Surface-modified composite nanofiltration membrane as well as preparation method and application thereof

By forming an interface polymerization layer on the nanofiltration membrane, tannin acid reacts with residual acid chloride, the problem of weakening connection of the surface modified layer of the nanofiltration membrane and increasing water mass transfer resistance is solved, and efficient anti-pollution performance and Flux recovery rate.

CN118904094APending Publication Date: 2024-11-08TIANJIN MOTIMO MEMBRANE TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411039742.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing surface modification method of nanofiltration membrane, the physical connection between the coating layer and the membrane surface is weak, which is easy to fall off during high pressure use, affecting service life. At the same time, the grafting method increases the mass transfer resistance of water or reduces desalting. Rate.

Method used

Using a surface-modified composite nanofiltration membrane preparation method, the reaction is formed by passing the aqueous solution, oily solution and tanninic acid solution on the base membrane to form an interfacial polymerization layer, and the tanninic acid reacts with residual acid chloride. , forming a negatively charged graft layer to improve the hydrophilicity and anti-pollution properties of the film.

Benefits of technology

Achieve high anti-pollution performance, with a minimum flux decay rate of 5.0%, a steady-state flux of up to 10.0L/(m2.h.bar), a maximum flux recovery rate of 98%, and a pure Water flux and desalination rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904094A_ABST
    Figure CN118904094A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of separation, and particularly relates to a surface-modified composite nanofiltration membrane and a preparation method and application thereof.The preparation method comprises the following steps that 1, an aqueous phase solution is introduced into a tube pass of a base membrane from bottom to top, and then a membrane assembly is purged through N2 to remove the redundant aqueous phase solution; 2) introducing an oil phase solution from bottom to top, and flushing the surface of the membrane with normal hexane to remove the redundant oil phase solution; and 3) introducing a tannic acid solution from bottom to top for reaction to obtain the surface-modified composite nanofiltration membrane. According to the surface-modified composite nanofiltration membrane, an interface polymerization layer is formed on the surface of the base membrane, a grafting layer of the surface-modified composite nanofiltration membrane is introduced through esterification reaction of tannic acid and residual acyl chloride on the surface of the nanofiltration membrane, and the surface of the prepared modified membrane is negatively charged and has high hydrophilicity. Therefore, compared with a nanofiltration original membrane, the prepared grafted membrane is slightly improved in pure water flux and sodium sulfate desalination rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of separation, and in particular relates to a surface-modified composite nanofiltration membrane and a preparation method and application thereof. Background Art

[0002] Membrane separation technology is widely used in water treatment, material separation, purification, concentration and other fields. At present, membrane technology has gradually replaced traditional water treatment processes due to its energy saving, high efficiency, simple process and easy operation.

[0003] In terms of improving the pollution resistance of nanofiltration membranes, the research and development focus of existing technologies is on developing a protective layer for the nanofiltration membrane, which mainly includes surface coating and surface grafting.

[0004] Since the surface coating method utilizes the effects of adsorption and interfacial cross-linking on the surface of the nanofiltration membrane, the modifier is attached to the surface of the nanofiltration membrane, and the membrane performance is improved by the formed coating layer. The surface coating method is a relatively simple modification method that can effectively improve the surface state of the nanofiltration membrane. For example, the coating layer is formed by soaking the surface of the commercial nanofiltration membrane with a solution of ferric ion tannic acid (FeIII-TA), and the anti-pollution performance is improved. However, in actual use, due to the relatively weak physical connection and adhesion between the coating and the membrane surface, the use of high pressure outside the membrane often causes the surface coating functional layer to form defects or even fall off, thereby affecting the use of the nanofiltration membrane and greatly reducing the service life of the nanofiltration membrane. Compared with surface coating, surface grafting has stronger bonding force and longer service life.

[0005] The surface grafting method of nanofiltration membranes is mostly to react with unhydrolyzed acyl chloride or carboxylic acid formed after hydrolysis on the surface of the nanofiltration membrane to form a stable amide bond, so that the grafted layer is firmly attached to the surface of the nanofiltration membrane. However, surface grafting often increases the mass transfer resistance of water, reduces the pure water flux, or changes the surface state of the membrane to reduce the desalination rate of monovalent / polyvalent salts. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a surface-modified composite nanofiltration membrane and a preparation method thereof.

[0007] To achieve the above object, the technical solution adopted by the present invention is:

[0008] A method for preparing a surface-modified composite nanofiltration membrane comprises the following steps: 1) passing an aqueous solution through a tube of a base membrane, preferably for 3-10 minutes, and then blowing N2 through the membrane assembly to remove excess aqueous solution; 2) then passing an oily solution through, preferably for 60-100 seconds, and washing the surface of the base membrane with n-hexane to remove excess oily solution; 3) passing a tannic acid solution through a reaction to obtain a surface-modified composite nanofiltration membrane.

[0009] The preparation method of the tannic acid solution adopts the following steps: adjusting the pH value of a tannic acid aqueous solution with a mass concentration of 0.01-2.0% to 7 using sodium hydroxide to obtain the tannic acid solution.

[0010] The concentration of the tannic acid aqueous solution is 0.05-0.15%, more preferably 0.15%.

[0011] The aqueous phase solution is a polyamine compound aqueous solution;

[0012] Preferably, the polyamine compound is one of piperazine, m-phenylenediamine, or p-phenylenediamine; preferably, the mass concentration of the polyamine compound is 0.05%-5.0%, preferably 1%.

[0013] The oil phase solution is a solution of multifunctional acyl chloride;

[0014] The multifunctional acyl chloride is one of trimesoyl chloride, adipoyl chloride and sebacoyl chloride; the solvent of the oil phase solution is one of n-hexane, cyclohexane and heptane;

[0015] Preferably, the mass concentration of the multifunctional acyl chloride is 0.05%-3.0%, preferably 0.15%.

[0016] The base membrane is one of polysulfone, polyvinylidene fluoride or polyvinyl chloride, and is in the shape of a hollow fiber or a flat plate.

[0017] The reaction time in step 3) is 3-9 min.

[0018] The present invention also includes a surface-modified composite nanofiltration membrane obtained by the preparation method.

[0019] The present invention also includes an application of the surface-modified composite nanofiltration membrane, which is applied to material separation, purification, or concentration. Compared with the prior art, the present invention has the following beneficial effects:

[0020] The surface-modified composite nanofiltration membrane of the present application forms an interfacial polymerization layer on the surface of the base membrane, and its grafted layer is introduced by esterification reaction between tannic acid and residual acyl chloride on the surface of the nanofiltration membrane. The surface of the prepared modified membrane is negatively charged and has a high hydrophilicity.

[0021] The anti-pollution performance test results of humic acid solution show that the flux attenuation rate can be as low as 5.0%; the final steady-state flux can reach up to 10.0L / (m2.h.bar) or more. Through simple deionized water washing, the flux recovery rate can reach up to 98%, showing excellent anti-pollution performance.

[0022] At the same time, since the conditions of interfacial polymerization were regulated during the preparation process of the grafted membrane, an asymmetric separation layer was formed, namely a loose interfacial polymerization layer and a dense grafted layer. Therefore, the pure water flux and sodium sulfate rejection rate of the prepared grafted membrane were slightly improved compared with the original nanofiltration membrane. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 Schematic diagram of the preparation process of the surface-modified composite nanofiltration membrane of the present invention;

[0024] Figure 2 The flux attenuation curves of the composite membranes to humic acid obtained in different embodiments of the present invention;

[0025] Figure 3 The cleaning recovery curves of Example 5 of the present invention and Comparative Example 1 are shown. DETAILED DESCRIPTION

[0026] In order to make those skilled in the art better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and the best embodiment. Unless otherwise specified in this application, concentrations are all mass concentrations.

[0027] A method for preparing a surface-modified composite nanofiltration membrane comprises the following steps: 1) introducing an aqueous solution into a tube of a base membrane, and then blowing N2 through the membrane assembly to remove excess aqueous solution; 2) then introducing an oily solution, and washing the surface of the base membrane with n-hexane to remove excess oily solution; and 3) introducing a tannic acid solution to react to obtain a surface-modified composite nanofiltration membrane.

[0028] The preparation method of the tannic acid solution adopts the following steps: adjusting the pH of a tannic acid aqueous solution with a mass concentration of 0.01-2.0% to 7 using sodium hydroxide, and the specific mass concentration of the tannic acid aqueous solution can be 0.01%, 0.05%, 0.1%, 0.15%, 0.5%, 1%, 2%. As a preferred form, the concentration of the tannic acid aqueous solution is 0.05-0.15%, more preferably 0.15%.

[0029] The aqueous phase solution is a polyamine compound aqueous solution;

[0030] The polyamine compound is one of piperazine, m-phenylenediamine, or p-phenylenediamine; preferably, the mass concentration of the polyamine compound is 0.05%-5.0%, specifically 0.05%, 0.1%, 0.15%, 0.5%, 1%, 2%, 5%, preferably 1%.

[0031] The oil phase solution is a solution of multifunctional acyl chloride; the multifunctional acyl chloride is one of trimesoyl chloride, adipoyl chloride and sebacyl chloride; the solvent of the oil phase solution is one of n-hexane, cyclohexane and heptane; the mass concentration of the multifunctional acyl chloride is 0.05%-3.0%, specifically 0.05%, 0.1%, 0.15%, 0.5%, 1%, 2% and 3%.

[0032] The base membrane is one of polysulfone, polyvinylidene fluoride or polyvinyl chloride, and is in the shape of a hollow fiber or a flat plate.

[0033] The reaction time in step 3) is 3-9 min, specifically 3 min, 6 min, 9 min.

[0034] The present invention also includes a surface-modified composite nanofiltration membrane obtained by the preparation method.

[0035] The present invention also includes an application of the surface-modified composite nanofiltration membrane for material separation, purification, or concentration.

[0036] The following is an illustrative description using preferred embodiments.

[0037] Example 1

[0038] Figure 1 A schematic diagram showing the preparation process of the surface-modified composite nanofiltration membrane of the present invention;

[0039] The preparation process of the surface-modified composite nanofiltration membrane specifically adopts the following steps: 1) Using a circulating pump, circulate the aqueous solution in the tube of the polyvinyl chloride-based membrane. In this embodiment, it is a 1.0% piperazine aqueous solution for 5 minutes, and then N2 purges the membrane assembly for 5 minutes to remove excess aqueous solution; 2) Then, the oil phase solution is passed. In this embodiment, it is a 0.15% hexane solution of trimesoyl chloride for 90 seconds, and the membrane surface is rinsed with 10mL of hexane to remove excess oil phase solution; 3) Then, a tannic acid solution is passed; react for 5 minutes. After the experiment, it is stored in deionized water and waits for the humic acid pollution resistance and separation performance test;

[0040] The tannic acid solution is prepared by the following steps: adjusting the pH of a tannic acid aqueous solution with a mass concentration of 0.01% to 7 using sodium hydroxide.

[0041] Example 2

[0042] The difference between Example 2 and Example 1 is that the mass concentration of the tannic acid aqueous solution is 0.03%, and the rest is the same as Example 1.

[0043] Example 3

[0044] The only difference between Example 3 and Example 1 is that the mass concentration of the tannic acid aqueous solution is 0.05%, and the rest is the same as Example 1.

[0045] Example 4

[0046] The only difference between Example 4 and Example 1 is that the mass concentration of the tannic acid aqueous solution is 0.1%, and the rest is the same as Example 1.

[0047] Example 5

[0048] The only difference between Example 5 and Example 1 is that the mass concentration of the tannic acid aqueous solution is 0.15%, and the rest is the same as Example 1.

[0049] Example 6

[0050] The only difference between Example 6 and Example 1 is that the mass concentration of the tannic acid aqueous solution is 0.3%, and the rest is the same as Example 1.

[0051] Example 7

[0052] The only difference between Example 7 and Example 1 is that the mass concentration of the tannic acid aqueous solution is 0.5%, and the rest is the same as Example 1.

[0053] Example 8

[0054] The only difference between Example 8 and Example 1 is that the mass concentration of the tannic acid aqueous solution is 1.0%, and the rest is the same as Example 1.

[0055] Example 9

[0056] The only difference between Example 8 and Example 1 is that the mass concentration of the tannic acid aqueous solution is 2.0% tannic acid solution, and the rest is the same as Example 1.

[0057] Comparative Example 1

[0058] The preparation process of the composite membrane specifically adopts the following steps: 1) passing an aqueous solution, a 1.0% piperazine aqueous solution, into the tube of the polyvinyl chloride-based membrane for 5 minutes, and then N2 purging the membrane assembly for 5 minutes to remove excess aqueous solution; 2) then passing an oily solution, which in this embodiment is a 0.15wt% hexane solution of trimesoyl chloride for 90 seconds, and rinsing the membrane surface with 10mL of hexane to remove excess oily solution; 3) then placing it in an oven at 50°C for heat treatment for 5 minutes.

[0059] Comparative Example 2

[0060] The preparation process of the composite membrane specifically adopts the following steps: 1) an aqueous solution, a 1.0% piperazine aqueous solution, is introduced into the tube of the polyvinyl chloride-based membrane for 5 minutes, and then N2 is purged into the membrane assembly for 5 minutes to remove excess aqueous solution; 2) an oily solution, in this embodiment, a 0.15wt% hexane solution of trimesoyl chloride is introduced for 90 seconds, and the membrane surface is rinsed with 10mL of hexane to remove excess oily solution.

[0061] Test method:

[0062] The membrane assembly was fixed on the cross-flow device, and the raw liquid passed through the membrane assembly under the internal pressure mode. First, pure water was pre-pressed at 0.30MPa for 1h, and then the pure water flux was tested by weighing method after an interval of 10min until the flux was stable. The pure water flux was recorded as J1; then the pure water was replaced with 200mg / L humic acid contaminated liquid and continued to run. The membrane flux was tested every 10min until the membrane flux was stable. The initial flux of filtering humic acid solution was recorded as J2, and the final steady-state flux was recorded as J3. It was washed with deionized water for 2h, and the pure water flux was tested, which was recorded as J4.

[0063] FDR (flux decay rate) = [(J1-J3) / J1] × 100%; the pure water flux in the table is J1.

[0064] The flux recovery rate is [(J1-J4) / J1]×100%; the flux recovery rates of Examples 3-5 can all reach more than 98%.

[0065] A 1 g / L Na2SO4 solution was prepared as the feed solution. The feed solution passed through the membrane assembly under the internal pressure mode with an operating pressure of 0.30 MPa. The conductivity of the output liquid was measured every 20 minutes and the desalination rate was calculated until the desalination rate was stable.

[0066] Table 1 shows the test results of different embodiments and comparative examples.

[0067] Table 1

[0068]

[0069]

[0070] Figure 2 The flux attenuation curves of humic acid obtained by the composite membranes of different embodiments of the present invention are shown in FIG. Figure 2 The results show that when the tannic acid with a mass concentration of 0.15wt% is used for modification, the attenuation rate of humic acid is the lowest, and the initial flux and steady-state flux of the humic acid solution are higher than those of the modified membranes with other concentrations. The membrane flux attenuation rate is the lowest, at 5.0%, and the steady-state flux is the highest, at 10.0L / (m2.h.bar).

[0071] Figure 3 The cleaning recovery curves of the preferred embodiment 5 of the present invention and the comparative example 1 are shown. The green curve represents the surface-modified composite nanofiltration membrane obtained in embodiment 5, and the red curve represents the composite membrane obtained in comparative example 1. Because the heat treatment process is omitted for the composite membrane in embodiment 5, and the grafting reaction is carried out based on this process, the prepared grafted modified membrane has an asymmetric separation layer, i.e., a loose polyamide skin layer and a relatively dense grafted layer, so the water flux of the modified membrane is higher than the pure water flux of the original polyamide nanofiltration membrane.

[0072] Compared with the original polyamide nanofiltration membrane (Comparative Example 1), the surface-modified composite nanofiltration membrane has stronger hydrophilicity and negative charge on the surface. Therefore, when filtering humic acid solution, the modified membrane has higher resistance to humic acid contamination and cleaning recoverability.

[0073] The surface-modified composite nanofiltration membrane of the present application forms an interfacial polymerization layer on the surface of the base membrane, and its grafted layer is introduced by esterification reaction between tannic acid and residual acyl chloride on the surface of the nanofiltration membrane. The surface of the prepared modified membrane is negatively charged and has a high hydrophilicity.

[0074] The anti-pollution performance test results of humic acid solution show that the flux attenuation rate can be as low as 5.0%; the final steady-state flux can reach up to 10.0L / (m2.h.bar). Through simple deionized water washing, the flux recovery rate can reach up to 98%, showing excellent anti-pollution performance.

[0075] At the same time, since the conditions of interfacial polymerization are regulated during the preparation of the grafted membrane, an asymmetric separation layer is formed, namely a loose interfacial polymerization layer and a dense grafted layer, so the prepared grafted membrane has a slightly improved pure water flux and sodium sulfate rejection rate compared to the original nanofiltration membrane. According to Example 5, at a pressure of 3 bar, the rejection rate of Na2SO4 is 98%, and the pure water flux is 10.1 L / (m2.h.bar).

[0076] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a surface-modified composite nanofiltration membrane, characterized in that: The method comprises the following steps: 1) introducing an aqueous solution into the tube of the base membrane, and then purging the membrane assembly with N2 to remove excess aqueous solution; 2) then passing the oil phase solution, and washing the surface of the base membrane with n-hexane to remove excess oil phase solution; 3) passing the tannic acid solution to react to obtain a surface-modified composite nanofiltration membrane.

2. The method for preparing a surface-modified composite nanofiltration membrane according to claim 1, characterized in that: The preparation method of the tannic acid solution adopts the following steps: adjusting the pH value of a tannic acid aqueous solution with a mass concentration of 0.01-2.0% to 7 using sodium hydroxide to obtain the tannic acid solution.

3. The method for preparing a surface-modified composite nanofiltration membrane according to claim 2, characterized in that: The concentration of the tannic acid aqueous solution is 0.05-0.15%, more preferably 0.15%.

4. The method for preparing a surface-modified composite nanofiltration membrane according to claim 1, characterized in that: The aqueous phase solution is an aqueous solution of a polyamine compound; Preferably, the polyamine compound is one of piperazine, m-phenylenediamine, or p-phenylenediamine; preferably, the mass concentration of the polyamine compound is 0.05%-5.0%; preferably 1%.

5. The method for preparing a surface-modified composite nanofiltration membrane according to claim 1, characterized in that: The oil phase solution is a solution of multifunctional acyl chloride; The multifunctional acyl chloride is one of trimesoyl chloride, adipoyl chloride and sebacoyl chloride; the solvent of the oil phase solution is one of n-hexane, cyclohexane and heptane; Preferably, the mass concentration of the multifunctional acyl chloride is 0.05%-3.0%, preferably 0.15%.

6. The method for preparing a surface-modified composite nanofiltration membrane according to claim 1, characterized in that: The base membrane is one of polysulfone, polyvinylidene fluoride or polyvinyl chloride, and is in the shape of a hollow fiber or a flat plate.

7. The method for preparing a surface-modified composite nanofiltration membrane according to claim 1, characterized in that: The reaction time in step 3) is 3-9 min.

8. A surface-modified composite nanofiltration membrane obtained by the preparation method according to any one of claims 1 to 7.

9. An application of the surface-modified composite nanofiltration membrane according to claim 8, characterized in that: Used for material separation, purification, or concentration.

Citation Information

Cited By

  • Preparation method of TA-modified aminated ZIF-90 polyamide reverse osmosis membrane

    CN120115031A

  • A preparation method of a ta-modified aminoated zif-90 polyamide reverse osmosis membrane

    CN120115031B