Method for preparing anti-pollution polyamide nanofiltration composite membrane based on hydrothermal method

The anti-polluting polyamide nanofiltration composite membrane was prepared by hydrothermal method, and a hydrated layer was formed in the thermal curing process of water bath using fluorine-containing surfactant, which solved the problem of nanofiltration membrane pollution, simplified the preparation process and improved the anti-pollution performance and water Molecular permeability.

CN118904091AActive Publication Date: 2024-11-08CHINA UNIV OF PETROLEUM (EAST CHINA)
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411037772.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-08
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

Nanofiltration membranes have serious membrane pollution problems in sewage treatment, resulting in reduced membrane flux, shortened service life and increased energy consumption. The existing surface modification method for preparing anti-polluting polyamide nanofiltration membranes is complicated and multiple grafts lead to membranes. The thickness increases, affecting the permeability of water molecules.

Method used

The anti-polluting polyamide nanofiltration composite membrane was prepared by hydrothermal method. A hydrated layer was formed during the thermal curing process of water bath by fluorinated surfactants. The hydrophilic end penetrated into the membrane holes and the hydrophobic end was exposed to the membrane surface, which simplified the preparation process and improved the Anti-pollution performance.

Benefits of technology

The preparation process is simplified, the anti-pollution and pollutant release ability of the composite membrane is improved, the interaction between the membrane surface and pollutants is reduced, the service life of the membrane is extended, and the permeability of water molecules is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904091A_ABST
    Figure CN118904091A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing an anti-pollution polyamide nanofiltration composite membrane based on a hydrothermal method, which comprises the following steps: (1) carrying out interlayer modification on a porous base membrane by using polyphenol-polyethyleneimine interlayer modification liquid, and marking as a PSF membrane; (2) carrying out interfacial polymerization reaction on the PSF membrane by using organic amine and organic acyl chloride to prepare a polyamide layer marked as a TFC membrane; and (3) putting the TFC membrane into a fluorine-containing surfactant aqueous solution, and heating in a water bath at 50-80 DEG C to obtain the anti-pollution nanofiltration composite membrane with stable crosslinking. The fluorine-containing surfactant is used for carrying out water bath thermocuring on the polyamide membrane, the hydrophilic end of the fluorine-containing surfactant permeates into membrane holes during hydrothermal crosslinking, a hydration layer is constructed on the surface of the membrane to resist pollutants, the hydrophobic end is exposed on the surface of the membrane, interaction between the surface of the membrane and the pollutants is weakened, release of the pollutants on the surface of the membrane is promoted, and the water-soluble polyamide membrane is prepared. The composite membrane has the capacity of resisting and releasing pollutants, the preparation process is simple, convenient and easy to amplify, and the composite membrane has industrial application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of anti-pollution nanofiltration composite membranes, and in particular to a method for preparing an anti-pollution polyamide nanofiltration composite membrane based on a hydrothermal method. Background Art

[0002] In the field of sewage treatment, nanofiltration membrane (NF) separation technology has broad application prospects due to its low energy consumption and wide application range. However, there are serious membrane pollution problems in the actual application of nanofiltration membranes. Pollutants will adhere to the membrane surface, resulting in a significant decrease in membrane flux, shortened service life, increased energy consumption and frequent cleaning. The main influencing factor of membrane pollution is membrane performance. The preparation of anti-pollution polyamide nanofiltration membranes through surface modification can reduce membrane pollution during wastewater treatment and fundamentally overcome the bottleneck of industrial application of nanofiltration membranes. At present, the preparation of anti-pollution polyamide nanofiltration membranes through surface modification usually adopts a method combining multiple grafting and thermal curing. The steps are cumbersome, which increases the difficulty of membrane preparation. In addition, multiple grafting usually leads to an increase in membrane thickness, and the number of active sites on the membrane surface after thermal curing is limited, which has a certain impact on the permeability of water molecules. Summary of the invention

[0003] In order to solve the above technical problems, the present invention provides a method for preparing anti-pollution polyamide nanofiltration composite membrane based on hydrothermal method, wherein the polyamide membrane is thermally cured in a water bath using a fluorinated surfactant. During hydrothermal crosslinking, the hydrophilic end of the fluorinated surfactant penetrates into the membrane pores, and a hydration layer is constructed on the membrane surface to resist pollutants. The hydrophobic end is exposed on the membrane surface, thereby simplifying the preparation process of the composite membrane and giving the composite membrane anti-pollution properties through a one-step preparation.

[0004] The technical solution adopted by the present invention is:

[0005] A method for preparing an anti-pollution polyamide nanofiltration composite membrane based on a hydrothermal method comprises the following steps:

[0006] (1) adding polyphenol to a NaOH solution, stirring to dissolve, then adding polyethyleneimine, stirring continuously until the polyethyleneimine is dissolved to obtain a polyphenol-polyethyleneimine intermediate layer modification liquid, applying the polyphenol-polyethyleneimine intermediate layer modification liquid to the surface of a porous support base membrane for soaking modification, pouring out excess modification liquid after the modification is completed, and then washing with deionized water to remove the modification liquid remaining on the membrane surface and in the membrane pores, thereby obtaining an intermediate layer modified porous base membrane, which is recorded as a PSF membrane;

[0007] (2) fixing the PSF membrane prepared in step (1) on a plate frame, coating the membrane surface with an organic amine aqueous solution and allowing it to stand, then pouring out excess aqueous solution and blowing off water droplets on the surface with an air knife; then pouring an organic acid chloride oil phase solution on the membrane surface at a uniform speed to perform an interfacial polymerization reaction to form a polyamide layer, and after the reaction is completed, washing unreacted organic acid chloride monomers with an organic solvent to obtain a polyamide nanofiltration composite membrane, which is recorded as a TFC membrane;

[0008] (3) placing the TFC membrane prepared in step (2) in an aqueous solution of a fluorinated surfactant and heating it in a water bath at 50 to 80° C. to obtain a cross-linked, stable, anti-fouling nanofiltration composite membrane.

[0009] Furthermore, the polyphenol in step (1) is at least one of hydroquinone, catechol, resorcinol, hydroquinone, pyrogallol and pyrogallol.

[0010] Furthermore, in the step (1), the mass concentration of polyphenol in the polyphenol-polyethyleneimine intermediate layer modification liquid is 0.5-3%, and the mass concentration of polyethyleneimine is 1-5%; and the modification time of the polyphenol-polyethyleneimine intermediate layer in the step (1) is 1-10 minutes.

[0011] Furthermore, in the step (1), the porous supporting base membrane is one of a polysulfone ultrafiltration membrane, a polyethersulfone ultrafiltration membrane, a polyimide ultrafiltration membrane, a polyacrylonitrile ultrafiltration membrane, a polyethylene microfiltration membrane, and a polypropylene microfiltration membrane.

[0012] Furthermore, in the step (2), the organic amine aqueous solution is obtained by dissolving an organic amine in water, and the organic amine is at least one of piperazine, m-phenylenediamine, o-phenylenediamine, p-phenylenediamine, 2-methylpiperazine, 2,5-dimethylpiperazine, 2,6-dimethylpiperazine, 1,2-diaminocyclohexane, 1,4-diaminocyclohexane, ethylenediamine, N,N-bis(2-aminoethyl)ethylenediamine, diethylenetriamine or polyethyleneimine;

[0013] The organic acid chloride oil phase solution in step (2) is obtained by dissolving an organic acid chloride in an organic solvent, wherein the organic acid chloride is at least one of trimesoyl chloride, terephthaloyl chloride, phthaloyl chloride, pyromellitoyl chloride, cyclohexanetricarboxylic acid chloride, cyclobutanetetracarboxylic acid chloride, cyclopentanetetracarboxylic acid chloride, malonyl chloride, glutaryl chloride and fumaroyl chloride; and the organic solvent is at least one of n-hexane, cyclohexane, n-heptane, toluene, benzene, isopar G, isopar E, isopar H, isopar L or isopar M.

[0014] Furthermore, in the process of washing the unreacted organic acid chloride monomer with an organic solvent in step (2), the organic solvent used is at least one of n-hexane, cyclohexane, n-heptane, toluene, benzene, isopar G, isopar E, isopar H, isopar L or isopar M.

[0015] Furthermore, in the step (2), the mass concentration of the organic amine aqueous solution is 0.1-5%; the mass concentration of the organic acid chloride oil solution is 0.01-2%.

[0016] Furthermore, the polymerization reaction time in step (2) is 10 to 90 seconds.

[0017] Furthermore, the mass concentration of the fluorine-containing surfactant aqueous solution in step (3) is 0.1-1.0%.

[0018] Furthermore, the fluorinated surfactant in step (3) is at least one of FS-63, sodium perfluorononenyloxybenzenesulfonate OBS, perfluorohexylethyl iodide, F-8903, FS-61, FC-4430, FS-3000, FS-3100, FS-8500, and FS-30.

[0019] Furthermore, in step (3), the water bath heating time is 0.5 to 5 minutes.

[0020] The beneficial effects of the present invention are:

[0021] The present invention provides a method for preparing an anti-pollution polyamide nanofiltration composite membrane based on a hydrothermal method, and proposes a hydrothermal crosslinking method for preparing an anti-pollution polyamide nanofiltration composite membrane. Compared with a multiple grafting method, the preparation process of the method is simple. During the hydrothermal crosslinking process, the hydrophilic end of an added fluorinated surfactant penetrates into the membrane pores, and a hydration layer is constructed on the membrane surface to resist pollutants. The hydrophobic end is exposed on the membrane surface, and a low surface energy micro-region is constructed to release pollutants, thereby weakening the interaction between the membrane surface and pollutants, and promoting the release of pollutants on the membrane surface, so that the composite membrane has excellent ability to resist and release pollutants. Moreover, the preparation process of the present invention is simple and easy to scale up, and has good industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1The flowchart of the preparation of the anti-pollution nanofiltration composite membrane prepared by the present invention;

[0024] Figure 2 The fluorine element distribution diagram, surface morphology SEM diagram and cross-sectional morphology SEM diagram of the anti-pollution nanofiltration composite membrane of Examples 1 and 3 of the present invention;

[0025] Figure 3 The water-oil contact angle, i.e., the surface energy, of the composite films of Examples 1-4 and Comparative Example 1 of the present invention;

[0026] Figure 4 The normalized flux and anti-pollution performance index changes of the composite membranes of Example 1 of the present invention and Comparative Example 1 during the filtration of pump oil emulsion;

[0027] Figure 5 are the normalized flux and flux reduction rate in the gypsum scaling experiment of the composite membranes of Example 1 of the present invention and Comparative Example 1;

[0028] Figure 6 This is a comparison chart of the separation selectivity test of the composite membrane of Example 1 of the present invention, Comparative Example 1 and the commercial membrane NF270 for monovalent / divalent anions. DETAILED DESCRIPTION

[0029] The present invention provides a method for preparing an anti-pollution polyamide nanofiltration composite membrane based on a hydrothermal method. In order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0030] The present invention is described in detail below with reference to the accompanying drawings.

[0031] Example 1

[0032] like Figure 1 As shown, this embodiment provides a method for preparing an anti-pollution polyamide nanofiltration composite membrane based on a hydrothermal method, comprising the steps of:

[0033] (1) Add 1g of Noria to 100mL of 0.25mol·L -1 After stirring and dissolving in a NaOH solution, 3 g of polyethyleneimine (PEI) was added. PEI reacted with Noria to form a Schiff base reaction. After continuous stirring, the polyethyleneimine was dissolved to obtain a polyphenol-polyethyleneimine intermediate layer modification liquid. The polyphenol-polyethyleneimine intermediate layer modification liquid was applied to the rinsed polysulfone-based membrane surface for soaking modification. The modification time was 7 min. After the modification was completed, the excess modification liquid was poured out, and then the membrane was fully washed with deionized water to remove the modification liquid remaining on the membrane surface and in the membrane pores, thereby obtaining an intermediate layer modified porous base membrane, which was recorded as N-PSF membrane.

[0034] (2) The PSF membrane prepared in step (1) is fixed on a plate frame, 20 mL of 1 wt% piperazine (PIP) aqueous solution is coated on the membrane surface and allowed to stand for 5 min, then the excess aqueous solution is poured out and the water droplets on the surface are blown away by a wind knife; then 10 mL of 1.0 wt% trimesoyl chloride (TMC) n-hexane oil phase solution is uniformly poured on the membrane surface for polymerization reaction to form a polyamide layer, and after reacting for 30 s, unreacted trimesoyl chloride is rinsed with n-hexane to obtain a polyamide nanofiltration composite membrane, which is recorded as an N-TFC membrane;

[0035] (3) The TFC membrane prepared in step (2) was placed in a 0.2 wt % FS-63 aqueous solution and heated in a water bath at 60° C. for 2 min to obtain a cross-linked, stable, anti-fouling nanofiltration composite membrane, which was recorded as N-TFC-FS63 membrane.

[0036] Example 2

[0037] The difference between Example 2 and Example 1 is that in this example, the concentration of the FS-63 aqueous solution is 0.4 wt %.

[0038] Example 3

[0039] The difference between Example 3 and Example 1 is that in this example, the concentration of the FS-63 aqueous solution is 0.6 wt %.

[0040] Example 4

[0041] The difference between Example 4 and Example 1 is that in this example, the concentration of the FS-63 aqueous solution is 0.8 wt %.

[0042] Example 5

[0043] The difference between Example 5 and Example 1 is that in this example, the concentration of the FS-63 aqueous solution is 1.0 wt %.

[0044] Example 6

[0045] The difference between Example 6 and Example 1 is that in this example, the water bath heating time is 1 min.

[0046] Example 7

[0047] The difference between Example 7 and Example 1 is that in this example, the water bath heating time is 4 minutes.

[0048] Example 8

[0049] This embodiment provides a method for preparing an anti-pollution polyamide nanofiltration composite membrane based on a hydrothermal method, comprising the steps of:

[0050] (1) Add 0.5 g of catechol and resorcinol to 100 mL of 0.5 mol·L-1 After stirring and dissolving in a NaOH solution, 1 g of polyethyleneimine (PEI) was added. PEI reacted with Noria to form a Schiff base reaction. After continuous stirring, the polyethyleneimine was dissolved to obtain a polyphenol-polyethyleneimine intermediate layer modification liquid. The polyphenol-polyethyleneimine intermediate layer modification liquid was applied to the surface of the rinsed polyethersulfone base membrane for soaking modification. The modification time was 1 min. After the modification was completed, the excess modification liquid was poured out, and then the membrane was fully washed with deionized water to remove the modification liquid remaining on the membrane surface and in the membrane pores, thereby obtaining an intermediate layer modified porous base membrane, which was recorded as a PSF membrane.

[0051] (2) The PSF membrane prepared in step (1) is fixed on a plate frame, and a 0.1 wt% aqueous solution of 2-methylpiperazine and 2,5-dimethylpiperazine is coated on the membrane surface and allowed to stand for 5 minutes, after which the excess aqueous solution is poured out and water droplets on the surface are blown off with an air knife; then a 0.05 wt% cyclohexane oil phase solution of terephthaloyl chloride is uniformly poured on the membrane surface for polymerization reaction to form a polyamide layer, and after reacting for 90 seconds, unreacted trimesoyl chloride is washed with cyclohexane to obtain a polyamide nanofiltration composite membrane, which is recorded as a TFC membrane;

[0052] (3) The TFC membrane prepared in step (2) was placed in a 0.2 wt % FS-61 aqueous solution and heated in a water bath at 80° C. for 0.5 min to obtain a cross-linked, stable, anti-fouling nanofiltration composite membrane, which was recorded as TFC-FS61 membrane.

[0053] The test showed that the flux was 16.8 L·m -2 ·h -1 bar -1 , the retention rate is 93.5%.

[0054] Comparative Example 1

[0055] This comparative example provides a method for preparing a polyamide nanofiltration composite membrane, comprising the steps of:

[0056] (1) Add 1g of Noria to 100mL of 0.25mol·L -1 After stirring and dissolving in a NaOH solution, 3 g of polyethyleneimine (PEI) was added. PEI reacted with Noria to form a Schiff base reaction. After continuous stirring, the polyethyleneimine was dissolved to obtain a polyphenol-polyethyleneimine intermediate layer modification liquid. The polyphenol-polyethyleneimine intermediate layer modification liquid was applied to the rinsed polysulfone-based membrane surface for soaking modification. The modification time was 7 min. After the modification was completed, the excess modification liquid was poured out, and then the membrane was fully washed with deionized water to remove the modification liquid remaining on the membrane surface and in the membrane pores, thereby obtaining an intermediate layer modified porous base membrane, which was recorded as N-PSF membrane.

[0057] (2) The PSF membrane prepared in step (1) is fixed on a plate frame, 20 mL of 1 wt% piperazine (PIP) aqueous solution is coated on the membrane surface and allowed to stand for 5 min, then the excess aqueous solution is poured out and the water droplets on the surface are blown away by a wind knife; then 10 mL of 1.0 wt% trimesoyl chloride (TMC) n-hexane oil phase solution is uniformly poured on the membrane surface for polymerization reaction to form a polyamide layer, and after reacting for 30 s, the unreacted trimesoyl chloride is rinsed with n-hexane to obtain a polyamide nanofiltration composite membrane;

[0058] (3) The polyamide nanofiltration composite membrane prepared in step (2) was placed in an oven at 60° C. for heat treatment for 2 min to obtain a cross-linked and stable polyamide nanofiltration composite membrane, which was recorded as N-TFC membrane.

[0059] The performance tests of the nanofiltration composite membranes prepared in the above Examples 1-7 and Comparative Examples 1 and 2 are shown in Table 1 below. Test conditions: The separation performance of the composite membrane was evaluated by using a Na2SO4 solution. First, the composite membrane was pre-pressed at 10 bar for 1 h at 25°C to reach a stable state, and then the separation performance test was performed. The permeate was collected and weighed to calculate the flux, and its conductivity was tested to calculate its retention rate.

[0060] Table 1

[0061]

[0062] The performance of the anti-pollution nanofiltration composite membranes of Examples 1-7 and Comparative Example 1 was compared. The flux and retention rate of the anti-pollution nanofiltration composite membranes obtained in Examples 1-6 were significantly improved, and Example 7 had the highest retention rate, but the flux decreased.

[0063] The anti-pollution composite nanofiltration membranes of Examples 1-4 and the composite nanofiltration membrane of Comparative Example 1 were tested as follows to analyze the reasons for the performance differences between the two and test their anti-pollution performance.

[0064] (I) Surface chemical properties of composite membranes

[0065] The chemical composition of the anti-pollution nanofiltration composite membranes of Examples 1-4 and the nanofiltration composite membrane of Comparative Example 1 was detected by XPS spectroscopy to study the changes in the chemical composition and structure of the composite membrane surface, as shown in Table 2 for the surface chemical composition of the composite membranes of Examples 1-4 and Comparative Example 1. As can be seen from Table 2, as the concentration of FS-63 increases, the content of F element in the prepared composite membrane also gradually increases, indicating that FS-63 is effectively grafted to the surface of the composite membrane.

[0066] Table 2

[0067]

[0068] (II) Surface morphology and cross-sectional morphology of composite membranes

[0069] The surface morphology and cross-sectional morphology of the anti-pollution nanofiltration composite membranes of Examples 1 and 3 were tested. Figure 2 As shown. Among them, Figure 2 (a1) and (a2) are EDX mapping images of the composite membranes of Example 1 (0.2 wt%) and Example 3 (0.6 wt%), respectively. The changes of element F in the separation layer of TFC-FS63 were analyzed using EDX mapping images. The yellow spots based on the black background represent the distribution of element F in the separation layer. Figure 2 It can be seen from (a1) and (a2) that compared with the TFC-FS63 membrane with a FS-63 concentration of 0.2wt%, the content of F element in the 0.6wt% membrane is significantly increased, and the fluorine element is more dense on the surface, which verifies that FS-63 is successfully exposed on the membrane surface, which is consistent with the results of XPS analysis. Figure 2 It can also be seen from (a1) and (a2) that the F element is evenly distributed on the surface of the composite membrane, indicating that FS-63 is evenly grafted onto the surface of the composite membrane. Figure 2 (b1) and (b2) are the surface SEM images of the composite membranes of Example 1 (0.2wt%) and Example 3 (0.6wt%). It can be seen from the SEM surface images that all membrane samples show a typical amide membrane particle nodular structure formed by the condensation reaction of PIP and TMC, and as the concentration of FS-63 increases, the particle nodular structure becomes smaller and denser, and the granular characteristics become more prominent. Figure 2 (c1) and (c2) are cross-sectional SEM images of the composite membranes of Example 1 (0.2wt%) and Example 3 (0.6wt%). It can be seen from the cross-sectional SEM images that the composite membrane with a higher FS-63 concentration is slightly thicker than that with a lower FS-63 concentration, and the thickness variation is relatively small. In the case of a small thickness variation, a rougher surface morphology is achieved, which helps to improve the water permeability performance.

[0070] (III) Surface wetting properties and surface energy of composite membranes

[0071] The surface wettability and surface energy of the composite films of Examples 1-4 and Comparative Example 1 were tested. Figure 3 As shown. Among them, Figure 3(a) is the water-oil contact angle of the composite membranes of Examples 1-4 and Comparative Example 1, from which it can be seen that: compared with Comparative Example 1, the composite membrane grafted with FS-63 has good hydrophilicity. By analyzing the change in the oil contact angle, the oil contact angle of FS-63 before grafting is 59°, and the surface is oleophilic, which easily attracts pollutants to adhere to the surface of the composite membrane. After FS-63 grafting, the oil contact angle gradually increases with the increase of FS-63 concentration, and the surface becomes oleophobic. When the grafting concentration is 0.6wt%, the oil contact angle reaches 105°, that is, the TFC-FS63 composite membrane has a hydrophilic and oleophobic surface. This is because the electronegativity of fluorine (3.98) is the highest among all chemical elements. For example, the bond energy of the carbon-fluorine bond (486kJ / mol) in carbon tetrafluoride is higher than that of the carbon-hydrogen bond (414kJ / mol) in methane, so the electric dipole moment of the CF bond is smaller than that of the CH bond. Compared with hydrocarbon chains, the intermolecular force of the fluorocarbon chain is weaker, and the end containing the fluorocarbon group is more likely to move from the water phase to the surface of the aqueous solution. The carbon-fluorine chain is oleophobic, which makes the composite membrane surface oleophobic. That is, for the TFC-FS63 composite membrane, a hydrophilic and oleophobic surface is formed, which is conducive to anti-pollution.

[0072] The surface energy (γ SV ),like Figure 3 (b) As shown in the figure, the surface energy (γ SV ) from 71.8 mJ·m -2 Reduced to 51.9 mJ·m -2 ; The introduction of FS63 also makes the dispersion component (γ d SV ) dropped significantly from 38.1mJ·m -2 Reduced to 6.4 mJ·m -2 This is because the intermolecular forces between fluorocarbons and hydrocarbon groups are weak, which reduces the interaction between the composite membrane surface and pollutants; in addition, the polar component (γ P SV ) from 33.6mJ·m -2 Increased to 51.0 mJ·m -2 The increase in polar components indicates that the interaction between the composite membrane and water molecules increases, which is also the reason why the water flux of the composite membrane increases with the increase of FS63 concentration. That is, the composite membrane prepared by hydrothermal cross-linking grafting FS63 has the ability to resist and release pollutants.

[0073] (IV) Anti-pollution performance

[0074] In addition, the anti-pollution performance tests were performed on the anti-pollution nanofiltration composite membranes of Example 1 and Comparative Example 1, including anti-organic pollutant tests and anti-inorganic pollutant tests.

[0075] For the anti-organic pollutant test, pump oil (100 ppm) was selected as a model pollutant for anti-pollution performance test. The test conditions were as follows: the membrane was pre-pressed with deionized water at a pressure of 4 bar for 2 hours to achieve a stable state. On this basis, the pure water flux (J w0 ), then the pump oil contaminant solution was added for testing, and the water flux (J) was measured every 1 hour during the test. p ); After the pollution experiment was completed, deionized water was used for three times at low pressure and high cross-flow velocity, each time for about 15 minutes to remove the reversible deposition and adsorbed pollutants on the membrane surface, and finally the pure water flux of the composite membrane after cleaning was measured (J w ).

[0076] The normalized flux during the test was monitored as a function of working time to study the anti-fouling effect of the membrane. Figure 4 As shown, Figure 4 (a) is the normalized flux of the composite membranes of Example 1 (N-TFC-FS63) and Comparative Example 1 (N-TFC) during the filtration of pump oil emulsion, Figure 4 (b) is the anti-pollution performance index of the composite membrane of Example 1 and Comparative Example 1 during the filtration of the pump oil emulsion, wherein FRR is the flux recovery rate, Rt is the flux reduction rate, DRr is the reversible flux reduction rate, and DRir is the irreversible flux reduction rate, and the calculation formulas are:

[0077]

[0078] In the formula, J w0 is the initial pure water flux, L·m -2 ·h -1 bar -1 ; J w is the pure water flux after cleaning, L·m -2 ·h -1 bar -1 ; J p is the stable permeation flux of the composite membrane in the fouling stage, L·m -2 ·h -1 bar -1 .

[0079] pass Figure 4 (a) It can be seen that the flux attenuation rate of Example 1 (N-TFC-FS63) is much smaller than that of the comparative example 1 (N-TFC), indicating that it has a better antifouling performance. The reason is that the hydrophilic end of the surfactant FS-63 can form a hydration layer on the surface of the composite membrane, and the hydration layer is conducive to increasing the Gibbs free energy of pollutants during the deposition process, thereby inhibiting the adhesion of pollutants on the membrane surface. In addition, by Figure 4 (b) It can be seen that the flux recovery rate of Example 1 (N-TFC-FS63) is significantly higher than that of Comparative Example 1 (N-TFC), and the reversible flux decline rate is reduced. This is because the grafting of FS-63 places the fluorine-containing end on the membrane surface, and the constructed low surface energy micro-region is conducive to the release of pollutants. In addition, from the perspective of the reversible flux decline rate and the irreversible flux decline rate, the introduction of FS-63 can simultaneously reduce the reversible pollution and irreversible pollution of the composite membrane, and the anti-pollution effect is greatly improved.

[0080] For the test of resistance to inorganic pollutants, a cross-flow test device was used to conduct a gypsum scaling experiment. The test conditions were: the test solution contained 2840 mg / L (30 mM) sodium sulfate and 2220 mg / L (30 mM) calcium chloride, the pH value was adjusted to 6, and the membrane was pre-pressed for 1 hour to reach a stable state, and then the water flux was measured every 0.5 hours for 14 hours. The test results are as follows: Figure 5 As shown, Figure 5 (a) is the normalized flux in the gypsum scaling test of the composite membranes of Example 1 (N-TFC-FS63) and Comparative Example 1 (N-TFC), Figure 5 (b) is the flux decrease rate. Figure 5 It can be seen that the normalized flux of the composite membranes of Example 1 (N-TFC-FS63) and Comparative Example 1 (N-TFC) begins to decrease slowly and then decreases rapidly. After 13 hours of the experiment until the end of the experiment, the flux attenuation rate of the membrane of Example 1 (N-TFC-FS63) is lower than that of the membrane of Comparative Example 1 (N-TFC).

[0081] Through the test of resistance to organic and inorganic pollutants, the anti-pollution performance of the composite membrane of Example 1 (N-TFC-FS63) is significantly better than that of Comparative Example 1 (N-TFC).

[0082] (V) Anti-pollution test on actual refining wastewater

[0083] The separation selectivity of the above-mentioned Example 1, Comparative Example 1 and the commercial membrane NF270 for monovalent / divalent anions was tested using actual refinery wastewater. The test results are shown in Table 3 and Figure 6 As shown, Table 3 is the wastewater component table before and after composite membrane treatment, Figure 6 This is a comparison chart of the molecular selectivity of the composite membrane for monovalent / divalent anions.

[0084] Table 3

[0085] Wastewater components NF270 N-TFC N-TFC-FS63 <![CDATA[Original solution conductivity / (μs·cm -1 )]]> 3963 3963 3963 <![CDATA[Permeate conductivity / (μs·cm -1 )]]> 2073 2129 1863 <![CDATA[Original solution COD / (mg·L -1 )]]> 68 68 68 <![CDATA[COD of permeate / (mg·L -1 )]]> 59 53 42 <![CDATA[Stock solution Cl - Concentration / (mg·L -1 )]]> 754.6 754.6 754.6 <![CDATA[Concentration of Cl- in permeate / (mg·L -1 )]]> 562.7 589.3 587.0 <![CDATA[Stock solution SO4 2- Concentration / (mg·L -1 )]]> 618.2 618.2 618.2 Permeate SO4 2- Concentration / (mg·L -1 )]]> 9.1 9.0 5.9 pH of stock solution 7.9 7.9 7.9 pH of permeate 7.8 7.6 8.1

[0086] It can be seen from Table 3 that the quality of the treated wastewater has improved and meets the wastewater quality reuse standard (GB / T41016-2021), but the water quality of the N-TFC-FS63 membrane is better; in addition, Figure 6 It can be seen that the composite membrane of Example 1 (N-TFC-FS63) has a higher SO4 2- Retention rate, lower Cl - Retention rate, and Cl - / SO4 2- The ion selectivity is very high, which means that the composite membrane of the embodiment exhibits good characteristics in terms of chloride ion and sulfate ion selectivity. Such high ion selectivity is conducive to maintaining a high rejection rate for multivalent ions while allowing monovalent ions to pass through the membrane.

[0087] It should be noted that some parts not described in the present invention can be implemented by adopting or drawing on existing technologies.

[0088] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.

Claims

1. A method for preparing anti-pollution polyamide nanofiltration composite membrane based on hydrothermal method, It is characterized in that Includes steps: (1) adding polyphenol to a NaOH solution, stirring to dissolve, then adding polyethyleneimine, stirring continuously until the polyethyleneimine is dissolved to obtain a polyphenol-polyethyleneimine intermediate layer modification liquid, applying the polyphenol-polyethyleneimine intermediate layer modification liquid to the surface of a porous support base membrane for soaking modification, pouring out excess modification liquid after the modification is completed, and then washing with deionized water to remove the modification liquid remaining on the membrane surface and in the membrane pores, thereby obtaining an intermediate layer modified porous base membrane, which is recorded as a PSF membrane; (2) fixing the PSF membrane prepared in step (1) on a plate frame, coating the membrane surface with an organic amine aqueous solution and allowing it to stand, then pouring out excess aqueous solution and blowing off water droplets on the surface with an air knife; then pouring an organic acid chloride oil phase solution on the membrane surface at a uniform speed to perform an interfacial polymerization reaction to form a polyamide layer, and after the reaction is completed, washing unreacted organic acid chloride monomers with an organic solvent to obtain a polyamide nanofiltration composite membrane, which is recorded as a TFC membrane; (3) placing the TFC membrane prepared in step (2) in an aqueous solution of a fluorinated surfactant and heating it in a water bath at 50 to 80° C. to obtain a cross-linked, stable, anti-fouling nanofiltration composite membrane.

2. A method for preparing an anti-pollution polyamide nanofiltration composite membrane based on a hydrothermal method according to claim 1, It is characterized in that In the step (1), the polyphenol is at least one of hydroquinone, catechol, resorcinol, hydroquinone, pyrogallol and pyrogallol.

3. A method for preparing an anti-pollution polyamide nanofiltration composite membrane based on a hydrothermal method according to claim 1, It is characterized in that In the step (1), the mass concentration of polyphenol in the polyphenol-polyethyleneimine intermediate layer modification liquid is 0.5-3%, and the mass concentration of polyethyleneimine is 1-5%; the modification time of the polyphenol-polyethyleneimine intermediate layer in the step (1) is 1-10 minutes.

4. The method for preparing an anti-pollution polyamide nanofiltration composite membrane based on a hydrothermal method according to claim 1, It is characterized in that The porous supporting base membrane in step (1) is one of polysulfone ultrafiltration membrane, polyethersulfone ultrafiltration membrane, polyimide ultrafiltration membrane, polyacrylonitrile ultrafiltration membrane, polyethylene microfiltration membrane and polypropylene microfiltration membrane.

5. The method for preparing an anti-pollution polyamide nanofiltration composite membrane based on a hydrothermal method according to claim 1, It is characterized in that The organic amine aqueous phase solution in step (2) is obtained by dissolving an organic amine in water, wherein the organic amine is at least one of piperazine, m-phenylenediamine, para-phenylenediamine, 2-methylpiperazine, 2,5-dimethylpiperazine, 2,6-dimethylpiperazine, 1,2-diaminocyclohexane, 1,4-diaminocyclohexane, ethylenediamine, N,N-bis(2-aminoethyl)ethylenediamine, diethylenetriamine or polyethyleneimine; The organic acid chloride oil phase solution in step (2) is obtained by dissolving an organic acid chloride in an organic solvent, wherein the organic acid chloride is at least one of trimesoyl chloride, terephthaloyl chloride, phthaloyl chloride, pyromellitoyl chloride, cyclohexanetricarboxylic acid chloride, cyclobutanetetracarboxylic acid chloride, cyclopentanetetracarboxylic acid chloride, malonyl chloride, glutaryl chloride and fumaroyl chloride; and the organic solvent is at least one of n-hexane, cyclohexane, n-heptane, toluene, benzene, isopar G, isopar E, isopar H, isopar L or isopar M.

6. The method for preparing an anti-pollution polyamide nanofiltration composite membrane based on a hydrothermal method according to claim 1, It is characterized in that The mass concentration of the organic amine aqueous solution in step (2) is 0.1-5%; the mass concentration of the organic acyl chloride oil phase solution is 0.01-2%.

7. A method for preparing an anti-pollution polyamide nanofiltration composite membrane based on a hydrothermal method according to claim 1, It is characterized in that The polymerization reaction time in step (2) is 10 to 90 seconds.

8. The method for preparing an anti-pollution polyamide nanofiltration composite membrane based on a hydrothermal method according to claim 1, It is characterized in that The mass concentration of the fluorine-containing surfactant aqueous solution in step (3) is 0.1-1.0%.

9. The method for preparing an anti-pollution polyamide nanofiltration composite membrane based on a hydrothermal method according to claim 1, It is characterized in that The fluorinated surfactant in step (3) is at least one of FS-63, sodium perfluorononenyloxybenzenesulfonate OBS, perfluorohexylethyl iodide, F-8903, FS-61, FC-4430, FS-3000, FS-3100, FS-8500, and FS-30.

10. The method for preparing an anti-pollution polyamide nanofiltration composite membrane based on a hydrothermal method according to claim 1, It is characterized in that The water bath heating time in step (3) is 0.5 to 5 minutes.

Citation Information

Patent Citations