Method for preparing MOF-808 film with assistance of zirconium-oxygen clusters and application of MOF-808 film

The MOF-808 film is assisted by the preparation of zirconium oxygen cluster powder, which solves the problems of low uranium content and interferes with ions in seawater uranium extraction technology, and realizes the preparation of high-efficiency MOF-808 film under mild conditions for uranium extraction and dyes in seawater Efficient separation of wastewater.

CN118904114AActive Publication Date: 2024-11-08DALIAN UNIV OF TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411057565.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-08
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

The existing seawater uranium extraction technology is low in uranium content and rich in interfering ions, which leads to cumbersome operation, serious pollution and high cost. The MOF-808 film is easily formed during preparation at high temperatures, which affects the separation performance. .

Method used

Using zirconium oxygen cluster powder as metal source, MOF-808 membrane was prepared on porous carrier by epitaxial growth method, reducing activation energy and regulating the number of ligand deletions, realizing the preparation of MOF-808 membrane under mild reaction conditions, using size screening The action achieves efficient selective separation of uranyl ions.

Benefits of technology

It significantly reduces the preparation activation energy of MOF-808 membrane, reduces mesometric defects, improves separation performance, realizes penetration of small-sized metal ions and efficient retention of large-sized uranyl ions, and is suitable for seawater uranium extraction and Desalination of salt-containing dye wastewater.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904114A_ABST
    Figure CN118904114A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing an MOF-808 film with assistance of zirconium oxygen clusters and application of the MOF-808 film. The preparation method comprises the following specific steps: firstly, preparing zirconium-oxygen cluster powder as a metal zirconium source; then adding zirconium-oxygen cluster powder and trimesic acid into the reaction solution, and reacting to obtain an MOF-808 seed crystal; and finally, preparing the MOF-808 film under different reaction conditions by utilizing an epitaxial growth method. The prepared molecular sieve membrane has good mechanical, chemical and thermal stability. The zirconium-oxygen cluster powder is used as a zirconium metal source, and the composition of the raw material solution is regulated, so that the reaction kinetics is remarkably reduced, and the ligand deletion number in the MOF-808 skeleton structure is precisely regulated. The membrane material shows excellent interception and selective separation performance in separation of dye desalination, uranium extraction from seawater and the like, so that a guidance scheme is provided for efficient separation of guest molecules in a solution phase.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of membrane separation, and specifically relates to a method for preparing a MOF-808 membrane assisted by zirconium oxygen clusters and an application thereof. Technical Background

[0002] As a clean energy, nuclear energy is gradually replacing traditional energy structure. Compared with land, uranium in seawater (usually UO2 2+ The content is extremely rich (about 4.5×10 9 Tons), which is more than 1,000 times that of terrestrial uranium mines [3-5]. So far, scientists have developed a variety of seawater uranium extraction technologies, including chemical precipitation, biological treatment, superconducting magnetic separation, solvent extraction, ion exchange, and adsorption. However, due to the low uranium content in seawater (~3.3 mg / t) and the high concentration of Na + , K + , Ca 2+ Mg 2+ , Fe 3+ The above technologies generally have problems such as complicated operation process, serious secondary pollution and high initial investment cost.

[0003] Membrane separation is a new technology that uses pressure difference as a driving force to achieve selective separation by utilizing the difference in mass transfer rates of different guest molecules or components in the membrane material. Since membrane separation is not limited by phase change and thermodynamic equilibrium, it has the advantages of low energy consumption, high separation efficiency, small footprint and simple operation. Among them, metal organic frameworks (MOFs) can accurately identify molecules or ions with different physicochemical properties and tiny structures due to their uniform pore size, flexible and adjustable skeleton structure and chemical composition. As far as the preparation of MOF-808 polycrystalline membrane is concerned, the rate-controlling step of its growth is the skeleton structure formation stage, and Zr6O needs to be pre-formed in the bulk solution. x (OH) y The secondary structural unit, this process requires sufficient external energy to overcome the activation energy required for growth; and the higher reaction temperature often leads to unnecessary intercrystalline defects in the membrane process, forming a large number of non-selective diffusion paths, resulting in the attenuation of separation performance. By tailoring the preparation of specific MOF-808 membranes, it is expected to show great application prospects in the fields of solution phase separation such as organic matter purification, seawater desalination, ion screening and seawater uranium extraction. Summary of the invention

[0004] Zirconium-oxygen clusters are important members of tetravalent transition metal clusters. The good coordination between the cluster core and the charge-compensating anion makes zirconium-oxygen clusters an ideal metal source for synthesizing MOF-808 membranes. Zirconium-oxygen cluster powders can pre-form cluster cores in the MOF-808 skeleton, significantly reducing the activation energy required to form the MOF-808 skeleton, and achieving mild reaction conditions to prepare MOF-808 membranes with good connectivity; at the same time, the number of missing ligands in MOF-808 can be precisely controlled by changing the composition of the raw material solution or the reaction temperature, achieving a huge breakthrough in the separation performance of MOF-808 membranes.

[0005] The present invention provides a method for preparing MOF-808 membrane with the aid of zirconium oxo clusters. Zirconium oxo cluster powder is prepared as a metal zirconium source, a ligand of trimesic acid is added to the reaction solution, and a polycrystalline membrane with good symbiosis is obtained on a porous carrier by an epitaxial growth method at -20 to 120°C. The MOF-808 membrane quickly penetrates small-sized interfering metal ions, effectively intercepts large-sized uranyl ions, and the inherent skeleton structure stability of the material itself in the water environment can realize the desalination of salt-containing dye wastewater and the efficient selective separation of uranyl ions through size screening.

[0006] The technical solution of the present invention is:

[0007] A method for preparing a MOF-808 film assisted by zirconium oxide clusters comprises the following steps:

[0008] (1) dissolving a metal zirconium salt in a mixture of an acid I and an organic solvent to react, and after the reaction is completed, washing and drying to obtain zirconium oxide cluster powder; the organic solvent comprises one or more of methanol, ethanol, propanol, isopropanol, water and acetonitrile; the acid I comprises one or more of formic acid, acetic acid, propionic acid and benzoic acid;

[0009] (2) dissolving trimesic acid and zirconium oxide cluster powder in a mixture of acid II and a reaction solvent, loading the mixture into a reaction kettle for reaction, and then washing and drying to obtain MOF-808 seed crystals;

[0010] (3) uniformly coating or dipping the MOF-808 seed solution on the surface of the porous support and drying it for later use;

[0011] (4) dissolving trimesic acid and zirconium oxide cluster powder in a mixed solution of acid II and a reaction solvent to obtain a film precursor solution;

[0012] (5) sealing both ends of the support modified with the seed crystal in (3), placing it in the film-forming precursor solution (4) above, and placing it in a reaction kettle for reaction;

[0013] (6) After the reaction is completed, washing and drying can obtain a MOF-808 molecular sieve membrane with good intergrowth properties;

[0014] The reaction solvent includes at least one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylformamide, methanol, chloroform, dichloroethane, methanol, ethanol, propanol, isopropanol, water and acetonitrile; the acid II includes one or more of formic acid, acetic acid, propionic acid, sulfuric acid, hydrochloric acid, nitric acid and benzoic acid.

[0015] Preferably, the metal zirconium salt described in step (1) includes one or more of zirconium tetrachloride, zirconium n-propoxide, zirconium disulfide, zirconium oxychloride, zirconium acetate, zirconium sulfate, zirconium nitrate and organic zirconium salts.

[0016] Preferably, in step (1), the mass ratio of the zirconium salt, the organic solvent and the acid I is 1:1-10:1-5.

[0017] Preferably, the reaction temperature in step (1) is 60-180° C., and the reaction period is 10 min-24 h.

[0018] Preferably, in step (2) and step (4), the mass ratio of the reaction solvent, acid II, zirconium oxycluster powder and trimesic acid is 1-100:1-80:1-100:1, and further, the mass ratio of the reaction solvent, acid II, zirconium oxycluster powder and trimesic acid is 1-20:1-5:1-20:1.

[0019] Preferably, the reaction temperature in step (2) and step (5) is -20 to 120°C, and the reaction time is 1 to 720 hours. Furthermore, the reaction temperature in step (2) and step (5) is 25 to 50°C.

[0020] Preferably, the concentration of the seed solution in step (3) is 0.1-0.5 wt. %; the coating methods include: dip coating, spin coating, spray coating, wiping coating or interface self-assembly.

[0021] Preferably, the porous carrier described in step (3) comprises: one or more of porous metal oxides, porous non-metallic oxides, porous metals, carbides and porous polymers; the structure of the porous carrier comprises a flat plate structure, a tubular structure, a hollow fiber structure or a rolled structure.

[0022] Preferably, the reaction solvent in step (2) and step (4) comprises at least one of methanol, ethanol, propanol, isopropanol, water and acetonitrile.

[0023] Preferably, the heating method in step (5) is convection heating or microwave heating (single mode or multi-mode heating).

[0024] The present invention also provides application of MOF-808 membrane in desalination of salt-containing dye wastewater.

[0025] The invention also provides application of MOF-808 membrane in uranyl ion interception and uranium extraction from seawater.

[0026] Examples of metals mainly contained in natural seawater are K + / Na + / Mg 2+ / Ca 2+ / Fe 3+ / UO2 2+ .

[0027] MOF-808 is a typical representative of zirconium-based metal organic frameworks. The MOF-808 membrane obtained based on microscopic size differences can accurately identify uranyl ions (molecular dynamics diameter: UO2 2+ : K + : Na + : Ca 2+ : Mg 2+ : and Fe 3+ : ), so the precise separation of uranyl ions or large-sized dye molecules from many other metal ions can be achieved through size screening, and the MOF-808 membrane material can specifically recognize uranyl ions and large-sized dye molecules.

[0028] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0029] The present invention uses synthetic zirconium oxygen cluster powder as a zirconium source, which can significantly reduce the activation energy required for the growth of MOF-808; a seed epitaxial growth method is used to prepare a MOF-808 membrane with excellent intergrowth and good density on a porous carrier. Using zirconium oxygen clusters as a metal source can realize the preparation of MOF-808 membrane at a lower reaction temperature on the one hand, and reduce the defects of MOF-808 membrane at the mesoscopic level as much as possible; on the other hand, it can accurately control the number of ligand deletions in the MOF-808 membrane skeleton at the microscopic level, which has a positive effect on the separation performance, ensuring effective penetration of small-sized hydrated metal ions, and efficient retention of large-sized dye molecules and uranyl ions, highlighting huge application prospects in pervaporation dehydration, (organic matter) nanofiltration, uranyl ion retention and uranium extraction from seawater. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 (a) SEM image and (b) XRD pattern of the zirconium oxide cluster powder prepared in Example 1.

[0031] Figure 2 (a) XRD pattern and (b) SEM image of MOF-808 seeds prepared in Example 1.

[0032] Figure 3 (a) XRD pattern of the MOF-808 film prepared in Example 2.

[0033] Figure 4 (a) SEM image and (b) SEM cross-sectional image of the MOF-808 membrane prepared in Example 2.

[0034] Figure 5 This is the SEM image of the MOF-808 membrane prepared in Example 3.

[0035] Figure 6 This is the SEM image of the MOF-808 membrane prepared in Example 4.

[0036] Figure 7 (a) XRD pattern and (b) SEM image of MOF-808 seeds prepared in Example 5.

[0037] Figure 8 (a) SEM plan view and (b) SEM cross-sectional view of the MOF-808 membrane prepared in Example 6.

[0038] Fig. 9 The separation performance of the MOF-808 membrane prepared in Example 2 for uranyl ions in seawater.

[0039] Figure 10-11 This is the separation stability test of the MOF-808 membrane prepared in Example 2.

[0040] Fig.12 This is the MOF-808 membrane prepared directly in situ on the original support of Comparative Example 1.

[0041] Fig.13 For Comparative Example 2, a MOF-808 membrane was prepared at room temperature using zirconium chloride as a zirconium source.

[0042] Fig.14 For Comparative Example 2, a MOF-808 membrane was prepared at room temperature using zirconium oxychloride as a zirconium source.

[0043] Fig.15 For Comparative Example 2, a MOF-808 membrane was prepared at room temperature using zirconium n-propoxide as a zirconium source.

[0044] Figure 16-18 This is a MOF-808 membrane prepared at room temperature by controlling the reaction time in comparison example 3.

[0045] Fig.19 This is a MOF-808 membrane prepared by temperature using liquid phase metal clusters in comparative example 4.

[0046] Fig. 20 (a) XRD pattern and (b) SEM pattern of MOF-808 seeds prepared in Comparative Example 5.

[0047] Fig.21 (a) XRD pattern and (b) SEM image of the MOF-808 film prepared in Comparative Example 6.

[0048] Fig. 22 This is the SEM cross-sectional image of the MOF-808 membrane prepared in Comparative Example 6. DETAILED DESCRIPTION

[0049] The present invention will be further described below in conjunction with specific examples. The following examples will help researchers and scientific researchers in the field to further understand the present invention. Once the technical personnel in the field know the concept of the present invention, they can make changes, modifications and even improvements to the following examples. Therefore, these should all fall within the scope of protection of the present invention.

[0050] Example 1: Hydrothermal preparation of MOF-808 seeds at room temperature (25°C)

[0051] (1) Add 10 g of zirconium tetrachloride to a mixed solution of 15 mL of acetic acid and 25 mL of isopropanol, heat and stir at 120° C. for 1 h, and wash and dry to obtain zirconium oxide cluster powder.

[0052] (2) 1.201 g of zirconium oxide and 0.301 g of trimesic acid were added to a mixed solution of 12 mL of formic acid and 20 mL of deionized water, and the solution was stirred to obtain a reaction precursor solution.

[0053] (3) The above reaction precursors were placed at room temperature for reaction for 3 days.

[0054] (4) After the reaction is completed, the mixture is washed with a large amount of deionized water and methanol and centrifuged, and finally dried in an oven at 80°C to obtain MOF-808 seed crystals.

[0055] The SEM (1a) image shows that the size of the zirconium oxygen cluster powder is about 1-2μm, and the XRD (1b) diffraction peak shows that the obtained powder is pure phase zirconium oxygen cluster; the XRD (2a) diffraction peak shows that the obtained powder is pure phase MOF-808, and the SEM (2b) image shows that the MOF-808 seed crystals are well dispersed and uniform in size, about 300nm. The number of missing ligands is 0.95.

[0056] Example 2: Hydrothermal preparation of MOF-808 membrane at room temperature (25°C)

[0057] (1) 0.375 g of the zirconium oxide cluster powder prepared in Example 1 and 0.095 g of trimesic acid were dissolved in a mixture of 12 mL of formic acid and 25 mL of deionized water, and stirred to obtain a film precursor solution.

[0058] (2) The MOF-808 seed crystals prepared in Example 1 were uniformly coated on the surface of the alumina support and fully dried in an oven at 80°C.

[0059] (3) The two ends of the alumina carrier coated with the seed crystals are sealed and placed in an inner liner, and then the membrane precursor solution is added. The reaction is carried out at room temperature for 7 days after the stainless steel reactor is sealed.

[0060] (4) After the reaction is completed, cool to room temperature, remove the tube membrane, wash it with deionized water and methanol, and dry it naturally.

[0061] XRD( Figure 3 ) diffraction peaks indicate that the prepared film is pure MOF-808; SEM ( Figure 4 a) It can be observed that the MOF-808 film is continuous and dense without obvious defects; the film thickness is 1.9 μm ( Figure 4 b).

[0062] Example 3: Preparation of MOF-808 membrane on a sheet support by room temperature hydrothermal method

[0063] The difference from Example 2 is that the tubular carrier in step (3) is replaced by a sheet carrier, and the remaining steps are the same as Example 4.

[0064] SEM( Figure 5 ) Figure 2 shows that the prepared MOF-808 membrane is continuous and dense without obvious defects.

[0065] Example 4: Hydrothermal preparation of MOF-808 membrane at 50°C

[0066] (1) 0.131 g of the zirconium oxide cluster powder prepared in Example 1 and 0.069 g of trimesic acid were dissolved in a mixture of 10 mL of formic acid and 26 mL of deionized water, and stirred to obtain a film precursor solution.

[0067] (2) The MOF-808 seed crystals prepared in Example 1 were uniformly coated on the surface of the alumina support and fully dried in an oven at 50°C.

[0068] (3) The two ends of the alumina carrier coated with the seed crystals are sealed and placed in an inner liner, and then the membrane precursor solution is added. The reaction is carried out at 50° C. for 3 days after the stainless steel reactor is sealed.

[0069] (4) After the reaction is completed, cool to room temperature, remove the tube membrane, wash it with deionized water and methanol, and dry it naturally.

[0070] SEM( Figure 6 ) It can be observed that the MOF-808 membrane is continuous and dense without obvious defects.

[0071] Example 5: Hydrothermal preparation of MOF-808 seeds at 80°C

[0072] (1) 0.101 g of the zirconium oxide cluster prepared in Example 1 and 0.051 g of trimesic acid were added to a mixed solution of 12 mL of formic acid and 21 mL of deionized water, and the solution was stirred to obtain a reaction precursor solution.

[0073] (2) Place the above reaction precursor in an oven at 80°C for 18 hours.

[0074] (3) After the reaction is completed, the mixture is washed with a large amount of deionized water and methanol and centrifuged, and finally dried in an oven at 80°C to obtain MOF-808 seed crystals.

[0075] XRD( Figure 7 a) The diffraction peaks show that the obtained powder is pure MOF-808. The SEM (7b) image shows that the MOF-808 seed crystals are well dispersed and uniform in size, about 360 nm. The number of missing ligands is 0.65.

[0076] Example 6: Hydrothermal preparation of MOF-808 membrane at 70°C

[0077] (1) 0.100 g of zirconium oxide cluster and 0.050 g of trimesic acid were dissolved in a mixture of 12 mL of formic acid and 20 mL of deionized water, and stirred to obtain a membrane precursor solution.

[0078] (2) The MOF-808 seed crystals prepared in Example 5 were uniformly coated on the surface of the alumina support and fully dried in an oven at 80°C.

[0079] (3) The two ends of the alumina carrier coated with the seed crystals are sealed and placed in an inner liner, and then the membrane precursor solution is added. The reaction is carried out at 70° C. for 2 days after the stainless steel reactor is sealed.

[0080] (4) After the reaction is completed, cool to room temperature, remove the membrane, wash it with deionized water and methanol, and dry it naturally.

[0081] SEM( Figure 8 a) It can be observed that the prepared MOF-808 membrane is continuous and dense, without obvious defects, and the membrane thickness is 2.1 μm ( Figure 8 b).

[0082] Example 7: Testing of the dye desalination performance of MOF-808 membrane

[0083] The MOF-808 membrane prepared in Example 2 was subjected to a dye desalination test, and the test conditions were as follows: the transmembrane pressure difference was 1 bar, the salt concentration was 2 g / L, the dye concentration was 0.1 g / L, and a cross-flow separation test was performed.

[0084] The ion separation performance of MOF-808 membrane is shown in Table 1. The membrane layer prepared by epitaxial growth selectively separates the NaCl / dye mixed system (intercepting large molecular dyes and permeating smaller water and Na + ions), the results are shown in Table 1, in which MG is malachite green, MB is methyl blue, CR is Congo red, Na + The rejection rate is 14.1% and the permeate flux is 7.21m -2 h - 1 bar -1 , the most selective Na + / CR can reach 429.5. The above results show that the MOF-808 membrane prepared at room temperature using clusters exhibits excellent separation performance for dye desalination.

[0085] Table 1 Dye desalination performance test of MOF-808 membrane

[0086]

[0087]

[0088] Example 8: Testing of metal retention performance of MOF-808 membrane

[0089] The MOF-808 membrane prepared in Example 2 was subjected to a uranyl ion interception test under the following test conditions: the transmembrane pressure difference was 1 bar, K + , Na + , Ca 2+ ,Mg 2+ , Fe 3+ The cross-flow separation test was carried out with an ion concentration of 1 mM and a uranyl ion concentration of 0.1 mM. The results are shown in Table 2. The prepared membrane has a good performance for metal ions with small hydrated ions (K + , Na + , Ca 2+ ,Mg 2+ , Fe 3+ ) showed low rejection (7.9-98.6%) and a permeate flux of 4.982 L m -2 h -1 bar -1 to 6.473L m -2 h -1 bar -1 ; It showed a retention rate of 99.99% for uranyl ions. The above results show that the MOF-808 membrane prepared using zirconium oxide clusters has a high efficiency in retaining uranyl ions and a high permeation flux.

[0090] Table 2 Ion interception performance test of MOF-808 membrane

[0091]

[0092] Example 9: Performance test of MOF-808 membrane for uranium extraction from seawater

[0093] The MOF-808 membrane prepared in Example 2 was used to test the uranium extraction performance of seawater. Seawater mainly contains K + (~357ppm),Na + (~9336ppm),Mg 2+ (~873ppm),Ca 2+ (~357ppm), Fe 3+ (0.0041ppm), UO2 2+ (0.0030ppm) plasma, MOF-808 membrane still shows excellent selectivity for uranyl ions in real seawater (such as Fig. 9 ), the highest K + / UO2 2+ The separation selectivity reached 315.0.

[0094] Example 10: MOF-808 membrane stability test

[0095] The MOF-808 membrane prepared in Example 2 was subjected to continuous testing for uranium extraction from seawater (e.g. Figure 10-11 ), after 12 h, the flux remained relatively stable, and the separation selectivity still reached 301.6, indicating that the MOF-808 membrane prepared with the assistance of zirconium and oxygen has excellent operational stability.

[0096] Comparative Example 1: Direct in-situ preparation of MOF-808 membrane using original carrier

[0097] The specific implementation steps are the same as those in Example 2, except that the alumina carrier used in step (3) is replaced with an alumina carrier that is not coated with MOF-808 seeds.

[0098] SEM( Fig.12 ) showed that only sporadic grains were scattered on the surface of the carrier and most of the carrier was still exposed, proving that the original carrier was not easy to form a dense MOF-808 film.

[0099] Comparative Example 2: Preparation of MOF-808 membrane at room temperature by changing the type of metal source

[0100] The specific implementation steps are the same as those in Example 2, except that the zirconium oxycluster metal source used in step (1) is replaced with common zirconium chloride, zirconium oxychloride and zirconium n-propoxide.

[0101] SEM( Figure 13-15) showed that there was no sign of intergrowth in the seed layer on the surface of the carrier, proving that the use of zirconium oxo clusters can greatly reduce the activation energy required to form MOF-808. Therefore, by investigating different metal sources, under the optimal formula and reaction conditions, selecting the best metal source (zirconium oxo cluster powder) is an effective means to prepare MOF-808 membranes with excellent performance.

[0102] Comparative Example 3: Preparation of MOF-808 membrane at room temperature with single controlled reaction time

[0103] The specific implementation steps are the same as those in Example 2, except that the reaction time in step (3) is changed to 24h, 72h, or 120h.

[0104] SEM( Figure 16-18 ) showed that with the gradual extension of reaction time, the seed layer and cross section on the carrier surface gradually showed signs of connection, indicating that under the optimal formula and reaction conditions, controlling the reaction time is one of the effective ways to prepare MOF-808 membranes with excellent performance.

[0105] Comparative Example 4: Preparation of MOF-808 membrane by liquid metal clusters at 50°C

[0106] (1) 42 mL of N,N-dimethylformamide and 20 mL of formic acid were mixed, and then 0.15 g of zirconium oxychloride was added, and the mixture was uniformly dissolved by ultrasonic treatment for 10 min to obtain a raw material solution. The raw material solution was then heated at 150° C. for 3 h, and allowed to stand and cool to room temperature to form liquid clusters as the metal source for preparing the film layer.

[0107] (2) Add 0.180 g of trimesic acid to the above solution (1) and dissolve it by ultrasonication for 30 min to obtain a precursor solution.

[0108] (3) MOF-808 seed crystals were prepared as in Example 1 and coated on the surface of the support, and then dried in an oven at 70° C. overnight.

[0109] (4) The carrier coated with MOF-808 seed crystals was placed in the liner, and the above-mentioned precursor solution was poured in, followed by standing at 50° C. for 7 days to react.

[0110] SEM( Fig.19 ) showed that even if the reaction time was extended to one week, the seed layer on the surface of the carrier still did not show any signs of intergrowth, and the seed layer showed signs of falling off, indicating that liquid zirconium oxygen clusters cannot achieve the preparation of MOF-808 membranes with good intergrowth at room temperature.

[0111] Comparative Example 5: Preparation of MOF-808 Seed Crystals by Thermal Solvent Method

[0112] (1) Solvothermal preparation of MOF-808 seeds.

[0113] (1) 0.965 g of zirconium oxychloride and 0.210 g of trimesic acid were dissolved in a mixture of 25 mL of formic acid and 45 mL of N,N-dimethylformamide, and stirred to obtain a precursor solution.

[0114] (2) The above precursor solution was reacted at 120°C for 24 hours.

[0115] (3) After the reaction is completed, the mixture is washed and centrifuged with a large amount of N,N-dimethylformamide and methanol, and finally dried in an oven at 80°C.

[0116] XRD( Fig. 20 a) Diffraction peaks indicate that the prepared powder is pure phase MOF-808; SEM ( Fig. 20 b) It can be observed that the MOF-808 seed crystals are well dispersed and uniform in size, about 360nm. The number of missing ligands is 0.08.

[0117] Comparative Example 6: Preparation of MOF-808 membrane by solvent thermal epitaxial growth

[0118] (1) 0.121 g of zirconium oxychloride and 0.086 g of trimesic acid were dissolved in a mixed solution of 20 mL of formic acid and 20 mL of N,N-dimethylformamide, and stirred to obtain a membrane precursor solution.

[0119] (2) The MOF-808 seed crystals prepared in Comparative Example 5 were uniformly coated on the surface of the alumina support and fully dried in an oven at 80°C.

[0120] (3) The two ends of the alumina carrier coated with the seed crystals are sealed and placed in an inner liner, and then the membrane precursor solution is added. The reaction is carried out at 120° C. for 36 hours after the stainless steel reactor is sealed.

[0121] (4) After the reaction is completed, cool to room temperature, remove the membrane, wash with N,N-dimethylformamide and methanol, and dry naturally.

[0122] XRD( Fig.21 a) The diffraction peaks show that the prepared MOF-808 membrane is pure phase; SEM ( Fig.21 b) It can be observed that the MOF-808 film is continuous and dense, without obvious defects, and has a thickness of ~2.3μm ( Fig. 22 ).

[0123] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they are aware of the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0124] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing MOF-808 membrane assisted by zirconium oxide clusters, characterized in that: The steps include: (1) dissolving a metal zirconium salt in a mixture of an acid I and an organic solvent to react, and after the reaction is completed, washing and drying to obtain zirconium oxide cluster powder; the organic solvent comprises one or more of methanol, ethanol, propanol, isopropanol, water and acetonitrile; the acid I comprises one or more of formic acid, acetic acid, propionic acid and benzoic acid; (2) dissolving trimesic acid and zirconium oxide cluster powder in a mixture of acid II and a reaction solvent, loading the mixture into a reaction kettle for reaction, and then washing and drying to obtain MOF-808 seed crystals; (3) uniformly coating or dipping the MOF-808 seed solution on the surface of the porous support and drying it for later use; (4) dissolving trimesic acid and zirconium oxide cluster powder in a mixed solution of acid II and a reaction solvent to obtain a film precursor solution; (5) sealing both ends of the support modified with the seed crystal in (3), placing it in a film-forming precursor solution, and placing it in a reaction kettle for reaction; (6) After the reaction is completed, washing and drying can obtain a MOF-808 molecular sieve membrane with good intergrowth properties; The reaction solvent includes at least one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylformamide, methanol, chloroform, dichloroethane, methanol, ethanol, propanol, isopropanol, water and acetonitrile; the acid II includes one or more of formic acid, acetic acid, propionic acid, sulfuric acid, hydrochloric acid, nitric acid and benzoic acid.

2. The method for preparing MOF-808 film assisted by zirconium oxide clusters according to claim 1, characterized in that: In step (1), the mass ratio of zirconium salt, organic solvent and acid I is 1:1-10:1-5.

3. The method for preparing MOF-808 film assisted by zirconium oxide clusters according to claim 1, characterized in that: In step (1), the reaction temperature is 60-180° C. and the reaction period is 10 min-24 h.

4. The method for preparing MOF-808 film assisted by zirconium oxide clusters according to claim 1, characterized in that: In step (2) and step (4), the mass ratio of the reaction solvent, acid II, zirconium oxide cluster powder and trimesic acid is 1-100:1-80:1-100:

1.

5. The method for preparing MOF-808 film assisted by zirconium oxide clusters according to claim 1, characterized in that: Preferably, the reaction temperature of step (2) and step (5) is -20 to 120°C; and the reaction time is 1 to 720 hours.

6. The method for preparing MOF-808 film assisted by zirconium oxide clusters according to claim 5, characterized in that: The reaction temperature in step (2) and step (5) is 25 to 50°C.

7. The method for preparing MOF-808 film assisted by zirconium oxide clusters according to claim 1, characterized in that: The concentration of the seed solution in step (3) is 0.1-0.5 wt. %; the coating methods include: dip coating, spin coating, spray coating, rubbing coating or interface self-assembly.

8. The method for preparing MOF-808 film with the aid of zirconium oxide clusters according to claim 1, characterized in that: The porous carrier described in step (3) includes: one or more of porous metal oxides, porous non-metallic oxides, porous metals, carbides and porous polymers; the structure of the porous carrier includes a flat plate structure, a tubular structure, a hollow fiber structure or a rolled structure.

9. Use of the MOF-808 membrane obtained by the method of claim 1 in desalination of salt-containing dye wastewater.

10. Use of the MOF-808 membrane obtained by the method of claim 1 in uranyl ion interception and uranium extraction from seawater.

Citation Information

Patent Citations

  • Hygroscopic metal organic framework material-chitosan mixed matrix membrane and preparation and application

    CN106621834A

  • Preparation method of oxidative desulfurization catalyst based on Zr-MOFs composite material

    CN112371191A