1,3-propane sultone relative to the electrolyte is less than or equal to 0.5%, for example, it can be 0.1%, 0.2%, 0.3%, 0.4% or 0.5%; optionally, the mass percentage of 1,3-propane sultone relative to the electrolyte is 0.5%. When the content of 1,3-propane sultone in the electrolyte is within the above range, it can promote the formation of SEI film at the negative electrode interface without causing other negative effects on the cycle performance of the battery.

[0028] In some embodiments, the mass percentage of vinyl sulfate relative to the electrolyte is greater than or equal to 0.8%, for example, it can be 0.8%, 0.9%, 1%, 1.2% or 1.5%, etc. The content of vinyl sulfate in the electrolyte must be sufficient. If the content of vinyl sulfate in the electrolyte is too low, it will lead to insufficient film formation of the negative electrode interface SEI film, which will have a negative impact on the battery cycle life and gas production.

[0029] Further, in one example, the mass percentage of vinyl sulfate relative to the electrolyte is any value between 0.8% and 1%, for example, 0.8%, 0.85%, 0.9%, 0.95% or 1%.

[0030] In some embodiments, linear carbonate includes one or more of dimethyl carbonate (DMC), diethyl carbonate (DEC) or ethyl methyl carbonate (EMC), that is, linear carbonate can be any one of the above-mentioned types, such as dimethyl carbonate, diethyl carbonate or ethyl methyl carbonate; linear carbonate can also be a composition of any two or three of the above-mentioned types, such as a composition of dimethyl carbonate and diethyl carbonate, or a composition of diethyl carbonate and ethyl methyl carbonate, or a composition of dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate. Optionally, in an example, linear carbonate includes dimethyl carbonate and ethyl methyl carbonate. It should be noted that when linear carbonate is a composition, there is no restriction on the ratio between the components in the composition, and it can be mixed in any proportion.

[0031] In addition, it should be noted that the lithium salt in the electrolyte can be selected from conventional lithium salts in the art. For example, the lithium salt is selected from lithium hexafluorophosphate (LiPF 6 ), lithium bis(fluorosulfonyl)imide (LiFSI), lithium tetrafluoroborate (LiBF 4 ), lithium bis(oxalatoborate) (LiBOB), lithium bis(fluorooxalatoborate) (LiODFB) and lithium bis(trifluoromethylsulfonyl)imide (LiTFSI). Preferably, the lithium salt is selected from lithium hexafluorophosphate (LiPF 6 ), or lithium hexafluorophosphate (LiPF 6 ) as the main component, and other lithium salts are added in appropriate amounts to take advantage of their advantages and improve the performance of the electrolyte. The concentration of the lithium salt can be set according to the conventional selection in the field. In some embodiments, the mass percentage of the lithium salt in the electrolyte is 8% to 20%. Further, the mass percentage of the lithium salt in the electrolyte is any value between 10% and 17%, such as 10%, 13%, 14%, 15% or 17%, etc.

[0032] The electrolyte of the present invention can be prepared according to a conventional preparation method, for example, the electrolyte is prepared in a glove box, the argon or nitrogen content in the glove box is 99.999%, the actual oxygen content in the glove box is 0.1ppm, and the moisture content is less than 10ppm. In the glove box, the solvent is mixed and stirred, and then the lithium salt is added to the mixed solvent under stirring conditions, and the stirring is continued until the lithium salt is completely dissolved, and finally the additive can be added and stirred evenly.

[0033] The present invention also provides a secondary battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and the electrolyte described in any one of the above embodiments. During the battery charging and discharging process, lithium ions are inserted and removed back and forth between the positive electrode sheet and the negative electrode sheet, and the separator is arranged between the positive electrode sheet and the negative electrode sheet to play a role of isolation; the electrolyte plays a role of conducting lithium ions between the positive electrode sheet and the negative electrode sheet.

[0034] The composition and preparation method of the secondary battery are described in detail below:

[0035] The positive electrode sheet includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector. Among them, the positive current collector is, for example, a foil formed after surface treatment of nickel, titanium, aluminum, nickel, silver, stainless steel or carbon. In addition to the foil, the positive current collector can also be used in any one or more combinations of various forms such as film, mesh, porous, foam or non-woven fabric. Among them, the thickness of the positive current collector is, for example, 8μm-15μm. In one embodiment, the positive current collector is, for example, aluminum foil, and the thickness of the aluminum foil is, for example, 13μm. The positive current collector has two surfaces opposite to each other in its own thickness direction, and the positive active material layer is disposed on any one or both of the two opposite surfaces of the positive current collector. The positive active material layer includes a positive active material, a positive conductive agent and a positive binder. There is no specific restriction on the positive active material, the positive conductive agent and the positive binder here, and those skilled in the art can choose according to actual needs.

[0036] As an example, the positive electrode active material can be selected from ternary materials, lithium-containing phosphates, and spinel materials, wherein the ternary materials include lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese oxide doped with metal ions, lithium nickel cobalt aluminum oxide doped with metal ions, etc.; lithium-containing phosphates include lithium iron manganese phosphate, lithium iron phosphate, lithium manganese phosphate, etc. The positive electrode binder is selected from polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE), etc. The positive electrode conductive agent is selected from one of carbon black, acetylene black, graphene, carbon nanotubes, carbon nanofibers, etc., or a combination of two or more of them mixed in any proportion.

[0037] The negative electrode plate includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector. The negative electrode current collector can be made of a material with good electrical conductivity and mechanical strength, such as copper foil. The negative electrode current collector has two surfaces opposite to each other in its own thickness direction, and the negative electrode active material layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material, a negative electrode conductive agent, a negative electrode binder and a thickener. The specific types of the negative electrode active material, the negative electrode conductive agent and the negative electrode binder are not specifically limited here. Materials known in the art that can be used in lithium-ion batteries can be used, and those skilled in the art can select according to actual needs.

[0038] As an example, the negative electrode active material is selected from one or more combinations of carbon materials and silicon materials. For example, carbon materials include hard carbon, artificial graphite, natural graphite, etc., and silicon materials include elemental silicon, silicon oxide compounds, silicon carbon compounds, etc. The negative electrode conductive agent is selected from one of carbon black, acetylene black, graphene, carbon nanotubes, carbon nanofibers, etc., or a combination of two or more mixed in any proportion. The negative electrode binder is selected from any one of polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), styrene-butadiene rubber (SBR), or a combination of several mixed in any proportion; the thickener is selected from carboxymethyl cellulose CMC-Na or CMC-Li.

[0039] The isolation membrane is selected from conventional types in the art, for example, PE or PP porous membrane can be selected as the isolation membrane, the thickness of the isolation membrane is 9 to 18 μm, the air permeability is 180 s / 100 mL to 380 s / 100 mL; the porosity is 30% to 50%.

[0040] The battery assembly is carried out according to conventional methods, for example, after preparation, the negative electrode sheet, the separator, and the positive electrode sheet are stacked in order, and placed in an aluminum plastic film to obtain a dry cell, and the dry cell is baked at 80°C to remove water. The prepared electrolyte is injected into the dry cell and packaged to obtain a finished lithium-ion battery.

[0041] In some embodiments, the upper limit of the working voltage of the secondary battery is greater than or equal to 4.15V. For example, in one example, the working voltage of the secondary battery is 2.5V to 4.25V. Since the upper limit of the working voltage of the secondary battery is mainly determined by the positive electrode active material, the positive electrode active material in this embodiment can be selected from conventional high energy density positive electrode materials in the art, such as high nickel ternary materials or nickel manganese spinel materials. Among them, the high nickel ternary material is LiNi a Co b M 1-a-b O 2 , 0.9≤a<1, 0<b≤0.1, M element is selected from at least one of Mn, Al, Ti, Zr, Cu, Ca, Ta and Mg, for example, the high nickel ternary material can be LiNi 0.9 Co 0.05 Mn 0.05 O 2 .

[0042] Among them, taking the high-nickel ternary material as an example, as the nickel content in the cathode active material increases, the stability of the cathode becomes worse and worse, manifested as an increase in the oxidizing property on the cathode surface and an increase in the catalytic activity caused by the increase in nickel content. During the charge and discharge cycle of the battery, the cathode active material is prone to side reactions with the electrolyte, resulting in the collapse of the lattice at the cathode interface and the release of oxygen. However, in this embodiment, based on its good conductivity and antioxidant ability at high temperature and high voltage, the electrolyte can be well adapted to the secondary battery with a high-energy density cathode system, effectively reducing the probability of side reactions with the cathode active material in a high-voltage environment above 4V while ensuring the conductivity of the battery, thereby effectively suppressing the increase in cyclic gas production of the battery, increasing the cycle life of the battery, and taking into account ensuring that the initial impedance of the battery does not deteriorate.

[0043] In some embodiments, the negative electrode active material is a composition of graphite and silicon material, and the silicon material includes at least one of elemental silicon, silicon oxide compound, and silicon-carbon composite. Among them, the silicon oxide compound can be SiO x (0 < x < 2). The mass percentage of the silicon material in the negative electrode active material is less than or equal to 5%, for example, it can be 1%, 2%, 3%, 4%, or 5%.

[0044] In the above embodiments, due to the increase in the content of the silicon material in the negative electrode active material, the potential volume expansion of the negative electrode plate increases during the charge and discharge cycle of the battery. By adding a suitable fluoroethylene carbonate component to the electrolyte, an SEI film is continuously formed at the interface of the negative electrode active material to prevent the over-expanded negative electrode from damaging the original SEI film layer on the interface and being exposed in the electrolyte, thereby realizing the protection of the negative electrode during the battery cycle. In one example, the mass percentage of fluoroethylene carbonate relative to the solvent is 0.5% to 3%.

[0045] In addition, in the above embodiments, the electrolyte also further helps the electrolyte form a stable SEI interface film at the negative electrode interface through the additive component, improves the film-forming effect of the electrolyte at the negative electrode interface, enhances the protection effect on the negative electrode interface, and improves the charge and discharge cycle performance of the battery. Among them, the additive includes 1,3-propane sultone and vinylene sulfate. The mass percentage of 1,3-propane sultone relative to the electrolyte is less than or equal to 0.5%, and the mass percentage of vinylene sulfate relative to the electrolyte is greater than or equal to 0.8%. Optionally, in one example, the mass percentage of vinylene sulfate relative to the electrolyte is 0.8% to 1%.

[0046] The technical solutions of the present invention will be described in detail below through several specific examples and comparative examples. Unless otherwise specified, the raw materials and reagents used in the following examples are all commercially available products or can be prepared by conventional methods in the art.

[0047] Example 1

[0048] This embodiment provides a secondary battery, the composition and preparation method of the secondary battery are as follows:

[0049] Preparation of electrolyte: In an argon atmosphere glove box with a water content of <10ppm, battery-grade ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), and fluoroethylene carbonate (FEC) are mixed in a mass ratio of 10:10:57:20:3 to form a solvent. In the prepared solvent, taking the total mass of the solvent as 100%, the mass ratio of ethylene carbonate (EC) to the solvent is 10%, the mass ratio of propylene carbonate (PC) to the solvent is 10%, the mass ratio of ethyl methyl carbonate (EMC) to the solvent is 57%, the mass ratio of fluoroethylene carbonate (FEC) to the solvent is 3%, and the mass ratio of diethyl carbonate (DEC) to the solvent is 20%. Then weigh a certain mass of lithium hexafluorophosphate (LiPF 6 ) as the main lithium salt is added to the above-prepared mixed solvent; finally, a certain amount of 1,3-propane sultone (PS) and dithiothioate (DTD) are added as additives, and finally mixed evenly to obtain an electrolyte. As shown in Table 1, based on the total mass of the electrolyte being 100%, the mass ratio of lithium hexafluorophosphate to the electrolyte is 14%, the mass ratio of 1,3-propane sultone (PS) to the electrolyte is 0.5%, and the mass ratio of dithiothioate (DTD) to the electrolyte is 1%. And it is calculated that the mass ratio of the total amount of solvent to the electrolyte is 84.5%.

[0050] Preparation of positive electrode sheet: LiNi 0.9 Co 0.05 Mn 0.05 O 2 , positive electrode conductive agent Super P and positive electrode binder polyvinylidene fluoride are mixed in a mass ratio of 98:1:1, and solvent N-methylpyrrolidone is added, and stirred in a vacuum mixer until it becomes uniform and transparent to obtain positive electrode slurry. The positive electrode slurry is evenly coated on aluminum foil, and the aluminum foil is dried at room temperature and then transferred to an oven for drying, and then cold pressed and cut to obtain positive electrode sheets.

[0051] Preparation of negative electrode sheet: negative electrode active material, negative electrode conductive agent Super P, negative electrode thickener sodium carboxymethyl cellulose (CMC-Na), negative electrode binder styrene butadiene rubber (SBR) are mixed in a mass ratio of 96:1:1:2 and fully stirred in a vacuum mixer to obtain negative electrode slurry; the negative electrode slurry is evenly coated on the negative electrode current collector copper foil, dried at room temperature, and then transferred to an oven for drying, and the negative electrode sheet is obtained through cold pressing, slitting and other processes. Among them, the negative electrode active material includes artificial graphite and silicon oxide compound SiO x(0 < x < 2), the mass percentage of artificial graphite relative to the negative electrode active material is 97%, and the mass percentage of silicon oxide relative to the negative electrode active material is 3%.

[0052] Selection of separator: A polypropylene film with a thickness of 12 μm is used as the separator.

[0053] Preparation of the battery: Stack the positive electrode sheet, separator, and negative electrode sheet in sequence, with the separator in the middle of the positive electrode sheet and the negative electrode sheet to play an isolation role, and stack them to obtain a bare battery core. Then wrap it with an aluminum-plastic film, transfer it to a vacuum oven, dry it at 120 °C, inject 3.0 g / Ah of electrolyte and then seal it, and carry out electrolytic liquefaction to prepare a lithium-ion secondary battery with a capacity of 1 Ah.

[0054] Example 2

[0055] This example provides a secondary battery with the same system as Example 1. The difference between this example and Example 1 is that the mass ratio of EC, PC, and FEC in the solvent is adjusted to 2%, 10%, and 3%, and the content of EMC is adjusted accordingly to maintain the same total amount of electrolyte as in Example 1.

[0056] Example 3

[0057] This example provides a secondary battery with the same system as Example 1. The difference between this example and Example 1 is that the mass ratio of EC, PC, and FEC in the solvent is adjusted to 10%, 7%, and 3%, and the content of EMC is adjusted accordingly to maintain the same total amount of electrolyte as in Example 1.

[0058] Example 4

[0059] This example provides a secondary battery with the same system as Example 1. The difference between this example and Example 1 is that the mass ratio of EC, PC, and FEC in the solvent is adjusted to 5%, 27%, and 3%, and the content of EMC is adjusted accordingly to maintain the same total amount of electrolyte as in Example 1.

[0060] Example 5

[0061] This example provides a secondary battery with the same system as Example 1. The difference between this example and Example 1 is that the mass ratio of EC, PC, and FEC in the solvent is adjusted to 10%, 10%, and 0.5%, and the content of EMC is adjusted accordingly to maintain the same total amount of electrolyte as in Example 1.

[0062] Example 6

[0063] This example provides a secondary battery with the same system as Example 1. The difference between this example and Example 1 is that in the electrolyte, the mass percentage of DTD relative to the electrolyte is adjusted to 0.8%.

[0064] Example 7

[0065] This embodiment provides a secondary battery of the same system as that of Embodiment 1. The difference between this embodiment and Embodiment 1 is that the mass percentage of the silicon oxide compound in the negative electrode active material is adjusted to 5%.

[0066] Comparative Example 1

[0067] This comparative example provides a secondary battery of the same system as that of Example 1. The difference between this comparative example and Example 1 is that EC is not added to the solvent, the mass ratios of PC, DEC, and FEC in the solvent are adjusted to 10%, 20%, and 3%, and the content of EMC is adaptively adjusted to maintain the total amount of the electrolyte the same as that of Example 1.

[0068] Comparative Example 2

[0069] This comparative example provides a secondary battery of the same system as Example 1. The difference between this comparative example and Example 1 is that the mass ratios of EC, DEC, and FEC in the solvent are adjusted to 15%, 10%, and 3%, and the content of EMC is adaptively adjusted to maintain the total amount of the electrolyte the same as that of Example 1.

[0070] Comparative Example 3

[0071] This comparative example provides a secondary battery of the same system as Example 1. The difference between this comparative example and Example 1 is that the mass ratios of EC, PC, and FEC in the solvent are adjusted to 10%, 5%, and 3%, and the content of EMC is adaptively adjusted to maintain the total amount of electrolyte the same as Example 1.

[0072] Comparative Example 4

[0073] This comparative example provides a secondary battery of the same system as Example 1. The difference between this comparative example and Example 1 is that the mass ratios of EC, PC, and FEC in the solvent are adjusted to 10%, 30%, and 3%, and the content of EMC is adaptively adjusted to maintain the total amount of electrolyte the same as Example 1.

[0074] Comparative Example 5

[0075] This comparative example provides a secondary battery of the same system as that of Example 1. The difference between this comparative example and Example 1 is that FEC is not added to the solvent, the mass ratio of EC and PC in the solvent is adjusted to 10% and 10%, and the content of EMC is adaptively adjusted to maintain the total amount of electrolyte the same as that of Example 1.

[0076] Comparative Example 6

[0077] This comparative example provides a secondary battery of the same system as Example 1. The difference between this comparative example and Example 1 is that the mass ratio of EC, PC, and FEC in the solvent is adjusted to 10%, 10%, and 5%, and the content of EMC is adaptively adjusted to maintain the total amount of electrolyte the same as Example 1.

[0078] Comparative Example 7

[0079] This comparative example provides a secondary battery of the same system as that of Example 1. The difference between this comparative example and Example 1 is that in the electrolyte, the mass percentage of DTD relative to the electrolyte is adjusted to 0.5%.

[0080] Comparative Example 8

[0081] This comparative example provides a secondary battery of the same system as that of Example 1. The difference between this comparative example and Example 1 is that in the electrolyte, the mass percentage of PS relative to the electrolyte is adjusted to 1%.

[0082] Comparative Example 9

[0083] This comparative example provides a secondary battery of the same system as that of Example 1. The difference between this comparative example and Example 1 is that the mass percentage of the silicon oxide compound in the negative electrode active material is adjusted to 6%.

[0084] Comparative Example 10

[0085] This comparative example provides a secondary battery of the same system as that of Example 1. The difference between this comparative example and Example 1 is that no PC is added to the solvent, the mass ratio of EC and FEC in the solvent is adjusted to 30% and 3%, and the content of EMC is adaptively adjusted to maintain the total amount of electrolyte the same as that of Example 1.

[0086] The secondary batteries provided by Examples 1 to 9 and Comparative Examples 1 to 10 were subjected to performance tests, wherein the battery parameters of Examples 1 to 9 and Comparative Examples 1 to 10 are shown in Table 1, the test results are shown in Table 2, and the test method is as follows:

[0087] (1) Battery DC resistance (DCR) test: In an oven at a specified temperature (high temperature 45°C), discharge the secondary battery at a 1C rate current to adjust the capacity to 50% SOC (State Of Charge), and then continue to discharge the secondary battery at a 4C rate current for 30 seconds, and detect the difference between the updated stable voltage and the original platform voltage. The ratio of its value to the 4C current value is the DC resistance of the battery. The DCR test result after the battery is fully charged for the first time is the initial DCR of the battery.

[0088] (2) Battery cycle life test: In an oven at a specified temperature (high temperature 45°C), cyclic charge and discharge are performed in the test voltage range of 2.5V (discharge cut-off voltage) to 4.25V (charge cut-off voltage) at a current rate of 1C, and the discharge capacity of the battery is recorded in each cycle. The test is terminated when the battery cycle capacity reaches 90% of the first cycle capacity, and the number of battery cycles is recorded.

[0089] (3) Battery cycle gas production test: In an oven at a specified temperature (high temperature 45°C), perform cyclic charge and discharge at a current rate of 1C in the test voltage range of 2.5V (discharge cut-off voltage) to 4.25V (charge cut-off voltage), record the discharge capacity of the battery in each cycle, and end the test when the battery cycle capacity reaches 90% of the first cycle capacity. Record the volume change of the battery before and after the cycle, calculate the battery volume growth rate = (volume after cycle - volume before cycle) / volume before cycle, and use the battery volume growth rate as the cycle gas production measurement indicator.

[0090] Table 1: Electrolyte and negative electrode active material components in Examples 1 to 9 and Comparative Examples 1 to 10.

[0091]

[0092] Table 2: Battery performance test results of Examples 1 to 9 and Comparative Examples 1 to 10.

[0093]

[0094]

[0095] Comparative Example 10 is an electrolyte solution used in the industry for high-nickel ternary positive electrode system batteries. Comparing the test results of Example 1 with those of Comparative Example 10, the high-temperature cycle life and high-temperature cycle gas production of the battery provided by Example 1 are both better than those of Comparative Example 10. It can be seen that the electrolyte solution of the present application has better advantages in high energy density batteries.

[0096] By comparing the test results of Examples 1 and 2 with Comparative Examples 1 and 2, it can be known that the EC content in the electrolyte has a great influence on the battery cycle performance. When the EC content in the solvent is in the appropriate range of 2% to 10%, it can enhance the antioxidant capacity of the electrolyte at high temperature and high voltage, and at the same time, it can also ensure the film-forming effect of the SEI film layer of the electrolyte on the surface of the negative electrode, thereby extending the battery cycle life and inhibiting the battery cycle gas production. When the EC content in the solvent is higher than 10%, the antioxidant stability of the electrolyte will be reduced, causing an increase in positive electrode side reactions and increasing the battery charge and discharge cycle gas production. When the EC content in the solvent is lower than 2%, the conductivity of the electrolyte will be reduced, affecting the kinetic performance of the electrolyte and increasing the DC resistance of the battery; at the same time, it will also lead to insufficient film formation of the SEI film on the surface of the negative electrode, causing the negative electrode to be co-embedded with the solvent during charge and discharge, resulting in a significant attenuation of the battery capacity during the charge and discharge cycle.

[0097] By comparing the test results of Examples 1, 3, 4 and Comparative Examples 3, 4, it can be seen that when the sum of the contents of PC and FEC in the solvent is in the appropriate range of 10% to 30%, it can effectively compensate for the decrease in dielectric constant and conductivity caused by the reduction in EC content, and ensure that the lithium ion transmission capacity of the electrolyte and the film-forming effect at the negative electrode interface are not deteriorated.

[0098] Moreover, by comparing the test results, it can be seen that when the PC content in the solvent is in the appropriate range of 7% to 27%, it will not have a negative impact on the cycle life and DC resistance of the battery. Among them, when the PC content in the solvent is less than 7%, the dielectric constant of the electrolyte decreases, the conductivity decreases, and the DC resistance of the battery increases accordingly; when the PC content in the solvent is higher than 27%, the excess PC component will undergo a continuous reduction and decomposition reaction with the graphite material of the negative electrode under low voltage conditions, increasing the risk of the electrolyte depriving the negative electrode active material, causing the battery cycle capacity to decay.

[0099] By comparing the test results of Examples 1 and 5 with Comparative Examples 5 and 6, it can be seen that when the content of FEC in the solvent is within the appropriate range of 0.5% to 3%, the electrolyte can take into account both the protection effect of the electrolyte on the negative electrode interface and the control of the battery's cycle gas production. When the content of FEC in the solvent is greater than 3%, the excess FEC is easily decomposed at high temperatures to produce hydrogen fluoride, which will cause the battery cycle gas production to increase; when the content of FEC in the solvent is less than 0.5%, too little FEC cannot play the role of negative electrode film formation to protect the negative electrode, and it is easy to cause propylene carbonate to embed into the carbon negative electrode active material, destroying the battery's cycle stability and causing the battery cycle capacity to decay.

[0100] By comparing the test results of Examples 1 and 6 with Comparative Examples 7 and 8, it can be seen that the dosage of additives DTD and PS in the electrolyte will have a substantial impact on the cycle performance of the battery. When the content of the additive DTD in the electrolyte is too little (less than 0.8%), it will lead to insufficient film formation of the SEI film at the negative electrode interface, which will have a negative impact on the battery cycle life and gas production; when the content of the additive PS in the electrolyte is too high (less than 0.5%), it will worsen the high-temperature cycle gas production of the battery.

[0101] By comparing the test results of Examples 1 and 7 with Comparative Example 9, it can be seen that the amount of FEC used for the silicon material in the negative electrode active material has a certain requirement. When there is more silicon material in the negative electrode, its volume expansion during the cycle is obvious, and a certain amount of FEC in the electrolyte is required to continuously form the SEI film at the interface of the negative electrode active material to avoid the excessive expansion of the negative electrode from destroying the original SEI film layer on the interface and exposing it in the electrolyte, thereby protecting the negative electrode during the battery cycle. If the silicon compound content exceeds 5%, the protective effect of the electrolyte proposed in the present invention on the negative electrode will no longer be obvious.

[0102] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. An electrolyte, characterized in that: include: Lithium salts; a solvent, the solvent comprising ethylene carbonate, propylene carbonate, fluoroethylene carbonate and linear carbonate; The mass percentage of the ethylene carbonate relative to the solvent is 2% to 10%, and the mass percentage of the sum of the mass of the propylene carbonate and the fluoroethylene carbonate relative to the solvent is 10% to 30%.

2. The electrolyte according to claim 1, characterized in that: The mass percentage of the fluoroethylene carbonate relative to the solvent is 0.5% to 3%.

3. The electrolyte according to claim 1, characterized in that: The electrolyte further includes an additive, wherein the additive includes 1,3-propane sultone and vinyl sulfate.

4. The electrolyte according to claim 3, characterized in that: The mass percentage of the 1,3-propane sultone relative to the electrolyte is less than or equal to 0.5%, and the mass percentage of the vinyl sulfate relative to the electrolyte is greater than or equal to 0.8%.

5. The electrolyte according to claim 4, characterized in that: The mass percentage of the vinyl sulfate relative to the electrolyte is 0.8% to 1%.

6. The electrolyte according to claim 1, characterized in that: The linear carbonate includes one or more of dimethyl carbonate, diethyl carbonate or ethyl methyl carbonate.

7. A secondary battery, characterized in that: The invention comprises a positive electrode sheet, a negative electrode sheet, a separator and the electrolyte according to any one of claims 1 to 6.

8. The secondary battery according to claim 7, characterized in that: The upper limit of the operating voltage of the secondary battery is above 4.15V.

9. The secondary battery according to claim 7, characterized in that: The negative electrode plate includes a negative electrode active material, the negative electrode active material includes a silicon material, and the mass percentage of the silicon material in the negative electrode active material is less than or equal to 5%; in the electrolyte, the mass percentage of the fluoroethylene carbonate relative to the solvent is 0.5% to 3%.

10. The secondary battery according to claim 9, characterized in that: The electrolyte also includes additives, including 1,3-propane sultone and vinyl sulfate; wherein the mass percentage of the 1,3-propane sultone relative to the electrolyte is less than or equal to 0.5%, and the mass percentage of the vinyl sulfate relative to the electrolyte is greater than or equal to 0.8%.