Hard coating film cutting tool
By controlling the surface roughness and hard film composition on the front and side cutting surfaces of the hard film cutting tool, the problem of insufficient adhesion between the hard film and the matrix material is solved, and excellent welding resistance and resistance are achieved Abrasiveness improves processing efficiency and tool life.
Patent Information
- Application Number
- CN202280092649.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-14
- Filing Date
- 2022-12-15
- Publication Date
- 2024-11-05
AI Technical Summary
When existing hard coating cutting tools process high-hard workpieces, the adhesion between the hard film and the matrix material is insufficient, resulting in a shortening of the tool life, and the post-treatment process limits the improvement of surface roughness, affecting welding resistance and abrasion resistance. .
By controlling the surface roughness on the front and side cutting surfaces of the hard membrane, 0.2μm≤SaR≤0.5μm and 0.15μm≤SaF≤0.4μm, combined with a specific hard membrane, Al(1-a-b-c)TiaCrbMecN is composed of TiaCrbMecN , and limit the maximum height roughness RyR and RyF within a certain range, reducing the number of droplets to improve adhesion and welding resistance.
It realizes excellent adhesion between the hard film and the matrix material and welding resistance of the workpiece, improves processing efficiency, and extends the service life of the tool.
Smart Images

Figure CN118900931A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a hard-coated cutting tool, which includes a hard base material such as cemented carbide, cermet, ceramic or cubic boron nitride used in the cutting tool, and a hard film formed on the hard-coated cutting tool, and more particularly, to a hard-coated cutting tool on which the surface roughness of each of a rake surface and a flank surface varies to adapt to the characteristics of each surface. Background Art
[0002] In tools for machining high-hardness workpieces (e.g., high-hardness steel) having a hardness of 50 or more according to the HRC standard, technology for applying hard films made of various ceramics to hard base materials (e.g., cemented carbide, cermets, end mills, and drills) is being adopted to improve cutting performance and life.
[0003] The hard film formed on the hard substrate material by deposition technology has the risk of peeling due to the difference in lattice constant between the hard substrate material and the hard film and the characteristics of the physical vapor deposition method, which increases the stress of the hard film. To solve this problem, the adhesion of the hard film to the substrate material is improved by pretreatment, etching, bonding layer, thin film with multilayer structure and post-treatment technology.
[0004] When processes such as pretreatment and etching are applied, the specific surface area of the surface of the hard base material can be increased to improve the adhesion between the base material and the film. However, depending on the workpiece, especially in stainless steel and Inconel cutting, the increase in specific surface area may lead to an increase in weldability between the film and the workpiece, thereby deteriorating the life of the tool due to the tearing of the hard film.
[0005] In order to solve this problem, in the related art, a post-treatment process of the hard film has been applied to reduce the surface roughness of the tool to improve lubricity. However, despite these efforts, there are limitations in improving the roughness by the post-treatment process of the hard film, and there are disadvantages in manufacturing efficiency due to the additional process. In addition, even in the case of processing in the state of the hard base material after the hard film is peeled off, since the specific surface area of the hard base material is still high, the weldability increases, thereby causing the problem of reduced tool life, so it is necessary to solve this problem. However, if the specific surface area of the hard base material is excessively reduced, the adhesion between the hard base material and the hard film may be reduced to accelerate the peeling of the film. Summary of the invention
[0006] Technical issues
[0007] An object of the present invention is to provide a hard-coated cutting tool having excellent welding resistance and wear resistance.
[0008] Technical Solution
[0009] In order to achieve the above-mentioned object, a hard-coated cutting tool according to the present invention comprises: a hard base material; and a hard film formed on the hard base material, wherein, if it is assumed that the chromatic diffuse reflectance value on the front cutting edge of the hard film is L SCER , and the total reflectivity value is L SCIR , then 0.65≤L SCER / L SCIR ≤0.85, and when the surface roughness is measured on the rake face of the hard film within a range of 100 μm from the edge, the arithmetic mean height S aR In 0.2μm≤S aR ≤0.5 μm, and if it is assumed that the chromatic diffuse reflectance value on the side blade surface of the hard film is L SCEF , and the total reflectivity value is L SCIF , then L SCEF / L SCIF ≥0.9, and when the surface roughness is measured on the side cutting surface of the hard film within a range of 100 μm from the edge, the arithmetic mean height S aF At 0.15μm≤S aF In the range of ≤0.4μm.
[0010] In addition, in the cross section of the cutting tool, on the rake face of the hard base material within a range of 300 μm from the edge, the maximum height roughness R of the hard base material is yR Can be 1μm≤R yR ≤2 μm, and in the cross section of the cutting tool, on the side cutting surface of the hard matrix material within a range of 300 μm from the edge, the maximum height roughness R of the hard matrix material is yF Can be 2μm≤R yF ≤5μm.
[0011] In addition, the hard film may have a composition satisfying the following Formula 1 and include one or more films each having a thickness in the range of 0.1 μm to 10 μm.
[0012] Formula 1: Al (1-a-b-c) Ti a Cr b Me cN, wherein Me is any one or more of B, Si, Zr, V, Mn, Nb, Mo, Ta, and W, 0≤a≤0.6, 0≤b≤0.5, and 0≤c≤0.15, and must include at least one of Ti and Cr.
[0013] Furthermore, the number of droplets each having a diameter of 3 μm or more within 100 μm from the edge on the rake face of the hard film may be 5% or less of the total number of droplets.
[0014] Beneficial effects
[0015] According to the present invention, a cutting tool having excellent adhesion between a hard film and a base material and excellent resistance to welding to a workpiece can be provided. In addition, in the manufacture of a cutting tool having a hard film, processing efficiency can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 1 is a schematic diagram for explaining a cutting tool according to an embodiment of the present invention, on which a hard film is provided on a hard base material.
[0017] Figure 2 is a scanning electron microscope image showing the surface of the hard film according to the embodiment of the present invention. DETAILED DESCRIPTION
[0018] Hereinafter, detailed descriptions related to well-known functions or configurations will be excluded to avoid unnecessarily obscuring the subject matter of the present invention. In addition, when described as including some elements, it should be understood that only these elements may be included, or other elements as well as these elements may be included if there is no specific limitation.
[0019] The hard-coated cutting tool according to the present invention may include: a hard base material; and a hard film formed on the hard base material, wherein, assuming that the chromatic diffuse reflectance value on the front cutting edge of the hard film is L SCER , and the total reflectivity value is L SCIR , then 0.65≤L SCER / L SCIR ≤0.85, and when the surface roughness is measured on the rake face of the hard film within a range of 100 μm from the edge, the arithmetic mean height S aR In 0.2μm≤S aR ≤0.5 μm, and if it is assumed that the chromatic diffuse reflectance value on the side blade surface of the hard film is L SCEF , and the total reflectivity value is L SCIF , then L SCEF / L SCIF≥0.9, and when the surface roughness is measured on the side cutting surface of the hard film within a range of 100 μm from the edge, the arithmetic mean height S aF At 0.15μm≤S aF In the range of ≤0.4μm.
[0020] One of the ways to measure surface roughness is to use a colorimeter. A colorimeter measures reflected light. Light that is incident on a surface and reflected at the same angle is called specular reflectance, and light that is not specularly reflected but scattered and reflected in various directions is called diffuse reflectance. The combination of specular and diffuse reflectance is called total reflection.
[0021] The amount of specular reflection is greater than diffuse reflection on a glossy surface, while the amount of diffuse reflection is relatively large on a rough surface. Therefore, the higher the diffuse reflection value is in the total reflectance value, the rougher the surface.
[0022] In a cutting tool, the side cutting surface and the rake cutting surface may experience different environments during machining. In particular, the rake cutting surface may be a surface through which machining chips generated from a workpiece during machining pass and on which a hard film is easily peeled off by fusion between the machining chips and the surface of the cutting tool.
[0023] Therefore, since the side face and the rake face need to have different characteristics to adapt to different environments, in the present invention, the surface roughness of the side face and the surface roughness of the rake face are set to be different from each other.
[0024] To this end, in the present invention, the roughness of the side blade surface is increased to increase the diffuse reflectivity and increase the adhesion between the hard film and the hard base material. On the other hand, the diffuse reflectivity of the rake face is lower than that of the side blade surface and is maintained within a certain range to control the surface roughness, thereby improving the welding resistance of the hard film.
[0025] For more details, refer to Figure 1 By ensuring that the diffuse reflection value is greater than 90% of the total reflection value, the roughness of the side cutting surface 22 of the hard film 20 increases, and at the same time, the arithmetic mean height S that appears when the roughness is measured aR Set at 0.2μm≤S aR≤0.5μm. Since the diffuse reflection value is obtained by measuring the amount of light scattered from the surface, it is difficult to determine how much difference occurs in the surface height due to the roughness. Therefore, it may be difficult to control the large height difference that occurs on the surface of the hard film 20, and therefore, since the wear resistance of the hard film 20 is reduced, when measuring the surface roughness, it is necessary to control the arithmetic mean height to a certain level. For this reason, the arithmetic mean height S on the side blade surface is aR It is preferably in the range of 0.2 μm to 0.5 μm, and if it is less than 0.2 μm, adhesion to the hard base material 30 may be problematic, and if it exceeds 0.5 μm, the chipping resistance of the side cutting surface 22 may deteriorate. In particular, as Figure 1 As shown, the arithmetic mean height is controlled within a range 24 within 100 μm from the edge because this area is an area that may come into contact with a workpiece in actual processing and control of fine features is particularly required.
[0026] Furthermore, as described above, it is advantageous that the front cutting surface 21 has a smaller roughness than the side cutting surface 22 for welding resistance. To this end, in the present invention, the ratio of the diffuse reflection value to the total reflection value is controlled within the range of 0.65 to 0.85 according to a colorimeter on the front cutting surface 21. If the roughness decreases too much and the diffuse reflection value becomes too low, the adhesion between the hard base material and the hard film decreases. On the contrary, if the roughness increases and the diffuse reflection value becomes too high, the welding resistance decreases. In addition, as with the side cutting surface 22, it is necessary to control the arithmetic mean height of the front cutting surface 21 within the range of 100 μm from the edge. That is, the arithmetic mean height S aF It is maintained within the range of 0.15 μm to 0.4 μm to ensure consistent adhesion with the hard base material 30, fusion resistance, and wear resistance.
[0027] In the hard-coated cutting tool according to the present invention, in the cross section of the cutting tool, the maximum height roughness R of the hard base material on the rake face of the hard base material within 300 μm from the edge is yR Can be 1μm≤R yR ≤2μm, and in the cross section of the cutting tool, the maximum height roughness R of the hard matrix material on the side cutting edge of the hard matrix material within 300μm from the edge yF Can be 2μm≤R yF ≤5μm.
[0028] As described above, it is necessary to control the surface roughness of the cutting tool with a hard film to a certain level to obtain welding resistance. To this end, a common method is to control the surface of the cutting tool with a hard film by polishing the surface. However, in this case, there is a problem of reducing the thickness of the hard film, so it is difficult to polish the surface to more than a certain level.
[0029] On the other hand, when the roughness of the hard base material is limited, although the surface roughness of the final cutting tool increases, there is a problem that the adhesion between the hard base material and the hard film is poor.
[0030] In order to solve this problem, in the present invention, the surface roughness on each of the rake face and the side face in the hard base material is limited to: reducing the roughness on the rake face, on which welding resistance is important and it is necessary to reduce the surface roughness on the rake face; and increasing the surface roughness on the side face, on which the chipping characteristics are relatively unimportant, in order to improve the adhesion between the hard base material and the hard film.
[0031] Refer again Figure 1 To explain this, in the cutting tool according to the present invention, the maximum height roughness R on the rake face of the hard base material 30 within a range of 300 μm from the edge is yR is set within a range of 1 μm to 2 μm. On the other hand, the maximum height roughness R of the side cutting surface 34 within 300 μm from the edge is yF It is set in the range of 2 μm to 5 μm.
[0032] On the rake face, the maximum height roughness R yR It needs to be below a certain level to improve the welding resistance to the workpiece. For this reason, the roughness of the hard base material is controlled so that the maximum height is 2 μm or less and the roughness is 1 μm or more for bonding to the hard film.
[0033] Since it is advantageous to have a higher roughness on the side cutting edge than on the rake cutting edge, it is necessary to set the maximum height roughness R yF Controlled within the range of 2 μm to 5 μm so as to be larger than the roughness on the rake face.
[0034] The roughness of the hard matrix material can be controlled to a certain level in this way, so that no additional polishing treatment of the cutting tool is required after the final hard film is formed.
[0035] The reason for limiting the measurement of the roughness of the hard base material to within 300 μm from the edge is that the boundary between the hard base material and the hard film can be confirmed within this range.
[0036] Furthermore, in the hard-coated cutting tool according to the present invention, the hard film may have a composition satisfying the following Formula 1, and include one or more films each having a thickness in the range of 0.1 μm to 10 μm.
[0037] Formula 1: Al (1-a-b-c) Ti aCr b Me c N, wherein Me is any one or more of B, Si, Zr, V, Mn, Nb, Mo, Ta, and W, 0≤a≤0.6, 0≤b≤0.5, and 0≤c≤0.15, and must include at least one of Ti and Cr.
[0038] A method of using a deposited film such as TiN, TiAlN, AlTiN or Al2O3, which is a hard film as a hard film formed on the surface of a cutting tool. Among them, the AlTiN film can improve high temperature oxidation resistance and wear resistance by forming an Al2O3 layer on the surface. However, there is still a need to improve bonding strength, toughness and lubricity. In order to improve this, the present invention optimizes the composition of the hard film by combining Cr and other metal elements to meet various requirements.
[0039] When the Al content is greater than the respective compositions of Ti and Cr, wear resistance, oxidation resistance and lubricity are excellent, but when the Al content is too high, there is a problem of increased fragmentation. Therefore, the Ti and Cr contents are preferably 0≤a≤0.6 and 0≤b≤0.5.
[0040] Me added as other elements can improve the chipping resistance, heat resistance and wear resistance of the hard film, but when the content is high, since it is the cause of increasing residual stress due to the increase of amorphous phase, it is preferred that the content c of Me as other elements is in the range of 0 to 0.15.
[0041] In the hard-coated cutting tool according to the present invention, the number of droplets each having a diameter of 3 μm or more within 100 μm from the edge on the rake face of the hard film may be 5% or less of the total number of droplets.
[0042] The hard film formed by deposition can be formed in a droplet shape according to the roughness of the hard base material (see Figure 2 ). The size of each droplet may affect the physical properties of the hard film. If the number of droplets is too large, the frequency of fragmentation and peeling of the hard film may increase, resulting in rapid termination of life during intermittent machining, and therefore, it is preferred that the number of droplets each having a diameter of 3 μm or more is less than 5% of the total number of droplets.
[0043] [Implementation Method]
[0044] A polishing process is applied to a hard base material made of cemented carbide through a micro plastic honing process or a diamond brush honing process, and then a hard film is formed using arc ion plating of a physical vapor deposition (PVD) method.
[0045] In the process of polishing the hard base material, a slurry containing diamond particles each having a size of 1 μm to 5 μm is used, and arc targets of TiAl, AlCr, TiAlSi, and AlCrSi are used as targets for applying a hard film.
[0046] The hard substrate material was subjected to wet micro-sandblasting and then washed with ultrapure water, dried, and installed in a coating furnace along a circumference at a predetermined radial distance from the central axis of the rotary table. The initial vacuum pressure in the coating furnace was set to 8.5×10 -5 Support below.
[0047] After heating to a temperature of 400 to 600° C., a bias of -400 to -200 V is applied to the rotating base material on a rotating table for Ar ion bombardment for 30 to 90 minutes in an Ar gas atmosphere. The gas pressure for coating is maintained below 50 mTorr, preferably below 40 mTorr to form a film.
[0048] Films are formed using TiAl, AlCr, TiAlSi and AlCrSi targets by injecting N2 as a reaction gas under conditions such as a bias voltage of -100V to -30V, an arc current of 100A to 150A and a pressure of 20mTorr to 40mTorr, and the coating conditions may vary depending on equipment characteristics and conditions.
[0049] Films were manufactured under the above conditions according to the comparative examples and embodiments of the present invention, and hard films with a thickness of 1.5 μm to 2.0 μm were formed using targets TiAl (composition ratio 50:50) and TiAlSi (composition ratio 30:60:10) as in comparative examples 1 to 3 and embodiment 1, and hard films with a thickness of 3.5 μm to 4.0 μm were formed using targets TiAl (composition ratio 50:50), AlCr (composition ratio 70:30) and AlCrSi (composition ratio 60:30:10) as in comparative examples 4 to 6 and embodiment 2. Information on chromaticity values, roughness values, and maximum height roughness values in cross sections of hard base materials on corresponding surfaces is shown in Table 1 below.
[0050] [Table 1]
[0051]
[0052] The welding resistance and chipping resistance of the cutting tools manufactured in this manner were evaluated under the following conditions.
[0053] (1) Evaluation of welding resistance and chipping resistance
[0054] Workpiece material: STS304 hexagonal material
[0055] Model: CNMG120408-VP3 (Comparative Examples 1 to 3, Implementation Example 1)
[0056] Cutting speed: 120m / min
[0057] Transfer per revolution: 0.15mm / rev
[0058] Cutting depth: 0.8mm
[0059] (2) Welding resistance evaluation
[0060] Workpiece material: SKD11
[0061] Model: ADKT170608PESR-MM (Comparative Examples 4 to 6, Implementation Example 2)
[0062] Cutting speed: 120m / min
[0063] Cutting transfer: 0.2mm / tooth
[0064] Cutting depth: 5mm
[0065] The processing results evaluated under the above two conditions are shown in Table 2 below.
[0066] [Table 2]
[0067]
[0068] As shown in Table 2 above, the cutting tool according to the embodiment is generally superior to the cutting tool according to the comparative example. Even if the same hard coating is applied, there are significant differences in cutting performance according to the surface treatment of the hard substrate material. In Comparative Examples 2 and 5, the results in which the roughness of the cutting tool is the best are shown, but the life is reduced due to the reduced adhesion between the hard substrate material and the hard film. In Comparative Examples 3 and 6, since the surface roughness of the cutting tool is improved, the life is improved, but there are limitations.
[0069] On the other hand, in Embodiments 1 and 2, peeling and chipping of the hard film were suppressed, and machining was performed most stably in the form of normal wear. Thus, it was confirmed that welding resistance and chipping resistance were improved by surface treatment of the hard base material before film formation.
Claims
1. A hard coating cutting tool, comprising: Hard matrix material; as well as a hard film formed on the hard base material, Among them, if it is assumed that the chromatic diffuse reflectivity value on the front cutting edge of the hard film is L SCER , and the total reflectivity value is L SCIR , then 0.65≤L SCER / L SCIR ≤0.85, and when the surface roughness is measured on the rake face of the hard film within a range of 100 μm from the edge, the arithmetic mean height S aR In 0.2μm≤S aR ≤0.5 μm, and if it is assumed that the chromatic diffuse reflectance value on the side blade surface of the hard film is L SCEF , and the total reflectivity value is L SCIF , then L SCEF / L SCIF ≥0.9, and when the surface roughness is measured on the side cutting surface of the hard film within a range of 100 μm from the edge, the arithmetic mean height S aF At 0.15μm≤S aF In the range of ≤0.4μm.
2. The hard-coated cutting tool according to claim 1, wherein: In the cross section of the cutting tool, on the rake face of the hard base material within a range of 300 μm from the edge, the maximum height roughness R of the hard base material is yR 1μm≤R yR ≤2μm, and In the cross section of the cutting tool, on the side cutting surface of the hard base material within a range of 300 μm from the edge, the maximum height roughness R of the hard base material is yF 2μm≤R yF ≤5μm.
3. The hard-coated cutting tool according to claim 1, wherein: The hard film has a composition satisfying the following Formula 1 and includes one or more films, each of the one or more films having a thickness in the range of 0.1 μm to 10 μm, Formula 1: Al (1-a-b-c) Ti a Cr b Me c N, wherein Me is any one or more of B, Si, Zr, V, Mn, Nb, Mo, Ta, and W, 0≤a≤0.6, 0≤b≤0.5, and 0≤c≤0.15, and must include at least one of Ti and Cr.
4. The hard-coated cutting tool according to claim 1, wherein: On the rake face of the hard film, within 100 μm from the edge, the number of droplets each having a diameter of 3 μm or more is 5% or less of the total number of droplets.