Aqueous dispersion composition

By using a composition of modified polyolefin, a non-ionic emulsifier containing nitrogen and an alkaline substance in the aqueous coating, the problem of insufficient adhesion of the aqueous coating under low-temperature baking conditions is solved, and the polyolefin-based group is realized The high peel strength and high adhesion of the material are suitable for automotive coatings and adhesives, improving the water resistance and stability of the coating film.

CN118900903AActive Publication Date: 2024-11-05TOYOBO MC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380027819.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-24
Publication Date
2024-11-05
Estimated Expiration
2043-03-24

AI Technical Summary

Technical Problem

The existing water-based coatings lack adhesion to polyolefin substrates under low temperature baking conditions, resulting in low adhesion, making it difficult to meet the demand for high adhesion in automotive coating production lines. At the same time, it can improve adhesion in low temperature baking. Challenge of force.

Method used

The aqueous dispersion composition containing modified polyolefins, non-ionic emulsifiers containing nitrogen and alkaline substances is used. The Z-average particle size of the modified polyolefin is less than 200 nm, the weight average molecular weight is more than 60,000, and non-nitrogen containing nitrogen is non- The amount of the ionic emulsifier is 10 to 45 mass %, and the amount of the alkaline substance is added appropriately to improve adhesion and water resistance.

Benefits of technology

It realizes high peel strength and high adhesion to polyolefin substrates under low temperature (80-90°C) baking conditions, and is suitable for automotive coatings and adhesives, improving the water resistance and storage stability of the coating film. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005043227060000161
    Figure BDA0005043227060000161
  • Figure BDA0005043227060000211
    Figure BDA0005043227060000211
Patent Text Reader

Abstract

The present invention relates to an aqueous dispersion composition which is aqueous, exhibits high peel strength when baked at a low temperature (80-90 DEG C), high adhesion, and good water resistance with respect to a polyolefin substrate that is difficult to adhere, has a weight-average molecular weight of 60,000 or more as measured by GPC, and is characterized by containing an alpha, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, beta, the present invention relates to an aqueous dispersion composition comprising (A) a modified polyolefin in which the modification amount of a [beta]-unsaturated carboxylic acid and / or an anhydride thereof is less than 1.0 mass%, (B) a nitrogen-containing nonionic emulsifier, and (C) a basic substance, wherein the Z-average particle diameter of the aqueous dispersion composition is 200 nm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an aqueous dispersion composition suitable for a coating agent, a primer, a paint, an ink, an adhesive and the like, comprising a polyolefin resin, a nitrogen-containing nonionic emulsifier and an alkaline substance. Background Art

[0002] Polyolefin resins such as polypropylene are widely used in automobile parts, various films, various molded products, etc. because they are cheap and have excellent properties. However, polyolefin resins are non-polar, so there are problems such as difficulty in painting and bonding. Therefore, modified polyolefins such as acid-modified polyolefins and acid-modified chlorinated polyolefins are being developed for painting, printing, laminating or bonding films of polyolefin resins.

[0003] In addition, due to the rise of global environmental protection activities, the entire paint industry is actively taking measures to reduce CO2, which is the cause of global warming, by reducing VOC in paint or reducing energy consumption in baking and drying furnaces. In the automotive painting production line, the use of water-based or low-VOC paints in each layer is also increasing.

[0004] Compared with water-based paints, solvent-based paints can be expected to have improved adhesion and good adhesion due to the penetration and diffusion effect of the solvent into the substrate or the swelling effect of the solvent into the substrate. In contrast, water-based paints cannot be expected to have the above-mentioned effects, so there is a problem of reduced adhesion.

[0005] On the other hand, in recent years, due to the change in the composition of bumper substrates to reduce material costs and reduce thickness, bumper substrates have become more difficult to adhere to paint on the substrates, and there is a further demand for improved adhesion of water-based paints to materials that are difficult to adhere to.

[0006] Furthermore, as a measure to reduce energy consumption as described above, studies are also being conducted to lower the baking temperature in automobile coating lines. In water-based coating lines, there is a problem of improving the adhesion during low-temperature baking from the viewpoint of the adhesion as described above. [Prior art literature] [Patent Literature]

[0007] [Patent Document 1] Japanese Patent No. 5023557 [Patent Document 2] Japanese Patent Application Publication No. 2005-126615 Summary of the invention [Problems to be solved by the invention]

[0008] Patent document 1 discloses a method for forming a coating, characterized in that a water-based modified polyolefin resin composition is applied to a substrate and baked and dried at 80 to 90°C, wherein the melting point of the water-based modified polyolefin resin composition is lower than the drying temperature by 19°C or more and 26°C or less. However, there is a problem of insufficient adhesion strength. In addition, Patent document 2 discloses an aqueous dispersion containing a high molecular weight polyolefin and a surfactant, but there is a problem that sufficient adhesion cannot be obtained during low-temperature baking.

[0009] In view of the above, the present invention provides an aqueous dispersion composition which is aqueous and exhibits high peel strength, high adhesion and good water resistance in low temperature (80-90° C.) baking to a polyolefin substrate that is difficult to adhere to.

Methods to solve the problem

[0010] The present inventors have conducted intensive studies and have found that an aqueous dispersion composition containing a specific modified polyolefin (A), a nitrogen-containing nonionic emulsifier (B) and an alkaline substance (C), wherein the Z-average particle size of the modified polyolefin (A) is not more than 200 nm, can solve the above-mentioned problems, thereby completing the present invention. That is, the gist of the present invention is as follows.

[0011] That is, the present invention is an aqueous dispersion composition, characterized in that it contains a modified polyolefin (A), a nitrogen-containing nonionic emulsifier (B) and an alkaline substance (C), wherein the weight average molecular weight of the modified polyolefin (A) measured by GPC is 60,000 or more, and the modification amount is less than 1.0% by mass, and the Z average particle size of the modified polyolefin (A) in the aqueous dispersion composition is 200 nm or less.

[0012] The melting point of the modified polyolefin (A) is preferably 60° C. to 85° C., and the modified polyolefin (A) is preferably chlorine-free.

[0013] The amount of the nitrogen-containing nonionic emulsifier (B) added is preferably 10 to 45% by mass based on 100 parts by mass of the modified polyolefin resin (A).

[0014] When the anionic group-containing water-soluble polymer (D) is contained, the acid value of the anionic group-containing water-soluble polymer (D) is preferably 100 to 500 mg KOH / g-resin, and the content thereof is 0 to 2% by mass based on 100 parts by mass of the modified polyolefin (A).

[0015] The acid-modified polyolefin (A) is preferably a propylene-α-olefin copolymer having a butene content of 2 to 35% by mass in the polyolefin component.

[0016] An adhesive and a coating material containing any of the above-mentioned aqueous dispersions. A coating film formed by removing an aqueous medium from any of the above-mentioned aqueous dispersions.

[0017] A laminate having a layer derived from the above-mentioned coating material or adhesive. [Effects of the invention]

[0018] When the aqueous dispersion composition of the present invention is used as a primer for a polypropylene substrate, it is aqueous and can provide a coating film having high peel strength, high adhesion and water resistance in low temperature (80-90° C.) baking for a polyolefin substrate that is difficult to adhere to, and can be suitable for use in coatings or adhesives, and is particularly suitable for use as a coating for automobiles. DETAILED DESCRIPTION

[0019] The embodiments of the present invention are described in detail below.

[0020] <Modified polyolefin (A)> The modified polyolefin (A) used in the present invention is a polyolefin obtained by acid-modifying a propylene-α-olefin copolymer. Examples of the acid component of the acid-modified polyolefin used in the present invention include α,β-unsaturated carboxylic acids and / or their anhydrides, preferably those obtained by grafting at least one of α,β-unsaturated carboxylic acids and their anhydrides onto a propylene-α-olefin copolymer.

[0021] The propylene-α-olefin copolymer is a copolymer containing propylene and α-olefin as copolymer components, preferably a propylene-1-butene copolymer, or a copolymer in which propylene-1-butene is copolymerized with α-olefin as the main component. As α-olefins other than propylene and butene, for example, one or more of ethylene, isobutylene, 1-pentene, 3-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 4-methyl-1-pentene, vinyl acetate, etc. can be used. Among these α-olefins, ethylene is preferred.

[0022] The propylene-α-olefin copolymer preferably has a propylene component of 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 65% ​​by mass or more. Within the above range, the adhesion (adhesion) to a polyolefin substrate represented by a propylene substrate is good. In addition, the 1-butene component is preferably 2 to 35% by mass in the olefin component. More preferably, it is 3 to 33% by mass, and particularly preferably 5 to 31% by mass. Within this range, a resin having a melting point suitable for a film forming process dried at 80°C to 90°C can be formed.

[0023] As at least one of the α,β-unsaturated carboxylic acids and their anhydrides, for example, maleic acid, itaconic acid, citraconic acid and their anhydrides can be cited. Among them, anhydrides are preferred, and maleic anhydride is more preferred. Specifically, maleic anhydride-modified propylene-butene copolymers, maleic anhydride-modified propylene-ethylene-butene copolymers, etc. can be cited, and these acid-modified polyolefins can be used alone or in combination of two or more.

[0024] The method for producing the acid-modified polyolefin is not particularly limited, and examples thereof include a radical graft reaction (i.e., a reaction in which a radical species is generated in a polymer constituting a main chain and an unsaturated carboxylic acid and anhydride are graft-polymerized using the radical species as a polymerization starting point).

[0025] As free radical initiator, it is not particularly limited, and organic peroxides and azo nitrile can be listed, and organic peroxide is preferably used. As organic peroxide, it is not particularly limited, and di-tert-butyl peroxyphthalate, tert-butyl hydroperoxide, diisopropylbenzene peroxide, benzoyl peroxide, tert-butyl peroxybenzoate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxypivalate, methyl ethyl ketone peroxide, di-tert-butyl peroxide, lauroyl peroxide, etc. can be listed, and as azo nitrile, azobisisobutyronitrile, azobisisopropionitrile, etc. can be listed.

[0026] The acid modification amount of the acid-modified polyolefin is preferably 0.1% by mass or more, particularly preferably 0.3% by mass or more. In addition, it is less than 1.0% by mass, preferably 0.9% by mass or less, particularly preferably 0.8% by mass or less. When it is 0.1% by mass or more, the dispersibility in water tends to be good, and when it is less than 1.0% by mass, the peel strength and water resistance of the coating film relative to the polyolefin substrate are particularly improved.

[0027] The weight average molecular weight (Mw) of the modified polyolefin (A) is 60,000 or more, preferably 70,000 or more, and particularly preferably 80,000 or more. By being 60,000 or more, the cohesive force becomes stronger, and the adhesion (adhesion) and water resistance become good. In addition, there is no particular provision for the upper limit, but it is ideally 150,000 or less. The solubility becomes good, and the preparation of the aqueous dispersion composition tends to become easy. The weight average molecular weight in the present invention refers to the value measured by GPC (gel permeation chromatography). About the specific measurement conditions, it is described in the following examples.

[0028] The modified polyolefin (A) is preferably crystalline. Crystallinity is advantageous because it has stronger cohesive force than amorphous polyolefins and is excellent in adhesion (tackiness), water resistance, heat resistance, and chemical resistance.

[0029] The so-called crystallinity in the present invention refers to a substance that shows a clear melting peak during the temperature increase from -100°C to 250°C at 10°C / min. using a differential scanning calorimeter (hereinafter also referred to as DSC. TA Instruments Japan, Q-2000). The melting point and heat of fusion are measured based on the peak temperature and area of ​​the melting peak when the temperature is increased at a rate of 10°C / min. using DSC to melt, cool to resinize, and then increase the temperature to melt again, and the values ​​are measured.

[0030] Regarding the melting point (Tm) of the modified polyolefin (A), it is desirable that the melting point of the modified polyolefin resin (A) is 20 to 5°C lower than the drying temperature during the film formation process dried at 80 to 90°C, and the melting point is preferably above 60°C. More preferably, it is above 63°C, and particularly preferably above 65°C. In addition, it is preferably below 85°C, more preferably below 83°C, and particularly preferably below 80°C. When it is above 60°C, the cohesive force from the crystal becomes stronger, and the peel strength, adhesion (adhesion), water resistance, heat resistance, and chemical resistance become better. On the other hand, when it is below 85°C, the solubility is good, and it becomes easy to form an aqueous dispersion composition.

[0031] <Nitrogen-containing nonionic emulsifier (B)> The emulsifier (B) contained in the aqueous dispersion of the present invention is a nonionic emulsifier containing nitrogen. By using this component, the water resistance of the coating film becomes good. As nonionic surfactants containing nitrogen, polyoxyethylene lauryl amine, polyoxyethylene stearyl amine, polyoxyethylene coconut amine, polyoxyethylene tallow amine and other polyoxyalkylene amine types, polyoxyethylene polyoxypropylene monoamine and other polyoxyalkylene amine types, polyoxyethylene oleamide, polyoxyethylene coconut fatty acid amide, polyoxyethylene lauramide, polyoxyethylene stearyl amide, polyoxyethylene tallow amide, polyoxyethylene coconut fatty acid monoethanolamide, polyoxyethylene lauryl monoethanolamide and other polyoxyalkylene alkylamide types can be cited. As these nonionic emulsifiers containing nitrogen, polyoxyethylene lauryl amine and polyoxyethylene coconut amine are preferred because of less exudation and better peel strength.

[0032] The nitrogen-containing nonionic emulsifier (B) preferably has an alkyl chain carbon number of 10 to 30, more preferably 12 to 25. When the carbon number is 10 or more and 30 or less, hydrophobic interaction becomes appropriate, stability with olefin particles is improved, water resistance is improved, and peel strength is improved.

[0033] The nitrogen-containing nonionic emulsifier (B) preferably has an ethylene oxide (EO) mole number (the number of ethylene oxide units per molecule) of 8 to 30. More preferably, it is 9 to 25 or more, and particularly preferably 10 to 20. When it is within the range of 8 to 30, water dispersibility during emulsification becomes stable.

[0034] The nitrogen-containing nonionic emulsifier (B) is preferably 10 parts by mass or more, more preferably 13 parts by mass or more, further preferably 20 parts by mass or more, and particularly preferably 25 parts by mass or more, relative to 100 parts by mass of the modified polyolefin resin (A). In addition, it is preferably 45 parts by mass or less, further preferably 42 parts by mass or less, and particularly preferably 40 parts by mass or less. By being 15 parts by mass or more, the emulsification is improved, the particle size is reduced, and the film-forming property is improved, so the peel strength tends to increase, and the water resistance of the coating film tends to become good at 45 parts by mass or less.

[0035] The method of mixing the nitrogen-containing nonionic emulsifier (B) is not particularly limited. For example, it can be mixed without diluting in water or the like, or it can be mixed in the form of an aqueous solution diluted to 1 to 50% by mass. In order to quickly mix in the aqueous dispersion composition, it is preferably mixed in the form of an aqueous solution diluted to 1 to 50% by mass. By mixing the emulsifier in the form of an aqueous solution into the aqueous dispersion composition, the emulsifier quickly adsorbs the particles and the particle size can be reduced.

[0036] <Alkaline substances (C)> The alkaline substance (C) used in the present invention can neutralize the acidic group (carboxyl group) of the modified polyolefin (A) and improve the dispersibility of the modified polyolefin (A).

[0037] The alkaline substance (C) is not particularly limited, but a volatile alkaline substance is preferred, among which ammonia and amines are preferred. As amines, there are no particular limitations, and examples thereof include monomethylamine, dimethylamine, trimethylamine, monoethylamine, mono-n-propylamine, dimethyl-n-propylamine, monoethanolamine, diethanolamine, triethanolamine, N-methylethanolamine, N-aminoethylethanolamine, N-methyldiethanolamine, monoisopropanolamine, diisopropanolamine, triisopropanolamine, N,N-dimethylethanolamine, and N,N-dimethylpropanolamine, among which triethylamine and N,N-dimethylethanolamine are particularly preferred. These volatile amines can be used alone or in combination of two or more.

[0038] The alkaline substance (C) is preferably 0.5 mass parts or more relative to 100 mass parts of modified polyolefin (A), more preferably 1 mass parts or more, further preferably 2 mass parts or more, particularly preferably 3 mass parts or more. In addition, it is preferably 10 mass parts or less, more preferably 9 mass parts or less, further preferably 8 mass parts or less, particularly preferably 7 mass parts or less. If too little, the particle size of the dispersed particles of the aqueous dispersion composition obtained is larger, and storage stability is sometimes reduced, and if too much, the water resistance of the coating is sometimes reduced.

[0039] <Water-soluble polymer containing anionic groups (D)> The water-soluble polymer (D) containing anionic groups used in the present invention can reduce the surface charge of the modified polyolefin (A) particles in the aqueous dispersion composition, thereby making the viscosity of the modified polyolefin in the aqueous dispersion composition at 30% by mass solid content constant within a range of 500 mPa·s or less.

[0040] Further, by using a water-soluble polymer (D) containing anionic groups, it is possible to play a role in reducing the viscosity of the aqueous dispersion composition, and it is also possible to not interfere with the excellent effect of the effect of the viscosity modifier when coating. The viscosity modifier shows the target viscosity by hydration in the coating and the association between polar groups, but when using low molecular weight compounds such as electrolytes as charge reducers, it will hinder the above-mentioned hydration and the association between polar groups, so the viscosity modifier sometimes becomes unable to function. On the other hand, it can be considered that since the water-soluble polymer (D) containing anionic groups is a polymer compound, the flow in the coating is suppressed, and the interaction with the viscosity modifier is small, and the effect of the viscosity modifier is not affected. That is, when making coatings, inks, sealants, primers and adhesives, in addition to the aqueous dispersion composition, various additives such as viscosity modifiers are also mixed to prevent the liquid from dripping during coating. When the water-soluble polymer (D) contains an anionic group, the effect of the viscosity adjuster and the like is not impaired, and therefore, there is no dripping during coating, and a good coating material, ink, sealant, primer, adhesive and the like can be obtained.

[0041] The water-soluble polymer (D) containing anionic groups refers to a polymer compound that dissolves in water and reduces the charge on the surface of the particles of the modified polyolefin (A). Specifically, acrylic resins, polyurethane resins, epoxy resins, etc. containing carboxyl groups, sulfonic acid groups, sulfate groups, and phosphate groups can be listed. More specifically, water-soluble polymers containing anionic groups whose main components are polystyrene sulfonic acid, polyacrylic acid, styrene-maleic anhydride copolymers, styrene-acrylic acid monomer copolymers, styrene-methacrylate monomer copolymers, etc. can be listed. These water-soluble polymers (D) containing anionic groups can be used alone or in combination of two or more.

[0042] The acid value of the water-soluble polymer (D) containing anionic groups is preferably more than 100mgKOH / g-resin, more preferably more than 130mgKOH / g-resin, more preferably more than 150mgKOH / g-resin, particularly preferably more than 160mgKOH / g-resin, more preferably more than 170mgKOH / g-resin, most preferably more than 180mgKOH / g-resin. Less than 100mgKOH / g-resin, the effect of the viscosity reduction of the aqueous dispersion composition sometimes decreases. In addition, preferably less than 500mgKOH / g-resin, more preferably less than 490mgKOH / g-resin, more preferably less than 480mgKOH / g-resin, particularly preferably less than 470mgKOH / g-resin, more preferably less than 460mgKOH / g-resin, most preferably less than 450mgKOH / g-resin. When greater than 500 mgKOH / g-resin, the water resistance of the coating is sometimes reduced, and the effect of the viscosity modifier when coating is sometimes hindered. When within the above range, the viscosity of the aqueous dispersion composition and the physical properties of the coating become good, so it is preferred. The acid value of the water-soluble polymer (D) containing anionic groups can be measured according to JIS K-0070-1992.

[0043] The weight average molecular weight (Mw) of the water-soluble polymer (D) containing anionic groups is preferably 1,500 or more, more preferably 2,000 or more, further preferably 3,000 or more, particularly preferably 5,000 or more, further preferably 7,000 or more, and most preferably 9,000 or more. If it is less than 1,500, the effect of the viscosity regulator during coating is sometimes hindered. In addition, it is preferably 30,000 or less, more preferably 29,000 or less, further preferably 28,000 or less, particularly preferably 27,000 or less, further preferably 26,000 or less, and most preferably 25,000 or less. When it is greater than 30,000, the solubility in water decreases, and the effect of viscosity reduction sometimes decreases. If it is within the range of 1,500 or more and 30,000 or less, the viscosity of the aqueous dispersion composition and the physical properties of the coating film become good, so it is preferred. The weight average molecular weight of the water-soluble polymer (D) containing an anionic group can be measured by GPC in an atmosphere at 40°C.

[0044] The solubility of the water-soluble polymer (D) containing anionic groups in water (20° C.) is preferably 5% by mass or more, more preferably 10% by mass or more, further preferably 20% by mass or more, and further preferably 30% by mass or more. The upper limit is not particularly limited, but is 50% by mass or less for practicality.

[0045] The water-soluble polymer (D) containing anionic groups is preferably 0.1 mass parts or more relative to 100 mass parts of modified polyolefin (A), more preferably 0.3 mass parts or more, further preferably 0.5 mass parts or more, and particularly preferably 0.8 mass parts or more. In addition, it is preferably 20 mass parts or less, more preferably 19 mass parts or less, further preferably 18 mass parts or less, and particularly preferably 17 mass parts or less. If it is too little, the effect of viscosity reduction sometimes becomes smaller, and if it is too much, the water resistance of the coating film is sometimes reduced, and in addition, the effect of the viscosity regulator when coating is sometimes hindered.

[0046] The Z average particle size in the aqueous dispersion containing the modified polyolefin (A) is 200 nm or less. Preferably, it is 150 nm or less, more preferably 120 nm or less, further preferably 100 nm or less, and particularly preferably 80 nm or less. By being 200 nm or less, it tends to be able to enter the gap of the propylene substrate, and the adhesion (adhesion) brought by the strong anchoring effect is obtained, and in addition, the fusion property during baking is improved, the film forming property is improved, and the peel strength is improved. The lower limit is not particularly specified, but it becomes good for storage stability, preferably 30 nm or more.

[0047] The viscosity of the aqueous dispersion composition containing the modified polyolefin (A) is preferably 5 mPa·s or more, more preferably 10 mPa·s or more. In addition, it is preferably 300 mPa·s or less, more preferably 250 mPa·s or less. The pH of the aqueous dispersion composition of the present invention is preferably 5 or more and 10 or less, more preferably 7 or more, particularly preferably 8.3 or more, and further preferably 8.5 or more.

[0048] The method for producing the aqueous dispersion composition is not particularly limited, and for example, the following production method can be cited: that is, the aqueous dispersion composition can be obtained by dissolving the modified polyolefin (A) and the emulsifier (B) in one or more solvents selected from ether solvents, alcohol solvents and aromatic solvents and water, adding an alkaline substance, cooling, and then removing the solvents.

[0049] From the viewpoint of the handleability of the aqueous dispersion, the solid content concentration of the aqueous dispersion of the resin composition in the present invention is preferably 10 to 60% by mass, more preferably 20 to 50% by mass, and even more preferably 25 to 45% by mass based on the total amount of the aqueous dispersion.

[0050] The ether solvent is not particularly limited, and examples thereof include tetrahydrofuran (hereinafter also referred to as THF), propylene glycol monomethyl ether, propylene glycol monoethyl ether, and propylene glycol monopropyl ether. These may be used alone or in combination of two or more.

[0051] The alcohol solvent is not particularly limited, and examples thereof include aliphatic alcohols having 1 to 7 carbon atoms, aromatic alcohols, alicyclic alcohols, and the like. These may be used alone or in combination of two or more.

[0052] Examples of the aromatic solvent include benzene, toluene, xylene, ethylbenzene, cumene, solvent naphtha, and the like, and these may be used alone or in combination of two or more.

[0053] The amount of the solvent and water used can be arbitrarily selected, and is preferably modified polyolefin (A): water: solvent = 100:50 to 800:11 to 900 (mass ratio), more preferably 100:200 to 400:43 to 233 (mass ratio).

[0054] In addition, relative to the aqueous dispersion composition of the present invention, in order to further improve the performances such as water resistance and solvent resistance, a curing agent can also be mixed as required. As a curing agent, there is no particular limitation, for example, water-based multifunctional carbodiimide resins, aqueous dispersions of multifunctional isocyanate compounds, water-based multifunctional oxazoline resins, water-soluble silane coupling agents containing multifunctional silyl groups, aqueous melamine compounds, etc. can be cited. These curing agents are preferably mixed with 2 to 30 parts by mass relative to 100 parts by mass of the resin in the aqueous dispersion composition of the present invention.

[0055] Further, in the scope that does not reduce the effect of the present invention, relative to the aqueous dispersion composition of the present invention, various additives such as fillers, pigments, colorants, antioxidants can also be mixed. The compounding amount of these additives is preferably below 150 mass parts relative to 100 mass parts of the resin in the aqueous dispersion composition, more preferably below 140 mass parts, and further preferably below 130 mass parts. In addition, it is preferably more than 5 mass parts, more preferably more than 2 mass parts. By being set in the above-mentioned scope, the excellent effect of the present invention can be brought into play.

[0056] The aqueous dispersion composition of the present invention can be used as an adhesive for various polyolefin substrates represented by polypropylene. In addition, a coating can be obtained by mixing the aqueous dispersion of the present invention and the pigment dispersion liquid, which can also be used as a coating. The coating film formed by removing the aqueous medium from the aqueous dispersion composition of the present invention can be used as an adhesive layer, and the substrates can be bonded to each other to form a laminate. In addition, the coating film formed by removing the aqueous medium from the aqueous dispersion composition of the present invention can be used as a coating layer and applied to a substrate to form a laminate. The aqueous dispersion composition of the present invention is not limited to polyolefin substrates, for example, it can also be applied to other plastics, wood, metal, etc. As polyolefin substrates, films, sheets, molded bodies, etc. can be listed. There is no particular limitation on the coating method.

[0057] The present invention will be described in detail below by way of examples, but the present invention is not limited to these examples. In the examples and comparative examples, the term "part" simply means part by mass. In addition, the measurement and evaluation methods used in the present invention are as follows.

[0058] 1) Determination of solid content concentration of aqueous dispersion composition Weigh about 1g of the sample of the aqueous dispersion in a 50ml glass weighing bottle and weigh it accurately. Then dry the weighing bottle with the sample in a hot air dryer at 120°C for 2 hours, put the weighing bottle out of the dryer, and place it at room temperature to cool for 30 minutes. Take out the weighing bottle from the dryer, weigh it accurately, and calculate the mass % of the solid content concentration of the aqueous dispersion from the weight change before and after hot air drying (the following formula). Solid content concentration of aqueous dispersion (mass %) = 100 - [(mass of sample before hot air drying) - (mass of sample after hot air drying)] / (mass of sample before hot air drying) × 100

[0059] 2) Determination of viscosity of aqueous dispersion composition 0.6 g of a sample was measured using "Viscometer TV-22" (E-type viscometer) manufactured by Toki Sangyo Co., Ltd. under the conditions of rotor No. 0.8° (=48') x R24, H-type range, rotation speed 5 rpm, and 25°C.

[0060] 3) Determination of pH of aqueous dispersion composition The value at 25° C. was measured using a pH meter F-52 manufactured by Horiba, Ltd. The measuring instrument was calibrated by three-point calibration using a phthalate pH standard solution (pH: 4.01), a neutral phosphate pH standard solution (pH: 6.86), and a borate pH standard solution (pH 9.18) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.

[0061] 4) Measurement of average particle size (Z-average particle size) of aqueous dispersion composition The average particle size (Z average particle size) based on the intensity distribution was measured by dynamic light scattering using a "Zetasizer Nano-ZS Model ZEN3600" manufactured by Malvern. The sample having the solid content of the aqueous dispersion composition adjusted to a concentration of 0.05 g / L was measured three times at 25°C and the average value was taken.

[0062] 5) Determination of acid modification amount The acid modification amount when maleic anhydride is used for acid modification is determined by FT-IR (manufactured by Shimadzu Corporation, FT-IR8200PC). First, maleic anhydride is dissolved at an arbitrary concentration to prepare a standard curve solution, and then the standard curve solution is measured by FT-IR. The stretching vibration peak (1780 cm-1) of the carbonyl (C=O) bond of maleic anhydride is -1 The modified polyolefin (A) was dissolved in chloroform and subjected to FT-IR measurement. Based on the above calibration curve, the stretching vibration peak of the carbonyl bond of maleic anhydride (1780 cm -1 ) was used to determine the acid modification amount of maleic anhydride.

[0063] 6) Determination of melting point The melting point and heat of fusion in the present invention are values ​​measured using a differential scanning calorimeter (DSC, manufactured by TA Instruments Japan, Q-2000) by heating at a rate of 10°C / min to melt, cooling to resinify, and heating again to melt.

[0064] 7) Determination of glass transition temperature The glass transition temperature (Tg) (°C) of the resin is measured by DSC, under the same conditions as for the melting point, at the point where a straight line equidistant from the extension of each baseline in the reheating process in the vertical direction intersects the curve of the glass transition stage change portion.

[0065] 8) Weight average molecular weight of modified polyolefin (A) The weight average molecular weight of the modified polyolefin (A) is a value measured by a gel permeation chromatograph Alliance e2695 manufactured by Waters Japan (hereinafter referred to as GPC, standard substance: polystyrene resin, mobile phase: tetrahydrofuran, chromatographic column: Shodex KF-806 + KF-803, column temperature: 40°C, flow rate: 1.0 ml / min, detector: photodiode array detector (wavelength 254 nm = ultraviolet light)).

[0066] Production Example 1 100 parts by mass of propylene-butene copolymer (propylene / butene=69 / 31% by mass), 300 parts by mass of toluene and 10 parts by mass of maleic anhydride were added to a 1L autoclave, and after heating to 120°C, 1 part by mass of di-tert-butyl peroxide was added and stirred for 1 hour. Then, the obtained reaction solution was cooled and injected into a container filled with a large amount of methyl ethyl ketone to precipitate the resin. Then, the liquid containing the resin was centrifuged to separate and purify the acid-modified propylene-butene copolymer grafted with maleic anhydride from the ungrafted maleic anhydride and low molecular weight substances. Then, by drying it at 70°C under reduced pressure for 5 hours, a maleic anhydride-modified propylene-butene copolymer (PO-1, melting point 72°C, maleic anhydride modification amount 0.6% by mass, weight average molecular weight 80,000) was obtained.

[0067] Production Example 2 100 parts by mass of propylene-butene copolymer (propylene / butene=75 / 25% by mass), 300 parts by mass of toluene and 10 parts by mass of maleic anhydride were added to a 1L autoclave, and after heating to 120°C, 2 parts by mass of di-tert-butyl peroxide were added and stirred for 1 hour. Then, the obtained reaction solution was cooled and injected into a container filled with a large amount of methyl ethyl ketone to precipitate the resin. Then, the liquid containing the resin was centrifuged to separate and purify the acid-modified propylene-butene copolymer grafted with maleic anhydride from the ungrafted maleic anhydride and low molecular weight substances. Then, by drying it at 70°C under reduced pressure for 5 hours, a maleic anhydride-modified propylene-butene copolymer (PO-2, melting point 80°C, modification amount of maleic anhydride 0.6% by mass, weight average molecular weight 80,000) was obtained.

[0068] Production Example 3 A maleic anhydride-modified propylene-butene copolymer (PO-3, melting point 72°C, modification amount of maleic anhydride 2.0% by mass, weight average molecular weight 50,000) was obtained by the same method as in Production Example 1, except that the added amount of maleic anhydride was changed to 20 parts by mass and that of di-tert-butyl peroxide was changed to 5 parts by mass.

[0069] Production Example 4 100 parts by mass of propylene-ethylene copolymer (MFR=5 g / 10 minutes in 230°C atmosphere), 150 parts by mass of toluene, 10 parts by mass of maleic anhydride, and 1 part by mass of di-tert-butyl peroxide were added to a 1L autoclave equipped with a stirrer, and the temperature was raised to 140°C, followed by further stirring for 3 hours. Then, the obtained reaction solution was cooled, and then poured into a container filled with a large amount of methyl ethyl ketone to precipitate the resin. Then, the liquid containing the resin was centrifuged to separate and purify the acid-modified propylene-ethylene copolymer grafted with maleic anhydride from (poly)maleic anhydride and low molecular weight substances. Then, the maleic anhydride-modified propylene-ethylene copolymer was obtained by drying it at 70°C under reduced pressure for 5 hours. Then, 100 parts by mass of the maleic anhydride-modified propylene-ethylene copolymer and 1700 parts by mass of chloroform were added to a 2L glass-lined reaction jar and sealed. The liquid in the reaction can was stirred and dispersed while being heated, and dissolved at a can temperature of 120°C for 1 hour. After the can temperature was cooled to 110°C, 0.5 parts by mass of tert-butyl peroxy-2-ethylhexanoate was added, and 70 parts by mass of chlorine was introduced. The can temperature was cooled to 60°C, 1400 parts by mass of chloroform was distilled off, and 4 parts by mass of p-tert-butylphenyl glycidyl ether was added as a stabilizer. Then, a maleic anhydride-modified chlorinated propylene-ethylene copolymer (CPO-1, melting point 75°C, modification amount of maleic anhydride 0.8% by mass, chlorine content 20% by mass, weight average molecular weight 103,000) was obtained by drying.

[0070] Production Example 5 A maleic anhydride-modified chlorinated propylene-ethylene copolymer (CPO-2, melting point 75° C., modification amount of maleic anhydride 2.5% by mass, chlorine content 20% by mass, weight average molecular weight 83,500) was obtained by the same method as in Preparation Example 4, except that the added amount of maleic anhydride was changed to 20 parts by mass and the added amount of di-tert-butyl peroxide was changed to 5 parts by mass.

[0071] Table 1 shows the compositions of the aqueous dispersions used in the following Examples and Comparative Examples.

[0072]

Table 1

[0073] [Example 1] 100 parts by mass of modified polyolefin (PO-1), 10 parts by mass of polyoxyethylene laurylamine (B-1) with an EO addition mole number of 10 as an emulsifier, 300 parts by mass of ion exchange water, 30 parts by mass of tetrahydrofuran and 50 parts by mass of toluene were added to a flask equipped with a stirrer, and the mixture was heated to 90°C and dissolved at the same temperature for 1 hour. Then, 3.5 parts by mass of N,N-dimethylethanolamine was added and stirred at the same temperature for 1 hour. Then, the mixture was slowly cooled to 40°C over 1 hour, and the organic solvent was distilled off at a reduced pressure of 91 kPa, and 1.0 parts by mass of ARUFON UC-3920 was added to obtain an aqueous dispersion with properties shown in Table 1.

[0074] Embodiments 2 to 7 Using the modified polyolefin (A) shown in Table 1, an aqueous dispersion composition was obtained in the same manner as in Example 1 except that the amount of polyoxyethylene laurylamine (B-1) having an EO addition mole number of 10 as an emulsifier was changed. The properties are shown in Table 1.

[0075] Comparative Examples 1 and 2 As shown in Table 1, an aqueous dispersion composition having the properties shown in Table 1 was obtained in the same manner as in Example 1 except that 15 parts by mass and 35 parts by mass of polyoxyethylene oleyl cetyl ether (B-2) having an EO addition mole number of 15 were used as the emulsifier.

[0076] Comparative Examples 3 and 4 An aqueous dispersion composition having the composition shown in Table 1 was obtained in the same manner as in Example 1 except that the modified polyolefin (PO-3) was changed to 100 parts by mass and the added amounts of polyoxyethylene laurylamine (B-1) having an EO addition mole number of 10 were changed to 25 and 45 parts by mass, respectively.

[0077] Comparative Example 5 An aqueous dispersion composition having the composition shown in Table 1 was obtained in the same manner as in Example 1 except that the modified polyolefin (CPO-2) was changed to 100 parts by mass and the amount of polyoxyethylene laurylamine (B-1) having an EO addition mole number of 10 was changed to 35 parts by mass.

[0078] Comparative Example 6 An aqueous dispersion composition as shown in Table 1 was obtained in the same manner as in Example 1 except that the amount of polyoxyethylene laurylamine (B-1) having an EO addition mole number of 10 as an emulsifier was changed to 5 parts by mass and the amount of N,N-dimethylethanolamine was changed to 0.4 parts by mass.

[0079] <Pigment dispersion> 4 parts by mass of a water-soluble acrylic resin, 2 parts by mass of conductive carbon black, 36 parts by mass of rutile titanium oxide, and 70 parts by mass of ion exchange water were added, stirred for 30 minutes, and dispersed for 30 minutes using a bead mill. Then, 5 parts by mass of a polyurethane associative thickener and 2 parts by mass of a leveling agent were added to obtain a pigment dispersion.

[0080] <Preparation of coating composition> 38 parts by weight of the above pigment dispersion and 16 parts by weight of polyester polyurethane dispersion (UXA-310 manufactured by Sanyo Chemical, solid content 38%) were added to 20 parts by weight of the aqueous dispersion obtained above, and stirred for 10 minutes using a dispersing mixer. Then, 1.0 parts by weight of BYK-349 as a leveling agent and 2 parts by weight of an alkali swelling thickener (ASE-60 manufactured by Rohm and Haas) were added dropwise, and stirred for 15 minutes to obtain a coating composition. The coating composition was evaluated as follows. The results are shown in Table 2.

[0081] (Evaluation of peel strength) The coating composition prepared above was applied to a polypropylene substrate for bumper (TYC-1175P-G01, manufactured by Standard Plaque, 150 mm × 1000 mm × 3 mm) with a spray gun so that the dry coating film was 10 μm, and heated and dried at 80°C for 10 minutes. Then, a commercially available water-based base paint (RETAN PG WB ECO manufactured by Kansai Paint) was applied with a spray gun so that the dry coating film was 150 μm. Then, the test piece was left for 15 minutes after coating in an environment of 23°C, and then baked and dried in a drying oven at 80°C for 30 minutes, and then the test piece was taken out. Then, after the test was left for 72 hours in an environment of 23°C, the peel strength of the test piece was measured at a tensile speed of 50 mm / min in an environment of 25°C using TENSILON RTM-100 manufactured by A&T. Evaluation Benchmarks A: When the peel strength is 1000 gf / cm or more B: When the peel strength value is 700 or more and less than 1000 gf / cm C: When the peel strength value is 500 or more and less than 700 gf / cm D: When the peel strength value is less than 500gf / cm

[0082] (Evaluation of Adhesion of Coating Film) The coating composition prepared above was applied to a polypropylene substrate for bumper (TYC-1175P-G01 Standard Plaque Co., Ltd., 150 mm × 1000 mm × 3 mm) with a spray gun so that the dry coating film was 10 μm, and heated and dried at 80°C for 10 minutes. Then, a commercially available water-based base paint (RETAN PG WB ECO manufactured by Kansai Paint) was applied with a spray gun so that the dry coating film was 35 μm. Then, the test body was left for 15 minutes after coating in an environment of 23°C, and then baked and dried in a drying oven at 80°C for 30 minutes, and the test piece was taken out. After standing for 36 hours in an atmosphere of 25°C, 100 grids were cut on the painted surface with a cutter at 2mm intervals, and the cellophane tape was peeled off at an angle of 60°. A new cellophane tape was used and the peeling was repeated 10 times. If the painted surface did not change after repeating 10 times, it was rated as 10 points and evaluated as A. If peeling occurred on the 10th time, it was rated as 9 points and evaluated as B. Below 8, 7, 6 points, and if peeling occurred on the first time, it was rated as 0 points and evaluated as C.

[0083] (Evaluation of water resistance of coating film) After the test piece prepared under the same conditions as the evaluation of the adhesion of the coating film was left to stand for 36 hours in an atmosphere at 25°C, it was immersed in warm water at 40°C for 10 days. After confirming the change of the coating film, the above-mentioned evaluation of the adhesion of the coating film was implemented. The case where there was no change in the coating film and the evaluation of the adhesion was 10 points was good, which was A. The case where there was no change in the coating film and the evaluation of the adhesion was 9 points was B. The case where bubbles were generated in the coating film and the evaluation of the adhesion was 8 points or less was poor, which was C.

[0084] (Storage stability) 200 g of the coating composition prepared above was sealed in a polypropylene container and stored at 40° C. for 10 days. The viscosity after storage was measured using a rotational viscometer (TVB-10M manufactured by Toki Sangyo), and the change rate from the viscosity before storage was measured. Evaluation Benchmarks A: The viscosity change rate before and after storage is less than 5% B: The viscosity change rate before and after storage is 5% or more and less than 10% C: The viscosity change rate before and after storage is 11% or more and less than 20% D: The viscosity change rate before and after storage is more than 20%

[0085]

Table 2

[0086] [Review of the results of Table 2] The aqueous dispersion compositions obtained in Examples 1 to 7 show good peel strength, good adhesion, and good water resistance relative to the polypropylene substrate for bumpers. On the other hand, since the nitrogen-containing nonionic emulsifier (B) was not used in Comparative Examples 1 and 2, poor water resistance and peel strength were obtained. In addition, since the weight average molecular weight of the modified polyolefin (A) in Comparative Examples 3 and 4 was 60,000 or less, poor water resistance and peel strength were obtained. In addition, since the modified polyolefin (A) with a modification amount of less than 1.0% by mass of α,β-unsaturated carboxylic acid and / or its anhydride was not used in Comparative Example 5, poor water resistance and peel strength were obtained. Furthermore, since the Z-average particle size of the modified polyolefin (A) in Comparative Example 6 was greater than 200nm, poor water resistance and peel strength were obtained.

Industrial Applicability

[0087] The aqueous dispersion composition of the present invention can provide a coating film that exhibits high peel strength, high adhesion and good water resistance when baked at low temperature (80-90° C.) on a polyolefin substrate that is difficult to adhere to. Therefore, it can contribute to reducing the coating defect rate in the aqueous coating system, reducing VOC, or reducing CO2, a cause of global warming, caused by reducing energy consumption in a baking and drying furnace.

Claims

1. An aqueous dispersion composition, It is characterized in that The invention discloses an aqueous dispersion composition comprising a modified polyolefin (A), a nitrogen-containing nonionic emulsifier (B) and an alkaline substance (C); the modified polyolefin (A) has a weight average molecular weight of 60,000 or more as measured by GPC, and the amount of modification with an α,β-unsaturated carboxylic acid and / or anhydride thereof is less than 1.0% by mass; and the Z average particle size of the aqueous dispersion composition is less than 200 nm.

2. The aqueous dispersion composition according to claim 1, It is characterized in that The melting point of the modified polyolefin (A) is 60°C to 85°C.

3. The aqueous dispersion composition according to claim 1, It is characterized in that The modified polyolefin (A) does not contain chlorine.

4. The aqueous dispersion composition according to claim 1, It is characterized in that The amount of the nitrogen-containing nonionic emulsifier (B) added is 10 to 45% by mass based on 100 parts by mass of the modified polyolefin (A).

5. The aqueous dispersion composition according to claim 1, It is characterized in that The present invention further comprises a water-soluble polymer (D) containing an anionic group, wherein the acid value of the water-soluble polymer (D) containing anionic group is 100 mg to 500 mg KOH / g-resin, and the content thereof is 0.1 to 20% by mass based on 100 parts by mass of the modified polyolefin (A).

6. The aqueous dispersion composition according to claim 1, It is characterized in that The modified polyolefin (A) is a propylene-α-olefin copolymer having a butene content of 2 to 35% by mass in the polyolefin component.

7. A coating, It is characterized in that The aqueous dispersion composition comprises the aqueous dispersion composition according to any one of claims 1 to 6.

8. An adhesive, It is characterized in that The aqueous dispersion composition comprises the aqueous dispersion composition according to any one of claims 1 to 6.

9. A coating film, It is characterized in that This is a coating film formed by removing the aqueous medium from the aqueous dispersion composition according to any one of claims 1 to 6.

10. A laminate, It is characterized in that It has a layer derived from the coating material according to claim 7.

11. A laminate, It is characterized in that It has a layer derived from the adhesive according to claim 8.

Citation Information

Patent Citations

  • Method for producing aqueous modified polyolefin dispersion composition

    CN104220492A

  • Dispersion resin composition

    CN113614166A

  • Aqueous resin composition

    CN113748167A

  • Modified polyolefin emulsion and method for producing the same