Wrinkled nanofiltration membrane for enhancing nano foaming based on low-temperature interfacial tension regulation and control and preparation method of wrinkled nanofiltration membrane
By using SDBS at low temperatures to enhance the nanofoaming effect, the bubble-like fold structure of the nanofiltration membrane is formed, which solves the problem of insufficient effective filtration area due to flat structure of the traditional nanofiltration membrane, and achieves the improvement of high water permeability and salt retention performance. , has the potential for industrial application.
Patent Information
- Application Number
- CN202411261450.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-08
AI Technical Summary
During the preparation process, traditional nanofiltration membranes are difficult to form sufficient nanobubbles due to the low interfacial reaction intensity, resulting in flat membrane structure, limiting the effective filtration area and water purification efficiency.
The nanofoaming effect is enhanced by using the surfactant SDBS at low temperature, reducing the interfacial tension, forming sufficient nanobubble to shape the PA layer, forming a nanofiltration membrane with a bubble-like fold structure, significantly increasing the specific surface area and water permeability.
It significantly improves water permeability while maintaining high salt retention performance, is low in cost and is easy to industrially apply.
Smart Images

Figure CN118904097A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of membrane separation, and in particular to a pleated nanofiltration membrane based on low-temperature interfacial tension regulation and enhanced nanofoaming and a preparation method thereof. Background Art
[0002] Wastewater treatment and recycling have become an important means to alleviate the global water crisis. With the increasing scarcity of water resources and increasingly stringent wastewater discharge standards, traditional treatment processes have been unable to meet the needs of deep wastewater treatment and recycling. Membrane separation technology occupies a dominant position in wastewater treatment and recycling. Nanofiltration membrane (NF) separation has nanoscale screening capabilities and controllable selectivity. It can efficiently remove small molecular pollutants and salts in water and is an important technology for achieving water pollution control and water resource regeneration.
[0003] Commercial NF / reverse osmosis (RO) membranes are generally thin-layer composite structures, consisting of a polyamide (PA) layer, a porous support layer, and a non-woven fabric. The PA layer is often formed by an interfacial polymerization (IP) reaction between water-phase monomers and oil-phase monomers on the support layer. During the preparation of the RO membrane, due to the violent reaction of the m-phenylenediamine monomer and the trimesoyl chloride (TMC) monomer, the interface temperature rises, causing the nanobubbles dissolved in the water to escape, thereby forming a rough peak-valley morphology, which ensures the effective area of water molecule transmission of the RO membrane. However, during the preparation of the NF membrane, the PA layer structure generated by the reaction of piperazine (PIP) and / TMC is relatively flat and does not have a peak-valley structure. This is because compared with the MPD / TMC system, the PIP / TMC system has a lower reaction intensity and it is difficult to produce a sufficient number of nanobubbles at the interface, so it is not easy to form a rough pleated structure, thereby limiting the effective filtration area of the membrane and seriously restricting the water purification efficiency of the NF technology. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a pleated nanofiltration membrane based on low-temperature interfacial tension regulation and enhanced nanofoaming and a preparation method thereof. Through the nanofoaming effect of SDBS and the characteristics of reducing interfacial tension, combined with lowering the temperature of the PIP solution to enhance gas solubility, sufficient nanobubbles are introduced at the IP interface for PA layer shaping to form a NF membrane with a bubble-like pleated structure, which significantly increases the specific surface area of the PA layer, thereby significantly improving the water permeability of the NF membrane. At the same time, since the PA layer has a high degree of cross-linking, the salt retention performance of the NF membrane will not be lost. The method is low-cost and easy to scale up in engineering, and has potential application prospects. The membrane significantly improves the water permeability while maintaining a high salt retention rate.
[0005] The first object of the present invention is to provide a method for preparing a pleated nanofiltration membrane based on low-temperature interfacial tension regulation and enhanced nanofoaming, comprising the following steps:
[0006] (1) mixing a surfactant solution and an amine monomer solution and dissolving them in water to obtain a surfactant / amine monomer aqueous solution;
[0007] (2) placing the surfactant / amine monomer aqueous solution obtained in step (1) in a low-temperature water bath to adjust the solubility of the bubbles;
[0008] (3) treating the base film in a surfactant / amine monomer aqueous solution and removing excess solution on the surface of the base film;
[0009] (4) treating the surface of the base membrane obtained in step (3) with trimesoyl chloride / n-hexane solution (TMC / n-hexane solution) for 30-90 seconds to react and form a PA layer, thereby obtaining the pleated nanofiltration membrane.
[0010] In the present invention, the surfactant (SDBS) has the functions of nano-foaming and reducing interfacial tension, and sufficient nano-bubbles can be formed at the PIP / TMC interface, which is helpful for shaping the PA layer. The gas solubility of the PIP solution is enhanced at low temperature, the number of nano-bubbles is further increased, and the encapsulation of nano-bubbles between the PA layer and the substrate is promoted to form a wrinkled structure.
[0011] In some embodiments of the present invention, in step (1), the surfactant is selected from sodium dodecylbenzene sulfonate and / or sodium dodecyl sulfate.
[0012] In some embodiments of the present invention, in step (1), the amine monomer is selected from piperazine.
[0013] In some embodiments of the present invention, in step (1), the concentration of the surfactant solution in the surfactant / amine monomer aqueous solution is 1-10 CMC (critical micelle concentration).
[0014] In some embodiments of the present invention, in step (1), the mass volume fraction of the amine monomer solution in the surfactant / amine monomer aqueous solution is 0.1-5.0 wt / v%.
[0015] In some embodiments of the present invention, in step (2), the temperature of the low-temperature water bath is set to 0-20°C, and the temperature is ensured to be stable at the set temperature, wherein the temperature fluctuation at 0°C does not exceed 0.3°C.
[0016] In some embodiments of the present invention, in step (3), the base membrane is selected from PVDF base membrane and / or polyethersulfone base membrane; and the treatment time is 1 to 5 minutes.
[0017] In some embodiments of the present invention, in step (4), the mass volume fraction of the trimesoyl chloride / n-hexane solution is 0.1-0.3 wt / v%.
[0018] In some embodiments of the present invention, step (4) further includes cleaning the pleated nanofiltration membrane with n-hexane and deionized water.
[0019] The second object of the present invention is to provide a pleated nanofiltration membrane prepared by the preparation method.
[0020] The present invention helps the NF membrane to form a wrinkled PA layer by introducing additional nanobubbles and generating sufficiently low interfacial tension at the same time. The surfactant sodium dodecylbenzene sulfonate (SDBS) has the functions of nanofoaming and reducing interfacial tension, and can form sufficient nanobubbles at the PIP / TMC interface, which helps to shape the PA layer. By enhancing the gas solubility of the PIP solution at low temperature, the number of nanobubbles can be further increased, and the encapsulation of nanobubbles between the PA layer and the substrate can be promoted to form a wrinkled structure.
[0021] The above technical solution of the present invention has the following advantages compared with the prior art:
[0022] (1) Compared with the traditional PIP / water system, surfactant / amine monomer (such as SDBS / PIP) can easily prepare a wrinkled NF membrane structure with a larger specific surface area by introducing only one additional substance and simultaneously controlling the temperature, which effectively increases the water transport area and significantly enhances the water permeability of the NF membrane.
[0023] (2) SDBS as a surfactant can improve the wettability of the base membrane, allowing it to fully absorb the PIP / water solution, thereby increasing the cross-linking degree of the PA layer and achieving excellent salt retention performance.
[0024] (3) The membrane preparation process of the pleated NF membrane is relatively simple and easy to operate, and it is easy to realize the industrialization of the new membrane preparation formula, and has high industrial application potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:
[0026] Figure 1 It is a scanning electron microscope image of the surface of five NF membranes prepared in Comparative Example 1 and Examples 1-4.
[0027] Figure 2 It is a comparison chart of the water permeability and Na2SO4 rejection rate of the five NF membranes prepared in Comparative Example 1 and Examples 1-4. DETAILED DESCRIPTION
[0028] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0029] The calculation methods of water permeability and salt retention rate of the present invention are conventional methods in the art.
[0030] (1) Water permeability: The nanofiltration membrane samples were pre-pressed with pure water at an operating pressure of 6 bar for 1 h. The test was carried out under cross-flow filtration conditions with an operating pressure of 6 bar, a water temperature of 25°C, and a cross-flow rate of 18 cm / s. At the same time, the water effluent from each sample membrane was taken and the volume was measured to calculate the water permeability.
[0031] (2) Na2SO4 retention rate: Use pure water to pre-press the nanofiltration membrane sample at an operating pressure of 6 bar for 1 h to prepare a 10 mM Na2SO4 aqueous solution. Then, test it under cross-flow filtration conditions with an operating pressure of 6 bar, a water temperature of 25°C, and a cross-flow rate of 18 cm / s. The salt concentration is determined based on the conductivity of the inlet and outlet water, and the salt retention rate is calculated.
[0032] (3) The nanofiltration membrane samples obtained in the embodiment and the comparative example were pre-pressed with pure water at an operating pressure of 6 bar for 1 hour. The test was carried out under cross-flow filtration conditions with an operating pressure of 6 bar, a water temperature of 25°C, and a cross-flow rate of 18 cm / s. Within the same period of time, the water effluent from each sample membrane was taken and the volume was measured to calculate the water permeability.
[0033] (4) At 20°C, place a certain amount of trimesoyl chloride (TMC) in 100 mL of n-hexane and stir thoroughly to obtain a TMC / n-hexane solution.
[0034] Example 1
[0035] This embodiment provides a method for preparing a pleated nanofiltration membrane, and the specific steps are as follows:
[0036] At 0°C, SDBS and PIP solutions were prepared in deionized water to obtain an SDBS / PIP aqueous solution with a SDBS concentration of 4CMC and a PIP concentration of 0.2wt / v%. The PVDF base membrane was immersed in the SDBS / PIP aqueous solution for 2 minutes, and then the excess solution on the surface of the base membrane was removed by a roller. Then, the surface of the base membrane was treated with a 0.16wt / v% TMC / n-hexane solution for 30 seconds. After the solution was poured off, the NF membrane was washed several times with n-hexane and deionized water to obtain a pleated nanofiltration membrane.
[0037] The structure of the pleated nanofiltration membrane obtained in Example 1 was characterized. Figure 1 ,according to Figure 1The results of scanning electron microscopy observations showed that the surface of the PA layer of Example 1 exhibited an obvious bubble-like wrinkle structure, which may be due to the increase in gas solubility at 0°C, which enhanced the abundance of nanobubbles and promoted the encapsulation of nanobubbles between the PA layer and the base film.
[0038] Example 2
[0039] This embodiment provides a method for preparing a pleated nanofiltration membrane, and the specific steps are as follows:
[0040] At 5°C, the PIP solution was prepared in deionized water to obtain an SDBS / PIP aqueous solution with a SDBS concentration of 4CMC and a PIP concentration of 0.2wt / v%. The PVDF base membrane was immersed in the SDBS / PIP aqueous solution for 2 minutes, and then the excess solution on the base membrane surface was removed by a roller. Then, the base membrane surface was treated with a 0.16wt / v% TMC / n-hexane solution for 30 seconds, and after the solution was poured off, it was washed with n-hexane and deionized water several times to obtain a pleated nanofiltration membrane.
[0041] The structure of the pleated nanofiltration membrane obtained in Example 2 was characterized. Figure 1 ,according to Figure 1 The scanning electron microscope observation results show that the bubble-like wrinkle structure on the surface of the PA layer of Example 2 is weaker than that of Example 1.
[0042] Example 3
[0043] This embodiment provides a method for preparing a pleated nanofiltration membrane, and the specific steps are as follows:
[0044] At 10°C, SDBS and PIP solutions were prepared in deionized water to obtain an SDBS / PIP aqueous solution with a SDBS concentration of 4CMC and a PIP concentration of 0.2wt / v%. The PVDF base membrane was immersed in the SDBS / PIP aqueous solution for 2 minutes, and then the excess solution on the base membrane surface was removed by a roller. Then, the base membrane surface was treated with a 0.16wt / v% TMC / n-hexane solution for 30 seconds, and after the solution was poured off, it was washed with n-hexane and deionized water several times to obtain a pleated nanofiltration membrane.
[0045] The structure of the pleated nanofiltration membrane obtained in Example 3 was characterized. Figure 1 ,according to Figure 1 The scanning electron microscope observation results show that the bubble-like wrinkle structure on the surface of the PA layer of Example 3 is weaker than that of Example 1 and Example 2.
[0046] Example 4
[0047] This embodiment provides a method for preparing a pleated nanofiltration membrane, and the specific steps are as follows:
[0048] At 20°C, SDBS and PIP solutions were prepared in deionized water to obtain an SDBS / PIP aqueous solution with a SDBS concentration of 4CMC and a PIP concentration of 0.2wt / v%. The PVDF base membrane was immersed in the SDBS / PIP aqueous solution for 2 minutes, and then the excess solution on the surface of the base membrane was removed by a roller. Then, the base membrane surface was treated with a 0.16wt / v% TMC / n-hexane solution for 30 seconds, and after the solution was poured off, it was washed with n-hexane and deionized water several times to obtain a pleated nanofiltration membrane.
[0049] The structure of the pleated nanofiltration membrane obtained in Example 4 was characterized. Figure 1 ,according to Figure 1 The scanning electron microscope observation results show that the bubble-like wrinkle structure presented on the surface of the PA layer of Example 4 is weaker than that of Example 1, Example 2, and Example 3.
[0050] Comparative Example 1 (Compared with Example 4)
[0051] This comparative example provides a method for preparing a NF membrane, and the specific steps are as follows:
[0052] At 20°C, the PIP solution was prepared in deionized water to obtain a PIP aqueous solution with a concentration of 0.2wt / v%. The PVDF base film was immersed in the PIP aqueous solution for 2 minutes, and then the excess solution on the surface of the base film was removed by a roller. Then, the surface of the base film was treated with a 0.16wt / v% TMC / n-hexane solution for 30 seconds, and after the solution was poured off, it was washed with n-hexane and deionized water several times to obtain a NF membrane.
[0053] The NF membrane obtained in Comparative Example 1 was structurally characterized. Figure 1 ,according to Figure 1 The results of scanning electron microscopy showed that no continuous PA layer was formed in Comparative Example 1. This may be because the relatively hydrophobic characteristics of the PVDF base film are not conducive to the adsorption and uniform distribution of PIP / water, making it difficult to form a typical PA layer.
[0054] Test Example 1
[0055] Water permeability: Use pure water to pre-press the nanofiltration membrane samples obtained in the embodiment and the comparative example at an operating pressure of 6 bar for 1 hour. The test is carried out under the cross-flow filtration conditions of an operating pressure of 6 bar, a water temperature of 25°C, and a cross-flow rate of 18 cm / s. In the same time, the water outflow of each sample membrane is taken and the volume is measured to calculate the water permeability. Detailed test results are shown in Figure 2 .
[0056] Na2SO4 retention rate: The nanofiltration membrane samples obtained in the embodiment and the comparative example were pre-pressed with pure water at an operating pressure of 6 bar for 1 hour to prepare a 10 mM Na2SO4 aqueous solution, and then tested under cross-flow filtration conditions of an operating pressure of 6 bar, a water temperature of 25°C, and a cross-flow rate of 18 cm / s. The salt concentration was determined based on the conductivity of the inlet and outlet water, and the salt retention rate was calculated. The detailed test results are shown in Figure 2 .
[0057] through Figure 2 It shows that as the temperature increases, the water permeability of the NF membrane decreases. The water permeabilities of Examples 1, 2, 3, and 4 decrease in turn, indicating that the PA layer of the NF membrane prepared by low temperature control has better water permeability and a larger water transmission area, thereby promoting water transmission. Among them, Example 1 shows the highest water permeability, reaching 36.25±0.42L·m -2 ·h -1 bar -1 , corresponding to Figure 1 In addition, the salt rejection (97.00 ± 0.58%) remained relatively stable compared with other temperature-controlled membranes.
[0058] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. A method for preparing a pleated nanofiltration membrane based on low-temperature interfacial tension regulation and enhanced nanofoaming, characterized in that: The following steps are involved: (1) mixing a surfactant solution and an amine monomer solution and dissolving them in water to obtain a surfactant / amine monomer aqueous solution; (2) placing the surfactant / amine monomer aqueous solution obtained in step (1) in a low-temperature water bath to adjust the solubility of the bubbles; (3) treating the base film in a surfactant / amine monomer aqueous solution and removing excess solution on the surface of the base film; (4) treating the surface of the base film obtained in step (3) with a trimesoyl chloride / n-hexane solution to react and form a PA layer, thereby obtaining the pleated nanofiltration membrane.
2. The preparation method according to claim 1, characterized in that: In step (1), the surfactant is selected from sodium dodecylbenzene sulfonate and / or sodium dodecyl sulfate.
3. The preparation method according to claim 1, characterized in that: In step (1), the amine monomer is selected from piperazine.
4. The preparation method according to claim 1, characterized in that: In step (1), the concentration of the surfactant in the surfactant / amine monomer aqueous solution is 1-10 CMC.
5. The preparation method according to claim 1, characterized in that: In step (1), the concentration of the amine monomer in the surfactant / amine monomer aqueous solution is 0.1-5.0 wt / v%.
6. The preparation method according to claim 1, characterized in that: In step (2), the temperature of the low-temperature water bath is set to 0-20°C.
7. The preparation method according to claim 1, characterized in that: In step (3), the base membrane is selected from PVDF base membrane and / or polyethersulfone base membrane; and the treatment time is 1 to 5 minutes.
8. The preparation method according to claim 1, characterized in that: In step (4), the mass volume fraction of the trimesoyl chloride / n-hexane solution is 0.1-0.3 wt / v%.
9. The preparation method according to claim 1, characterized in that: In step (4), the time for treating the surface of the base film is 30-90 seconds.
10. A pleated nanofiltration membrane, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 9.