Functional powder as well as preparation method and application thereof
By using dual film forming agent materials in powder production, combining acrylic copolymers and silicone resin coating technology, the problem of insufficient bonding power of the powder is solved, the dispersion and anti-dusity properties of the powder are improved, and the effect of the powder is realized. It has better makeup effect.
Patent Information
- Application Number
- CN202411257997.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-08
AI Technical Summary
In the treatment of modified powders, the film-forming agent is insufficient in binding force, which may cause the powder to detach after use, resulting in dullness in the makeup layer and poor experience.
Using dual film forming agent materials, first add acrylic copolymer to the post-treatment inorganic envelope process for powder production, and then coated with silicone resin to form a core-shell structure to improve the combination of the surface treatment agent of the powder and the powder. Firmness and dispersion.
It improves the anti-mobility and dispersion of the powder, enhances its skin adhesion and anti-dullness in the product, reduces the amount of film-forming agent, and improves the stability and makeup-holding effect of the product.
Smart Images

Figure CN118902875A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cosmetics, in particular to functional powders and preparation methods and applications thereof. Background Art
[0002] After applying makeup, consumers generally complain about the problem that the makeup layer becomes dull and darker as the makeup is worn for a longer time. This phenomenon is called "dullness". The essence of dull makeup is that under the influence of internal factors of the skin and the surrounding environment, the originally uniform and complete makeup layer has the problem of powder rearrangement, that is, the powder particles are unevenly distributed and accumulate in the skin texture, causing the overall visual effect of the makeup to change. In order to improve the problem of dull makeup, one of the current technical means in this field is to add more film-forming agents to the formula to improve the firmness of the makeup layer. However, improper selection of film-forming agents or excessive addition will cause the skin to feel tight and the experience to be poor. Another technical means is to modify the surface of the powder to improve the powder's dispersibility and compatibility with the skin, so as to avoid the rearrangement of powder particles in the makeup layer under the influence of various factors.
[0003] At present, in the post-processing process of traditional powder production, an indispensable inorganic coating process is generally carried out first to shield the photocatalytic activity of the powder and improve durability, and then an organic surface treatment is further performed to increase the added value of the powder. With the growing development of the cosmetics market, consumers' demand for cosmetics products has become more and more refined. The treatment technology of powders has evolved from single surface treatment to multiple composite treatments, and now more and more functional powders are gradually being developed and applied. However, if the new treatment agent is not selected and matched appropriately, and the process is not properly handled, the powder and the surface treatment agent are combined only by physical adsorption, or only by hydrogen bonding without subsequent curing treatment. Both of these bonding forces are weaker than the chemical covalent bond bonding force. In the subsequent application of the formula, the treatment agent may separate from the powder and re-precipitate and agglomerate separately.
[0004] At present, there are many patents for surface modification of powders at home and abroad. Among them, in patent CN 114224747A, the inventor directly uses a film-forming agent solution of a certain viscosity to mix with the powder, and the volatile solvent in the film-forming agent solution evaporates. After the treated powder is dried, the modified powder is obtained; in patent CN 111544340A, the inventor mixes the film-forming agent with the powder at a high speed, so that the film-forming agent is compounded on the surface of the powder to improve the skin adhesion and makeup durability of the product. The above existing technologies are all single film-forming agent treatment powders, and their encapsulation range is limited. The film-forming agent is directly compounded on the surface of the powder. It does not show the specific binding force between the film-forming agent and the powder, and it is impossible to directly indicate whether the modified powder is re-precipitated and dispersed in the product system in actual application; and if the film-forming agent is only physically bonded to the powder, after the application product is used, as the volatile oil in the product system evaporates, the film-forming agent may precipitate out of the powder, resulting in a poor product experience. Among them, patent CN101151015A, the inventor first polymerizes three monomers to form a (meth) acrylic copolymer containing siloxy groups, and then directly mixes it with the powder for surface coating to improve the water resistance and skin adhesion of the powder. During mixing, the silane groups on the treatment agent chain may first contact the powder and only bind to the powder by physical adsorption or hydrogen bonding, and may be separated from the powder during subsequent applications. Secondly, the exposed molecular chains of the acrylic copolymer on the surface of the powder are anionic, which limits the application system of the powder. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides functional powders and preparation methods and applications thereof, wherein the powders are modified by using dual film-forming agent materials, and acrylic copolymers are directly added to the powders for modification in the post-processing inorganic coating process of powder production, and then the powders are further coated with silicone resins, thereby simplifying the process flow of treating powders with composite organic materials, while also improving the surface bonding firmness between the surface treatment agent and the powder, enhancing the dispersibility and anti-migration properties of the powders in product applications, and improving the skin adhesion and long-lasting makeup anti-dullness performance of the applied products.
[0006] The present invention achieves the purpose of the present invention by the following methods:
[0007] The first object of the present invention is to provide a functional powder, which has a core-shell structure, with an original powder particle wrapped with an inorganic film as the core, and a high molecular acrylic copolymer layer and a silicone resin layer sequentially wrapped on the surface of the original powder particle.
[0008] In some embodiments of the present invention, the high molecular weight acrylic copolymer layer is a high molecular weight organic polymer having a carboxylated structure.
[0009] In some embodiments of the present invention, the amount of the acrylic copolymer in the high molecular acrylic copolymer layer is 0.1-10 wt % of the powder particles. The acrylic copolymer is a high molecular weight organic polymer with a carboxylated structure, preferably an acrylic acid (ester) / octylacrylamide copolymer.
[0010] In some embodiments of the present invention, the silicone resin in the silicone resin layer is selected from one or more of trimethylsiloxysilicate, trimethylsiloxysilicate / polydimethylsiloxane crosspolymer, polymethylsilsesquioxane, polypropylsilsesquioxane, diphenylsiloxyphenyl polytrimethylsiloxane, and polyphenylsilsesquioxane.
[0011] In some embodiments of the present invention, the amount of the organic silicone resin in the organic silicone resin layer is 0.1-8 wt % of the powder particles.
[0012] In some embodiments of the present invention, the powder particles are selected from at least one of titanium dioxide, red iron oxide, yellow iron oxide, black iron oxide, talc, mica powder, kaolin, boron nitride, silicon dioxide, chromium oxide green, ultramarine blue, and ultramarine violet.
[0013] The second object of the present invention is to provide a method for preparing the functional powder, comprising the following steps:
[0014] S1, stirring and dispersing the powder particles into a slurry, adding an inorganic coating agent, mixing evenly, adjusting the pH of the mixed solution to neutral or alkaline, and then adding an acrylic acid copolymer, stirring and reacting to obtain powder A;
[0015] S2, adding the organic silicone resin dispersion to the powder A, stirring evenly to obtain powder B;
[0016] S3, filtering, drying and crushing the powder B to obtain the functional powder.
[0017] In some embodiments of the present invention, in step S1, the inorganic coating agent is selected from water-soluble aluminum salts and / or water-soluble silicon salts; preferably, it is a water-soluble aluminum salt. It is worth noting that inorganic coating of the original powder particles is an indispensable process before organic surface treatment in the powder production process, which aims to block and cover the lattice defects of the powder itself, enhance the weather resistance of the powder, and play a role in shielding photocatalytic activity. In the present invention, the inorganic coating agent is fixed to the surface of the original powder particles under the dual forces of physical adsorption and chemical bonding and forms core points for in-situ polymerization. Adjacent core points are continuously polymerized to form a uniform, stable and dense coating.
[0018] In the present invention, in step S1, a high molecular weight acrylic copolymer is directly added to the original powder particle slurry, and the steric hindrance formed by the outward extension of the polymer chain is utilized to limit the spontaneous aggregation movement of the original powder particles in the slurry due to the van der Waals force, so that the original powder is dispersed into a single particle to form a uniform system, thereby avoiding the uneven surface film layer when the original powder particles are inorganically coated due to poor dispersion of the original powder.
[0019] In the present invention, after adding the inorganic coating agent and adjusting the pH in step S1, the acrylic copolymer with a carboxylated structure is immediately added, so that the inorganic coating agent reacts with the original powder to form a coating, and at the same time, the acrylic copolymer polymer chain gradually opens, exposing a plurality of highly reactive carboxyl groups, which have a greater affinity for the surface hydroxyl groups exposed on the original powder, and the carboxyl groups are bonded to the surface hydroxyl groups of the original powder and are also combined with the end groups of the inorganic coating agent on the powder to form a chemical covalent bond, and the two-way bonding makes it more solid. After bonding, the acrylic copolymer molecules penetrate and diffuse on the surface of the coated powder to form a continuous organic coating layer. In addition, the acrylic copolymer is a long carbon chain compound with carbon as the skeleton, and the surface is locally negatively charged. According to the electrostatic stabilization mechanism, when the powder interface after coating is positively charged, the copolymer and the powder are attracted to each other through Coulomb electrostatic attraction, so that the copolymer and the powder are combined with each other, and the acrylic copolymer is firmly combined with the coated powder surface through the dual mechanism of physical adsorption and chemical bonding.
[0020] The amount of the inorganic coating agent used is 0.5-10wt% of the powder particles, preferably 1-5wt%.
[0021] In some embodiments of the present invention, in step S1, the pH range is 7-10. The pH adjustment is specifically: using an acidic or alkaline regulator to adjust the pH to 7-10, preferably adjusting the pH to 9-10. It is worth noting that the pH adjustment here is to use a neutralization method to hydrolyze the inorganic coating agent to deposit a layer of metal hydroxide or hydrated oxide film on the surface of the original powder particles.
[0022] In the present invention, in step S1, the solvent used to disperse the original powder particles into a slurry is deionized water. It is worth noting that deionized water is a conventional dispersion medium used in the post-production coating treatment process of powders in the art. Evenly stirring can disperse the original powder and prepare it into an original powder dispersion. The preparation of the original powder slurry here is to coat the original powder using a wet process, aiming to better allow the treatment agent to fully contact with the original powder particles, and to coat them more evenly and firmly.
[0023] In step S1 of the present invention, the stirring reaction time is 1-10 hours, preferably 3-7 hours, and more preferably 5 hours.
[0024] Furthermore, if the stirring reaction time is too short, the generated coating structure will be loose, and a continuous, uniformly thick, and densely structured coating layer cannot be formed; if the time is too long, the powder production cost will be increased.
[0025] In one embodiment of the present invention, step S2 specifically comprises: transferring powder A into a blender, adding pre-dispersed silicone resin dispersion, stirring and reacting in the blender for a period of time, and obtaining powder B with the silicone resin coated on the surface.
[0026] In one embodiment of the present invention, in step S2, the silicone resin is a film-forming substance, selected from one or more of trimethylsiloxysilicate, trimethylsiloxysilicate / polydimethylsiloxane crosspolymer, polymethylsilsesquioxane, polypropylsilsesquioxane, diphenylsiloxyphenyl polytrimethylsiloxane, and polyphenylsilsesquioxane, preferably trimethylsiloxysilicate or polymethylsilsesquioxane.
[0027] Furthermore, silicone resin is an organic polymer of polysiloxane with Si-O-Si as the main chain, organic groups connected to silicon atoms, and hydroxyl groups at the end groups, and has a dense three-dimensional network structure. At the same time, silicone resin and commonly used silicone oil components in cosmetics have a silicon-oxygen bonding structure, are highly compatible, and can be well dispersed in cosmetics.
[0028] In one embodiment of the present invention, in step S2, the dispersion medium of the organic silicone resin dispersion is a volatile liquid, and is not limited to a specific type, as long as it can disperse the organic silicone resin to open its structure and is volatile.
[0029] Furthermore, after the organic silicone resin is dispersed to form a dispersion, the network structure unfolds, exposing more hydroxyl contact angles, chemically bonding with the carboxyl groups of the acrylic copolymer in the organic coating layer on the surface of powder A, and hydrogen bonding with the exposed hydroxyl groups of powder A, and the silicone resin macromolecular structure opens, entangled and cross-linked with the polymer chains of the acrylic copolymer; that is, the silicone resin forms a dense three-dimensional network structure of the polysilicic acid coating layer on the surface of powder A through the synergistic action of the triple binding forces of chemical bonding, hydrogen bonding and physical attachment.
[0030] Furthermore, the present invention provides a method for preparing functional powders, wherein acrylic copolymer is first completely bonded with the coated powder, and then an organic silicone resin is added for coating, so as to ensure that the acrylic copolymer is bonded with a stable chemical covalent bond between the powder and the organic silicone resin; secondly, most of the acrylic macromolecular polymers are anionic, and as the inner layer of the powder coating layer, it strengthens the mutual attraction and bonding between the powder and the powder through the Coulomb electrostatic attraction, and also avoids excessive exposure of anions in its molecular chain, resulting in compatibility problems with the cationic raw materials in the application system of the coated powder. In addition, the organic silicone resin is terminated on the powder surface with a molecular chain containing a siloxy group, and the terminated molecular chains are intertwined with each other, forming a continuous and complete layer of exposed siloxane molecular chains on the powder surface coated with the acrylic copolymer, which has a similar siloxane bonding structure to the silicone oil in the commonly used application system, thereby improving the compatibility and dispersibility of the powder in the system.
[0031] Furthermore, the acrylic copolymer and the silicone resin both have a certain film-forming effect, and the coated powder is subjected to organic surface treatment, which synergistically improves the anti-friction and anti-migration properties of the powder itself from the root, and the powder is automatically and firmly attached to the skin when applied to cosmetic products, giving the makeup layer persistence and tolerance, resisting internal influences such as skin secretions or microscopic movements of the skin, and responding to external influences such as touch. Secondly, the powder surface is coated with a double polymer organic layer, and the surface-terminated macromolecular chains form a steric hindrance, avoiding the Brownian motion between the powder particles to cause collisions to form agglomerates, improving the dispersibility of the powder in cosmetic products, improving the stability of the product system, and reducing the difference between its apparent color and smear color.
[0032] In one embodiment of the present invention, in step S2, the amount of the silicone resin used is 0.1-8Wt% of the original powder, preferably 1-4Wt%.
[0033] In one embodiment of the present invention, in step S2, the stirring time is 2-8 hours, preferably 5 hours.
[0034] Furthermore, when the stirring time is too short, the silicone resin is not completely reacted and bonded to the powder A, and only forms a polymer through its own hydroxyl group and accumulates on the powder through physical adsorption. Its physical binding force is weak and it is easy to separate from the powder in subsequent product applications; if the time is too long, the production cost of the powder will increase.
[0035] In one embodiment of the present invention, the filtering, drying and pulverizing in step S3 are commonly used means for powder production in the technical field. The instruments used are not specifically limited. The solvent in powder B can be filtered, the powder can be dried and the powder can be pulverized into fine powder.
[0036] The third object of the present invention is to provide a color cosmetic comprising the functional powder.
[0037] The above technical solution of the present invention has the following advantages compared with the prior art:
[0038] The present invention adopts acrylic copolymer and organic silicon resin to carry out organic surface treatment on powder, wherein acrylic copolymer coating is directly carried out simultaneously in the powder inorganic coating process, thereby simplifying the process of coating the powder surface with double film-forming agent organic materials.
[0039] The present invention adopts a carboxylated high molecular acrylic copolymer as the inner layer of the double organic coating layer, and the carboxyl groups with high reactivity on the molecular chain thereof form a strong chemical covalent bond with the groups on the original powder and the inorganic coating agent; at the same time, the extended molecular chain thereof is cross-linked and entangled with the high molecular chain of the organic silicone resin, and the carboxyl groups thereof form a chemical bond with the terminal hydroxyl groups of the silicone resin; the double organic polymer is coated with the powder particles under the synergistic action of the triple bonding bonds of chemical covalent bonds, hydrogen bonds and physical bonds, so as to form a double-layer continuous, dense, stable and strong organic coating layer, thereby avoiding the situation that the organic coating layer on the surface of the powder is separated from the powder and recrystallized and precipitated due to the influence of the high-speed stirring process and the various components when the powder is subsequently applied to cosmetic products.
[0040] The present invention uses a dual organic polymer with film-forming properties to perform surface treatment on the powder, and the acrylic copolymer and the silicone resin are cross-linked to form a coating layer with a three-dimensional network structure, which synergistically improves the dispersibility, firmness and migration resistance of the powder, and improves the waterproof, sweat-proof and sebum-resistant properties of the powder; when the functional powder is used in a makeup product, it forms a makeup-control film after application, which helps to improve the product's long-lasting makeup and anti-dullness properties, and can reduce the amount of film-forming agent used in the formula. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:
[0042] Figure 1 Schematic diagram of the organic coating layer of functional powders.
[0043] Figure 2 These are microscopic observation pictures of the powders prepared in Example 6 and Comparative Example 1 dispersed in synthetic oil. In the picture, A represents the microscopic observation picture of the functional powder prepared in Example 6 in synthetic oil, and B represents the microscopic observation picture of the powder prepared in Comparative Example 1 in synthetic oil.
[0044] Figure 3 These are microscopic observation pictures of the liquid foundation bodies of Application Example 1 and Application Comparative Example 1. In the pictures, A represents the microscopic observation picture of the liquid foundation body of Application Example 1, and B represents the microscopic observation picture of the liquid foundation body of Application Comparative Example 1. DETAILED DESCRIPTION
[0045] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0046] Unless otherwise specified, the raw materials, reagents or devices used in the examples of the present invention can be obtained from conventional commercial sources.
[0047] Example 1
[0048] This embodiment provides a method for preparing functional powder, and the specific steps are as follows:
[0049] S1. Pour 100g of titanium dioxide and deionized water into a stirrer and stir to disperse into a slurry, add 1g of water-soluble aluminum sulfate, mix well, adjust the pH to 9-10 with an alkaline regulator (10wt% sodium hydroxide aqueous solution), add 1g of acrylic acid (ester) / octylacrylamide copolymer, stir well for 5 hours, and react to obtain powder A;
[0050] S2. Powder A is transferred into a stirrer, 1 g of trimethylsiloxysilicate isomeric dodecane solution is added, and the mixture is stirred for 5 hours to obtain powder B;
[0051] S3. Powder B is transferred into a filter for filtration, and the solid matter obtained by filtration is then transferred into a constant temperature drying oven at 105° C. for drying for 2 hours, and then transferred into a grinder for pulverization to obtain functional powder.
[0052] Example 2
[0053] This embodiment provides a method for preparing functional powder, and the specific steps are as follows:
[0054] S1. Pour 100 g of titanium dioxide and deionized water into a stirrer and stir to disperse into a slurry, add 3 g of water-soluble aluminum sulfate, mix well, adjust the pH to 9-10 with an alkaline regulator (10 wt % sodium hydroxide aqueous solution), add 1 g of acrylic acid (ester) / octylacrylamide copolymer, stir well for 5 hours, and react to obtain powder A;
[0055] S2. Powder A is transferred into a stirrer, 1 g of trimethylsiloxysilicate isomeric dodecane solution is added, and the mixture is stirred for 5 hours to obtain powder B;
[0056] S3. Powder B is transferred into a filter for filtration, and the solid matter obtained by filtration is then transferred into a constant temperature drying oven at 105° C. for drying for 2 hours, and then transferred into a grinder for pulverization to obtain functional powder.
[0057] Example 3
[0058] This embodiment provides a method for preparing functional powder, and the specific steps are as follows:
[0059] S1. Pour 100g of titanium dioxide and deionized water into a stirrer and stir to disperse into a slurry, add 5g of water-soluble aluminum sulfate, mix well, adjust the pH to 9-10 with an alkaline regulator (10wt% sodium hydroxide aqueous solution), add 1g of acrylic acid (ester) / octylacrylamide copolymer, stir well for 5 hours, and react to obtain powder A;
[0060] S2. Powder A is transferred into a stirrer, 1 g of trimethylsiloxysilicate isomeric dodecane solution is added, and the mixture is stirred for 5 hours to obtain powder B;
[0061] S3. Powder B is transferred into a filter for filtration, and the solid matter obtained by filtration is then transferred into a constant temperature drying oven at 105° C. for drying for 2 hours, and then transferred into a grinder for pulverization to obtain functional powder.
[0062] Example 4
[0063] This embodiment provides a method for preparing functional powder, and the specific steps are as follows:
[0064] S1. Pour 100 g of titanium dioxide and deionized water into a stirrer and stir to disperse into a slurry, add 3 g of water-soluble aluminum sulfate, mix well, adjust the pH to 9-10 with an alkaline regulator (10 wt % sodium hydroxide aqueous solution), add 2 g of acrylic acid (ester) / octylacrylamide copolymer, stir well for 5 hours, and react to obtain powder A;
[0065] S2. Powder A is transferred into a stirrer, 1 g of trimethylsiloxysilicate isomeric dodecane solution is added, and the mixture is stirred for 5 hours to obtain powder B;
[0066] S3. Powder B is transferred into a filter for filtration, and the solid matter obtained by filtration is then transferred into a constant temperature drying oven at 105° C. for drying for 2 hours, and then transferred into a grinder for pulverization to obtain functional powder.
[0067] Example 5
[0068] This embodiment provides a method for preparing functional powder, and the specific steps are as follows:
[0069] S1. Pour 100 g of titanium dioxide and deionized water into a stirrer and stir to disperse into a slurry, add 3 g of water-soluble aluminum sulfate, mix well, adjust the pH to 9-10 with an alkaline regulator (10 wt % sodium hydroxide aqueous solution), add 3 g of acrylic acid (ester) / octylacrylamide copolymer, stir well for 5 hours, and react to obtain powder A;
[0070] S2. Powder A is transferred into a stirrer, 1 g of trimethylsiloxysilicate isomeric dodecane solution is added, and the mixture is stirred for 5 hours to obtain powder B;
[0071] S3. Powder B is transferred into a filter for filtration, and the solid matter obtained by filtration is then transferred into a constant temperature drying oven at 105° C. for drying for 2 hours, and then transferred into a grinder for pulverization to obtain functional powder.
[0072] Example 6
[0073] This embodiment provides a method for preparing functional powder, and the specific steps are as follows:
[0074] S1. Pour 100 g of titanium dioxide and deionized water into a stirrer and stir to disperse into a slurry, add 3 g of water-soluble aluminum sulfate, mix well, adjust the pH to 9-10 with an alkaline regulator (10 wt % sodium hydroxide aqueous solution), add 2 g of acrylic acid (ester) / octylacrylamide copolymer, stir well for 5 hours, and react to obtain powder A;
[0075] S2, transfer powder A into a stirrer, add 2 g of isomeric dodecane solution of trimethylsiloxysilicate, and stir thoroughly for 5 hours to obtain powder B;
[0076] S3. Powder B is transferred into a filter for filtration, and the solid matter obtained by filtration is then transferred into a constant temperature drying oven at 105° C. for drying for 2 hours, and then transferred into a grinder for pulverization to obtain functional powder.
[0077] Example 7
[0078] This embodiment provides a method for preparing functional powder, and the specific steps are as follows:
[0079] S1. Pour 100g of titanium dioxide and deionized water into a stirrer and stir to disperse into a slurry, add 3g of water-soluble aluminum sulfate, mix well, adjust the pH to 9-10 with a 10wt% sodium hydroxide aqueous solution as an alkaline regulator, add 2g of acrylic acid (ester) / octylacrylamide copolymer, stir well for 5 hours, and react to obtain powder A;
[0080] S2, transfer powder A into a stirrer, add 3 g of isomeric dodecane solution of trimethylsiloxysilicate, and stir thoroughly for 5 hours to obtain powder B;
[0081] S3. Powder B is transferred into a filter for filtration, and the solid matter obtained by filtration is then transferred into a constant temperature drying oven at 105° C. for drying for 2 hours, and then transferred into a grinder for pulverization to obtain functional powder.
[0082] Example 8
[0083] This embodiment provides a method for preparing functional powder, and the specific steps are as follows:
[0084] S1. Pour 100 g of titanium dioxide and deionized water into a stirrer and stir to disperse into a slurry, add 3 g of water-soluble aluminum sulfate, mix well, adjust the pH to 9-10 with an alkaline regulator (10 wt % sodium hydroxide aqueous solution), add 2 g of acrylic acid (ester) / octylacrylamide copolymer, stir well for 5 hours, and react to obtain powder A;
[0085] S2, transfer powder A into a stirrer, add 2 g of isododecane solution of polymethylsilsesquioxane, and stir thoroughly for 5 hours to obtain powder B;
[0086] S3. Powder B is transferred into a filter for filtration, and the solid matter obtained by filtration is then transferred into a constant temperature drying oven at 105° C. for drying for 2 hours, and then transferred into a grinder for pulverization to obtain functional powder.
[0087] Example 9
[0088] This embodiment provides a method for preparing functional powder, and the specific steps are as follows:
[0089] S1. Pour 100g of yellow iron oxide and deionized water into a stirrer and stir to disperse into a slurry, add 3g of water-soluble aluminum sulfate, mix well, adjust the pH to 9-10 with an alkaline regulator (10wt% sodium hydroxide aqueous solution), add 2g of acrylic acid (ester) / octylacrylamide copolymer, stir well for 5 hours, and react to obtain powder A;
[0090] S2, transfer powder A into a stirrer, add 2 g of isomeric dodecane solution of trimethylsiloxysilicate, and stir thoroughly for 5 hours to obtain powder B;
[0091] S3. Powder B is transferred into a filter for filtration, and the solid matter obtained by filtration is then transferred into a constant temperature drying oven at 105° C. for drying for 2 hours, and then transferred into a grinder for pulverization to obtain functional powder.
[0092] Example 10
[0093] This embodiment provides a method for preparing functional powder, and the specific steps are as follows:
[0094] S1. Pour 100 g of red iron oxide and deionized water into a stirrer and stir to disperse into a slurry, add 3 g of water-soluble aluminum sulfate, mix well, adjust the pH to 9-10 with an alkaline regulator (10 wt % sodium hydroxide aqueous solution), add 2 g of acrylic acid (ester) / octylacrylamide copolymer, stir well for 5 hours, and react to obtain powder A;
[0095] S2, transfer powder A into a stirrer, add 2 g of isomeric dodecane solution of trimethylsiloxysilicate, and stir thoroughly for 5 hours to obtain powder B;
[0096] S3. Powder B is transferred into a filter for filtration, and the solid matter obtained by filtration is then transferred into a constant temperature drying oven at 105° C. for drying for 2 hours, and then transferred into a grinder for pulverization to obtain functional powder.
[0097] Embodiment 11
[0098] This embodiment provides a method for preparing functional powder, and the specific steps are as follows:
[0099] S1. Pour 100g of black iron oxide and deionized water into a stirrer and stir to disperse into a slurry, add 3g of water-soluble aluminum sulfate, mix well, adjust the pH to 9-10 with an alkaline regulator (10wt% sodium hydroxide aqueous solution), add 2g of acrylic acid (ester) / octylacrylamide copolymer, stir well for 5 hours, and react to obtain powder A;
[0100] S2, transfer powder A into a stirrer, add 2 g of isomeric dodecane solution of trimethylsiloxysilicate, and stir thoroughly for 5 hours to obtain powder B;
[0101] S3. Powder B is transferred into a filter for filtration, and the solid matter obtained by filtration is then transferred into a constant temperature drying oven at 105° C. for drying for 2 hours, and then transferred into a grinder for pulverization to obtain functional powder.
[0102] Comparative Example 1
[0103] This comparative example provides a powder, which is different from the embodiment in that only the original powder is subjected to inorganic coating treatment, and the powder is not subjected to organic polymer coating treatment. The specific steps are as follows:
[0104] S1. Pour 100 g of titanium dioxide and deionized water into a stirrer and stir to disperse into a slurry, add 3 g of water-soluble aluminum sulfate, mix well, adjust the pH to 9-10 with an alkaline regulator (10 wt % sodium hydroxide aqueous solution), stir well for 5 hours, and react to obtain powder A;
[0105] S2. Powder A is transferred into a filter for filtration, and the solid matter obtained by filtration is transferred into a 105°C constant temperature drying oven for drying for 2 hours, and then transferred into a pulverizer for pulverization to obtain a powder.
[0106] Comparative Example 2
[0107] This comparative example provides a powder, which is different from the embodiment in that only the original powder is subjected to inorganic coating and acrylic copolymer single-layer organic coating treatment, and no silicone resin coating treatment is performed. The specific steps are as follows:
[0108] S1. Pour 100 g of titanium dioxide and deionized water into a stirrer and stir to disperse into a slurry, add 3 g of water-soluble aluminum sulfate, mix well, adjust the pH to 9-10 with an alkaline regulator (10 wt % sodium hydroxide aqueous solution), add 2 g of acrylic acid (ester) / octylacrylamide copolymer, stir well for 5 hours, and react to obtain powder A;
[0109] S2. Powder A is transferred into a filter for filtering, and the solid matter obtained by filtration is transferred into a constant temperature drying oven at 105° C. for drying for 2 hours, and then transferred into a grinder for crushing to obtain functional powder.
[0110] Comparative Example 3
[0111] This comparative example provides a powder, which is different from the embodiment in that only the original powder is subjected to inorganic coating and single-layer organic coating of silicone resin, and no acrylic copolymer coating is performed. The specific steps are as follows:
[0112] S1. Pour 100 g of titanium dioxide and deionized water into a stirrer and stir to disperse into a slurry, add 3 g of water-soluble aluminum sulfate, mix well, adjust the pH to 9-10 with an alkaline regulator (10 wt % sodium hydroxide aqueous solution), stir well for 5 hours, and react to obtain powder A;
[0113] S2, transfer powder A into a stirrer, add 2 g of isomeric dodecane solution of trimethylsiloxysilicate, and stir thoroughly for 5 hours to obtain powder B;
[0114] S3. Powder B is transferred into a filter for filtration and then transferred into a 105°C constant temperature drying oven for drying for 2 hours, and then transferred into a grinder for crushing to obtain functional powder.
[0115] Comparative Example 4
[0116] This comparative example provides a powder, and the process for treating yellow iron oxide is the same as that of comparative example 1, and the specific steps are as follows:
[0117] S1. Pour 100g of yellow iron oxide and deionized water into a stirrer and stir to disperse into a slurry, add 3g of water-soluble aluminum sulfate, mix well, adjust the pH to 9-10 with an alkaline regulator (10wt% sodium hydroxide aqueous solution), stir well for 5 hours, and react to obtain powder A;
[0118] S2. Powder A is transferred into a filter for filtering, then transferred into a 105°C constant temperature drying oven for drying for 2 hours, and then transferred into a pulverizer for pulverization to obtain a powder.
[0119] Comparative Example 5
[0120] This comparative example provides a powder, and the process for treating red iron oxide is the same as that of comparative example 1, and the specific steps are as follows:
[0121] S1. Pour 100 g of red iron oxide and deionized water into a stirrer and stir to disperse into a slurry, add 3 g of water-soluble aluminum sulfate, mix well, adjust the pH to 9-10 with an alkaline regulator (10 wt % sodium hydroxide aqueous solution), stir well for 5 hours, and react to obtain powder A;
[0122] S2. Powder A is transferred into a filter for filtering, then transferred into a 105°C constant temperature drying oven for drying for 2 hours, and then transferred into a pulverizer for pulverization to obtain a powder.
[0123] Comparative Example 6
[0124] This comparative example provides a powder, and the process for treating black iron oxide is the same as that of comparative example 1, and the specific steps are as follows:
[0125] S1. Pour 100 g of black iron oxide and deionized water into a stirrer and stir to disperse into a slurry, add 3 g of water-soluble aluminum sulfate, mix well, adjust the pH to 9-10 with an alkaline regulator (10 wt % sodium hydroxide aqueous solution), stir well for 5 hours, and react to obtain powder A;
[0126] S2. Powder A is transferred into a filter for filtering, then transferred into a 105°C constant temperature drying oven for drying for 2 hours, and then transferred into a pulverizer for pulverization to obtain a powder.
[0127] Contact angle test
[0128] Take an appropriate amount of powder in a powder cake pan and use a powder press to press it into a powder cake. Deionized water, artificial sweat, and artificial sebum are used as contact liquids. Use a pipette to drop 5μL of the three contact liquids on the surface of the pressed powder cake, and use a contact angle analyzer to observe and record the contact angle of the droplets. According to the contact angle principle, the larger the contact angle when the contact liquid contacts the powder cake interface, the better the resistance of the powder. The contact angle test results of different contact liquids are shown in Table 1.
[0129] Table 1 Contact angle test results of different contact liquids
[0130]
[0131]
[0132] From the results in Table 1, we can see that:
[0133] 1. From the comparison results of Examples 1-11 and Comparative Examples 1 and 4-6, it can be seen that under the three contact liquids, the contact angles of Comparative Examples 1 and 4-6 are all 0°, indicating that organic coating treatment of the powder can improve its water, sweat and sebum resistance.
[0134] 2. From the comparison results of Examples 1-11 and Comparative Examples 2-3, it can be seen that under the three contact liquids, the contact angles of Examples 1-11 are larger than those of Comparative Examples 2-3, indicating that the double-layer organic coating is more helpful in improving the water-resistant, sweat-resistant and sebum-resistant properties of the powder than the single-layer organic coating; and by comparing the results of Example 1 and Comparative Examples 2-3, the contact angle of Example 1 is also greater than the contact angle of Comparative Examples 2-3, indicating that when the total amount of organic coating agent is constant, the use of acrylic copolymer and silicone resin dual organic material composite coating is better than the single coating of the powder, and can synergistically improve the water-resistant, sweat-resistant and sebum-resistant properties of the powder.
[0135] 3. From the comparison results of Examples 1-3, it can be seen that as the amount of the inorganic coating agent increases, the corresponding contact angle changes with deionized water and artificial sweat as the contact liquid are not particularly obvious; with artificial sebum as the contact liquid, the corresponding contact angle increases first, and when it reaches a certain amount, the rate of increase of the contact angle slows down, indicating that the inorganic coating agent has completely coated the original powder, avoiding increasing the cost of powder surface treatment, and the optimal amount of the inorganic coating agent to coat the original powder is 3wt% of the original powder.
[0136] 4. From the comparison results of Example 2 and Examples 4-5, it can be seen that as the amount of the organic coating agent acrylic copolymer increases, the corresponding contact angles of the three different contact liquids all increase significantly. However, when a certain amount is reached, the contact angles of the three contact liquids increase more slowly when the amount of acrylic copolymer is increased. This indicates that the hydroxyl groups on the original powder and the bonding between the inorganic coating agent and the acrylic copolymer on its surface have reached a saturated state. In order to reduce the production cost of the organic surface coating of the powder, the optimal amount of the acrylic copolymer coated powder is 2Wt% of the original powder.
[0137] 5. From the comparison results of Example 4 and Examples 6-8, it can be seen that with the increase in the dosage of the silicone resin film-forming agent, the contact angles of the three different contact liquids all increase rapidly, but at a certain dosage, the contact angle does not increase significantly, indicating that the coating of the powder by the silicone resin film-forming agent has reached a completely saturated state, and further addition of the silicone resin may cause excessive overflow. The optimal dosage of the silicone resin coating powder is 2wt% of the original powder. From the comparison results of Example 6 and Example 8, it can be seen that under the three contact liquids, the contact angle of Example 6 is slightly larger than the contact angle of Example 8, indicating that the use of trimethylsiloxysilicate is better than polymethylsilsesquioxane for the second layer of organic coating of the powder.
[0138] Dispersion test
[0139] The powders prepared in Examples 1-11 and Comparative Examples 1-6 were dispersed in representative oils of three types of oils, namely mineral oil, silicone oil and synthetic oil; the powder content in the dispersion system was 20%, and then a homogenizer was used to homogenize at a speed of 6000 r / min for 4 minutes to obtain a uniform system, and a biological microscope was used to microscopically observe the dispersion or aggregation of the dispersion system. The dispersion test results are shown in Table 2.
[0140] Table 2 Dispersion test results
[0141]
[0142]
[0143] From the results in Table 2, we can see that:
[0144] By comparing the dispersion results of Examples 1-11 and Comparative Examples 1-6, it can be seen that the powder coated with acrylic copolymer and silicone resin can improve the dispersion performance of the powder, and further comparing Example 6 with Comparative Examples 2-3, it can be seen that the powder coated with dual organic materials of acrylic copolymer and silicone resin has better dispersibility than the powder coated alone, and there is no situation in which the surface coating agent of the powder is precipitated due to poor binding force when the powder is stirred at high speed during use, resulting in obvious aggregation of the powder, indicating that the acrylic copolymer, as an organic coating inner layer, forms a strong chemical covalent bond with the powder and the hydroxyl group of the silicone resin through the carboxyl group on the chain; and the dual organic polymer coats the powder particles through the synergistic action of the triple bonding bonds of chemical covalent bonds, hydrogen bonds and physical bonds, and the comprehensive binding force between the powder and the dual organic coating agent is stronger than the binding force between the powder and the acrylic copolymer or the silicone resin alone.
[0145] Application Example 1
[0146] The functional powders prepared in Examples 6 and 9-11 of the present invention were formulated according to the foundation liquid formula shown in Table 3 to obtain sample A. The total mass of the formula components was 100 g.
[0147] Application Comparative Example 1
[0148] The powders prepared in Comparative Example 1 and Comparative Examples 4-6 of the present invention were formulated according to the liquid foundation formula shown in Table 3 to obtain sample B. The total mass of the formula components was 100 g.
[0149] Table 3 Liquid foundation formula
[0150]
[0151]
[0152] Note: The raw materials in Table 3 are connected by “&”, which means that the component is a composite raw material and is a whole.
[0153] The liquid foundation of Application Example 1 and Application Comparative Example 1 was prepared by the following process steps:
[0154] (1) Weigh phase A and add it into a beaker, stir evenly, and disperse evenly with high-speed homogenizer;
[0155] (2) Weighing phase B and adding it to the mixture of step (1), stirring and heating to 70° C., and dispersing evenly by high-speed homogenization;
[0156] (3) Weigh the raw materials of phase C and add them into a beaker. Stir and dissolve evenly in a 70°C water bath.
[0157] (4) While heating in a 70° C. water bath and stirring rapidly, slowly pour the mixture of step (3) into the mixture of step (2), stir evenly, and homogenize at high speed after complete emulsification; start cooling, and when the temperature drops below 40° C., add phase D and stir evenly at low speed.
[0158] (5) After the mixture is cooled to room temperature, the mixture is discharged to obtain a liquid foundation.
[0159] Liquid foundation anti-dullness performance test
[0160] In vitro testing of foundation products for makeup durability and anti-dullness often uses the L*a*b* colorimetric system to comprehensively evaluate and reflect the change in color. The color difference comprehensive deviation △E is obtained by testing the color value change using a colorimeter; the smaller the △E, the better the anti-dullness effect and the better the makeup durability. The test method is determined specifically under three different conditions: ① Under the influence of natural dullness conditions: take the foundation liquid on the PMMA board, use the applicator to evenly apply a 50-micron thick sample on the PMMA board, use the colorimeter to measure the initial color value, record the position, and measure the color value again after 3 hours. Test three times in parallel, measuring 5 points each time. ② Under the influence of artificial sweat conditions: take the foundation liquid on the PMMA board, use the applicator to evenly apply a 50-micron thick sample on the PMMA board, let it stand for half an hour, test the initial color value, record the position, put it in 37℃ artificial sweat to soak for 30 minutes, take it out and dry it for 4 hours, and measure the color value again. Test three times in parallel, measuring 5 points each time. ③ Under the influence of artificial sebum conditions: weigh the foundation liquid and artificial sebum and stir and mix them evenly to obtain a mixture. Take the mixture on the PMMA plate, use an applicator to evenly apply a 50 micron thick sample, test the initial color value, record the position, put it in an empty beaker and place it in a 37°C water bath, take it out after 3 hours and measure the color value again. Test three times in parallel, each time measuring 5 points. The specific test color difference comprehensive deviation △E index results are shown in Table 4.
[0161] Table 4 Test results of anti-dullness performance of liquid foundation
[0162]
[0163] Liquid foundation microstructure observation test
[0164] Take a drop of foundation liquid on a glass slide, cover it with a glass slide, press it lightly, place it under a biological microscope, adjust the parameters of the 10x eyepiece and 10x objective lens, and observe the microscopic conditions of the foundation liquid materials of Application Example 1 and Comparative Example 1. See the attached Figure 3 .
[0165] From the results in Table 4 and the attached Figure 3 It can be seen that:
[0166] 1. From the attachment Figure 3 It can be seen that compared with the corresponding proportion 1, the powder liquid material of Example 1 is finer and more uniform, and there is no situation in which the organic coating layer is separated from the powder and precipitated due to poor binding force, resulting in powder aggregation. In addition, in actual application, the functional powder has a steric hindrance formed by the surface-capped polysilicate macromolecular network structure, which reduces the probability of collision between powder particles and disperses more evenly, helping to improve the stability of the product.
[0167] 2. From the comparison results in Table 4, it can be seen that under the influence of different conditions, the color difference value of Example 1 is smaller than that of Comparative Example 1, that is, the functional powder is applied to the product and its long-lasting makeup and anti-dullness effect is better. It can be seen that the present invention uses acrylic copolymer with film-forming properties and silicone resin to double-film-forming agent coating of the powder and applies it to cosmetic products to help improve the skin adhesion of the product and the long-lasting waterproof, sweat-proof and anti-sebum effects, increase the makeup holding time, and improve its persistence or tolerance to internal factors such as skin secretions or skin micro-expression movements after makeup, as well as external factors such as scratches.
[0168] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. Functional powder, characterized in that: The functional powder is a core-shell structure, with the original powder particles wrapped with an inorganic film as the core, and a high-molecular acrylic copolymer layer and an organic silicone resin layer sequentially wrapped on the surface of the powder particles.
2. The functional powder according to claim 1, characterized in that: The high molecular acrylic copolymer layer is a high molecular organic polymer having a carboxylated structure.
3. The functional powder according to claim 1, characterized in that: The amount of the acrylic copolymer in the high molecular acrylic copolymer layer is 0.1-10 wt % of the powder particles.
4. The functional powder according to claim 1, characterized in that: The organic silicone resin in the organic silicone resin layer is selected from one or more of trimethylsiloxysilicate, trimethylsiloxysilicate / polydimethylsiloxane cross-linked polymer, polymethylsilsesquioxane, polypropylsilsesquioxane, diphenylsiloxyphenyl polytrimethylsiloxane, and polyphenylsilsesquioxane.
5. The functional powder according to claim 1, characterized in that: The amount of the organic silicone resin in the organic silicone resin layer is 0.1-8 wt % of the powder particles.
6. The functional powder according to claim 1, characterized in that: The original powder particles are selected from at least one of titanium dioxide, red iron oxide, yellow iron oxide, black iron oxide, talcum powder, mica powder, kaolin, boron nitride, silicon dioxide, chromium oxide green, ultramarine blue and ultramarine violet.
7. The method for preparing the functional powder according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. The original powder particles are stirred and dispersed into a slurry, an inorganic coating agent is added, the mixture is mixed evenly, the pH of the mixture is adjusted to neutral or alkaline, and then an acrylic acid copolymer is added, and the mixture is stirred and reacted to obtain powder A; S2, adding the organic silicone resin dispersion to the powder A, stirring evenly, to obtain powder B; S3. Filter, dry and crush the powder B to obtain the functional powder.
8. The preparation method according to claim 7, characterized in that: In step S1, the inorganic coating agent is selected from water-soluble aluminum salt and / or water-soluble silicon salt; The amount of the inorganic coating agent used is 0.5-10wt% of the powder particles.
9. The preparation method according to claim 7, characterized in that: In step S1, the pH range is 7-10.
10. A color cosmetic, characterized in that: The functional powder comprises the functional powder according to any one of claims 1 to 6.