Preparation method and application of zero-valent iron biochar-based repair material
By preparing biochar material loaded with nano zero-valent iron, the limitations of nitrate nitrogen purification in the water body in the prior art are solved, and efficient removal of nitrate under different pH conditions is achieved, which significantly improves the stability and adsorption performance of the material. , meets the needs of efficient, low-cost and environmentally friendly water purification.
Patent Information
- Application Number
- CN202410964841.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
The existing technology has many limitations in the method of purifying nitrate nitrogen in water bodies, including the need for strict environmental control of biological denitrification technology, high cost of chemical reduction and toxic by-products, high cost of reverse osmosis or electrodialysis and high energy consumption, and wetland treatment technology The area is large and the efficiency is unstable, and it cannot fully meet the needs of high efficiency, low cost and environmentally friendly.
Using the preparation method of zero-valent iron biochar based restoration material, the nano-valent iron-loaded biochar is prepared by drying, crushing, pyrolysis, ball milling and calcining of corn stalks, and combined with potassium ferrate to improve the material Stability and adsorption properties ensure efficient removal of nitrates under different pH conditions.
It has achieved efficient removal of nitrates in a wide pH range, with a removal rate of 80% to 98%, improved material stability, low cost, and environmentally friendly, and is suitable for high-concentration nitrogen-polluted wastewater treatment, achieving the purpose of green and efficient treatment.
Smart Images

Figure CN118904283A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of water pollution control, and in particular to a preparation method and application of a zero-valent iron biochar-based repair material. Background Art
[0002] In the past few decades, global agriculture has used a large amount of synthetic nitrogen fertilizers to meet the growing demand for food. According to the latest statistics from the International Fertilizer Association (IFA), the global production of nitrogen fertilizers in 2018 was about 103.7 million tons. However, the excessive use of nitrogen fertilizers has caused serious environmental problems, including soil quality degradation, water resource pollution, increased greenhouse gas emissions, and global warming. In addition, nitrogen pollution also poses a threat to human health, increasing the risk of diseases such as methemoglobinemia and colorectal cancer.
[0003] Urban, industrial and agricultural wastewater contains high concentrations of nitrogen. Direct discharge of these nitrogen-rich wastewaters into water bodies will lead to eutrophication of water bodies and destroy the balance of aquatic ecosystems. Nitrate (NO3 - -N) is one of the pollutants widely present in aquatic ecosystems. Due to its high water solubility and stability, it is easy to accumulate in the environment, leading to a decrease in oxygen concentration in water bodies, the death of a large number of fish, and the overgrowth of algae and phytoplankton, thus causing serious damage to the ecosystem. In addition, excessive NO3 in drinking water - -N pollution seriously affects human health and increases the risk of methemoglobinemia and colorectal cancer. Therefore, developing an efficient and environmentally friendly nitrate removal material has become an urgent scientific task.
[0004] Deficiencies of existing technology:
[0005] At present, there are many problems in the method of purifying nitrate nitrogen in water:
[0006] Biological denitrification technology: requires strict environmental control (such as temperature, pH value, dissolved oxygen), and may produce other pollutants such as N2O.
[0007] Chemical reduction: The use of sulfide reduction is costly and may produce toxic or hazardous by-products.
[0008] Reverse osmosis or electrodialysis: high cost, membrane fouling, short life and high energy consumption.
[0009] Wetland treatment technology: requires a larger area, reduces land use efficiency, and wetland plants are sensitive to climate and soil conditions, and the purification effect is unstable.
[0010] These methods have their own limitations and cannot fully meet the needs of practical applications. Therefore, there is an urgent need for a new material that can remove nitrate from water in an efficient, low-cost and environmentally friendly manner. Summary of the invention
[0011] In view of the shortcomings of the prior art, the zero-valent iron biochar-based remediation material of the present invention has significantly improved the stability, adsorption and reduction properties of the material through an innovative preparation method. It has broad application prospects and significant environmental benefits. It is particularly suitable for treating high-concentration nitrogen-contaminated wastewater, achieving the goal of green and efficient treatment.
[0012] To achieve the above objectives, the present invention is implemented by the following technical scheme: A method for preparing a zero-valent iron biochar-based repair material, comprising the following steps:
[0013] (1) The washed corn stalks are placed in an oven and dried at 105°C for 24 hours to ensure that the moisture is completely removed and to prevent excessive water vapor from being generated in the subsequent steps; the dried corn stalks are crushed with a pulverizer to make the particles uniform, and sieved through a 20-mesh nylon sieve to obtain fine-grained corn stalk powder. The sieved corn stalk powder is collected in a drying container for later use;
[0014] (2) Pyrolysis process: The crushed corn stalks were placed in a carbonization tank, and then placed in a muffle furnace, and nitrogen (flow rate 0.1m 3 / h), heated to 550℃ to 650℃ at a heating rate of 3℃ / min to 7℃ / min, and maintained for 1.5 to 2.5 hours. During the pyrolysis process, a nitrogen flow was used to maintain an oxygen-free environment to prevent the straw from being oxidized. After pyrolysis, the temperature was naturally cooled to room temperature and the black solid was collected.
[0015] Washing and drying: Wash the black solid (biochar) after pyrolysis with deionized water several times to remove the residual substances on the surface. After washing, put the biochar into an oven and dry it at 70-80℃ to ensure that the biochar is dry. Finally, grind the dried biochar and pass it through a 100-mesh nylon sieve to obtain uniform corn straw biochar (BC) and store it for later use;
[0016] (3) The prepared corn straw biochar (BC) was mixed with potassium ferrate (K2FeO4) at a mass ratio of 0.2:1 to 0.8:1 to ensure uniform mixing. The mixture was placed in a zirconia tank of a planetary ball mill (YXQM-2L) (zirconia ball diameter 5 mm, ball-to-material ratio of 20:1), operated in ambient air, and the ball mill speed was set to 400 to 600 r / min, forward rotation for 15 minutes, reverse rotation for 15 minutes, and a total time of 30 minutes. The ball milling process ensures adequate mixing and improves the uniformity of the material;
[0017] (4) Calcination process: The ball-milled mixed solid was placed in a muffle furnace for secondary calcination, and nitrogen (flow rate 0.1m 3 / h), heated to 750℃ to 850℃ at a heating rate of 3℃ / min to 7℃ / min, and maintained for 1.5 to 2.5 hours. During the calcination process, an oxygen-free environment was maintained by a nitrogen flow to ensure the reduced state of zero-valent iron. After pyrolysis, the temperature was naturally cooled to room temperature and a black solid was collected.
[0018] Washing and drying: The black solid after secondary calcination was washed with deionized water several times to remove the residual substances on the surface. After washing, the black solid was placed in an oven and dried at 70-80°C to ensure that the material was dry. Finally, the dried material was ground and passed through a 100-mesh nylon sieve to obtain the nano-zero-valent iron-loaded biochar (nZVI-BC), which was stored for later use.
[0019] Preferably, the mass ratio of potassium ferrate to corn straw biochar is 0.2:1 to 0.8:1;
[0020] The optimal mass ratio of potassium ferrate to biochar can ensure the uniform distribution and stable loading of nano-zero-valent iron, provide sufficient reduction activity, and control costs.
[0021] Preferably, the corn straw biochar is heated to 550° C. to 650° C. in a muffle furnace at a heating rate of 3° C. / min to 7° C. / min;
[0022] Controlling the heating rate and final temperature can optimize the pore structure and surface area of biochar, ensuring it has good adsorption properties.
[0023] Preferably, the rotation speed of the potassium ferrate and corn straw biochar mixture in the planetary ball mill is 400 to 600 r / min;
[0024] Appropriate ball milling speed can ensure adequate mixing of biochar and potassium ferrate, improve reaction efficiency, and prevent excessive wear of the materials.
[0025] Preferably, the nano-zero-valent iron biochar has a specific surface area of 50 to 200 m 2 / g, pore volume is 0.1 to 0.5cm 3 / g;
[0026] Preferably, the content of zero-valent iron in the nano-zero-valent iron-loaded biochar is 10% to 20%;
[0027] The high specific surface area and pore volume increase the adsorption capacity and reactivity of the material, while the appropriate zero-valent iron content ensures efficient nitrate reduction ability.
[0028] Preferably, the repair material has the ability to remove nitrates at a pH value of 2 to 12;
[0029] The material maintains the ability to efficiently remove nitrates over a wide pH range, ensuring its applicability to a variety of complex water quality environments.
[0030] Preferably, the nitrate removal rate of the repair material is 80% to 98%;
[0031] The high removal rate ensures that the treated water meets environmental protection standards and is suitable for actual water purification projects.
[0032] Preferably, the zero-valent iron biochar-based remediation material is used to remove nitrate pollution in water bodies.
[0033] The present invention provides a preparation method and application of a zero-valent iron biochar-based repair material, which has the following beneficial effects:
[0034] 1. The present invention adopts a secondary calcination method, by subjecting a mixture of potassium ferrate and corn straw biochar to high temperature treatment in a nitrogen environment, so that nano zero-valent iron (nZVI) is evenly embedded in the biochar structure. The secondary calcination process not only effectively reduces the oxidation of zero-valent iron, but also enhances its distribution stability in biochar, avoiding the problem of easy shedding and diffusion of zero-valent iron particles during use. This treatment method significantly improves the stability and long-term use effect of the composite material.
[0035] 2. The present invention combines potassium ferrate with biochar to prepare a biochar-zero-valent iron composite material with a high specific surface area (50 to 200 m 2 / g) and pore volume (0.1 to 0.5 cm 3 / g). This high specific surface area and pore structure help increase the contact area between the material and the pollutants, thereby improving the adsorption and reaction efficiency. This makes the material exhibit extremely strong adsorption and reduction performance when treating wastewater and sewage containing high concentrations of active nitrogen.
[0036] 3. Potassium ferrate (K2FeO4) of the present invention is used as a modifier, which has strong oxidizing ability during the preparation process and can effectively convert the iron source into nano zero-valent iron. At the same time, potassium ferrate has the characteristics of low cost, easy acquisition and environmental friendliness. Its use not only reduces the production cost of composite materials, but also reduces the negative impact on the environment, which meets the requirements of green chemistry and sustainable development.
[0037] 4. The biochar-zero-valent iron composite material of the present invention exhibits good nitrate removal ability in a wide range of pH values from 2 to 12, with a removal rate of 80% to 98%. Especially under acidic conditions, the material has a particularly significant effect on nitrate reduction, which indicates that the material can maintain high pollutant removal performance under different environmental conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 The effect diagram of nZVI-BC with different iron-carbon ratios on nitrate reduction at different pH values;
[0039] Figure 2 This is a graph showing the effect of nZVI-BC with different iron-carbon ratios on nitrate removal at different pH values. DETAILED DESCRIPTION
[0040] The following will be combined with the drawings in the specification of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] Example:
[0042] Please see attached Figure 1 -Attached Figure 2 :
[0043] Example 1: Preparation of zero-valent iron biochar-based repair materials
[0044] Biochar preparation:
[0045] Step 1: Collect corn stalks and wash them with deionized water to ensure that the surface soil and impurities are removed. Place the washed corn stalks in an oven and dry them at 105°C for 24 hours to completely remove moisture and prevent excessive water vapor from being generated in subsequent steps.
[0046] Step 2: Use a crusher to crush the dried corn stalks to ensure uniform particle size, and pass through a 20-mesh nylon sieve to obtain fine-grained corn stalk powder. The screened corn stalk powder is collected in a drying container for later use.
[0047] Step 3: Put the crushed corn stalks into the carbonization tank, then place it in the muffle furnace and introduce nitrogen (flow rate 0.1m 3 / h), heated to 600℃ at a heating rate of 5℃ / min, and maintained for 2 hours. During the pyrolysis process, a nitrogen flow was used to maintain an oxygen-free environment to prevent straw oxidation. After pyrolysis, the temperature was naturally cooled to room temperature and the black solid was collected.
[0048] Step 4: Wash the black solid (biochar) after pyrolysis with deionized water several times to remove the residual substances on the surface. After washing, put the biochar into an oven and dry it at 70-80℃ to ensure that the biochar is dry. Finally, grind the dried biochar and pass it through a 100-mesh nylon sieve to obtain uniform corn straw biochar (BC) and store it for later use.
[0049] Zero-valent iron biochar preparation:
[0050] Step 1: Mix the prepared corn straw biochar (BC) with potassium ferrate (K2FeO4) at a mass ratio of 0.2:1 to 0.8:1 to ensure uniform mixing. The ratio of potassium ferrate can be adjusted as needed to optimize the loading amount of nano zero-valent iron.
[0051] Step 2: Place the mixture in a zirconia jar in a planetary ball mill (YXQM-2L) with a zirconia ball diameter of 5 mm and a ball-to-material ratio of 20:1. Ball milling is performed in a ball mill with a speed of 500 r / min, 15 minutes forward and 15 minutes reverse, for a total of 30 minutes. The ball milling process is performed in ambient air to ensure adequate mixing and improve the uniformity of the material.
[0052] Step 3: Place the ball-milled mixed solid in a muffle furnace for secondary calcination and introduce nitrogen (flow rate 0.1m 3 / h), heated to 750℃ to 850℃ at a heating rate of 3℃ / min to 7℃ / min, and maintained for 1.5 to 2.5 hours. During the calcination process, an oxygen-free environment was maintained by a nitrogen flow to ensure the reduced state of zero-valent iron. After pyrolysis, the temperature was naturally cooled to room temperature and a black solid was collected.
[0053] Step 4: Wash the black solid after secondary calcination with deionized water several times to remove residual substances on the surface. After washing, put the black solid into an oven and dry it at 70-80°C to ensure that the material is dry. Finally, grind the dried material and pass it through a 100-mesh nylon sieve to obtain nano-zero-valent iron-loaded biochar (nZVI-BC), which is stored for later use.
[0054] Example 2: Preparation of biochar-nano zero-valent iron composites with different Fe / C ratios
[0055] Preparation of biochar-nano zero-valent iron composites with different Fe / C ratios:
[0056] Step 1: Take a certain amount of corn straw biochar (BC) powder and mix it with four different doses of potassium ferrate (K2FeO4) at the mass ratio of iron to carbon of 0.2:1, 0.4:1, 0.6:1 and 0.8:1, respectively, ensuring that the mixture of each mixing ratio is uniform.
[0057] Step 2: Prepare according to the steps in Example 1. The mixture was placed in a planetary ball mill for ball milling, and then calcined twice to finally obtain nano zero-valent iron biochar materials with different Fe / C ratios, which were marked as nZVI-BC0.2, nZVI-BC0.4, nZVI-BC0.6 and nZVI-BC0.8, respectively.
[0058] Example 3: Experimental study on nitrate removal by biochar-nano zero-valent iron composite materials with different Fe / C ratios Experimental method:
[0059] Material characterization: An elemental analyzer (Vario MicroCube, Germany) was used to determine the content of elements (C, H, O and N) in the material to provide basic composition information of the material. X-ray diffraction (XRD, BrukerD8Advance) was used to determine the crystal structure of the material and determine the existence form of zero-valent iron in the material. A specific surface area analyzer (BET, MicrotracBEL Corp.) was used to calculate the pore size distribution and specific surface area of the biochar and analyze the adsorption properties of the material. Scanning electron microscopy (SEM) and energy dispersive spectrometer (EDS, Zeiss Auriga FIB) were used to observe the morphology of biochar and the relative content of surface elements to further verify the loading of zero-valent iron. X-ray photoelectron spectroscopy (XPS, AXIS SupraKratos Analytical Ltd) was used to determine the surface chemical properties of the material and analyze the chemical state of zero-valent iron. The magnetization intensity of the biochar was cyclically measured in the range of -20000 to 20000 Oe at room temperature using a vibrating probe sample magnetometer (MPMS3, Quantum Design) to evaluate its magnetic separation performance.
[0060] Experimental steps:
[0061] Step 1: Weigh 0.1 g of biochar (BC, nZVI-BC0.2, nZVI-BC0.4, nZVI-BC0.6 and nZVI-BC0.8) respectively and place them in a 50 mL centrifuge tube, and add 40 mL of 100 mg / L KNO3 solution.
[0062] Step 2: Use 0.5 mol / L HCl or NaOH solution to adjust the initial pH value of the solution, and set the pH gradient to 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, and 12 to ensure the comparability of experimental results under different pH conditions.
[0063] Step 3: Place the sample in a constant temperature shaker for 24 hours to ensure adequate reaction. After shaking, filter with a 0.22 μm filter membrane, collect the filtrate, store in a 15 mL centrifuge tube, and freeze to prevent sample deterioration.
[0064] Step 4: Use AA3 fully automatic continuous flow analyzer (Bran+Luebbe, Germany) to determine the contents of nitrate nitrogen, ammonium nitrogen and nitrite nitrogen in the filtrate and analyze the effect of the material on nitrate reduction.
[0065] Experimental results:
[0066] Material structure characterization and element content: The pH value of the material ranges from 11.4 to 12.6, the electrical conductivity (EC) is not less than 1400μs / cm, and the O / C atomic ratio is 0.15-0.85. The surface of the material has a layered structure, and the loaded iron particles increase the surface roughness and improve the adsorption capacity. The magnetization value of the material is between 7.11-19.32emu / g, showing good magnetic separation properties and easy recycling. The presence of Fe(0) was detected in the material, and the proportion of Fe(0) was 12.62-16.06%, indicating that the zero-valent iron loading is effective.
[0067] Table 1 Physical and chemical properties of biochar
[0068] Material pH EC(μs / cm) C(%) H(%) O(%) N(%) BC 9.58 454 37.21 0.34 3.84 0.71 nZVI-BC0.2 11.48 1492 29.96 0.11 4.42 0.41 nZVI-BC0.4 12.08 3820 22.97 0.19 7.01 35 nZVI-BC0.6 12.49 9950 18.1 0.29 11 0.28 nZVI-BC0.8 12.62 13810 14.6 0.44 12.36 0.53
[0069] Effects of nZVI-BC with different iron-carbon ratios on nitrate reduction at different pH values:
[0070] Ammonium nitrogen production: The ammonium nitrogen content generated by nZVI-BC0.6 and nZVI-BC0.8 is significantly higher than that of BC, nZVI-BC0.2 and nZVI-BC0.4, especially at low pH (pH = 2). As the pH value increases, the amount of ammonium nitrogen produced gradually decreases, but after the pH value exceeds 7, the reduction capacity of nZVI-BC0.6 and nZVI-BC0.8 tends to be stable. Figure 1 (A) shown.
[0071] Nitrate nitrogen removal effect: All nZVI-BC treatments had the lowest residual nitrate nitrogen content in the solution at pH = 2, which were 16.83, 12.63, 4.35 and 2.85 mg / L, respectively. As the pH value increased, the nitrate nitrogen concentration gradually increased, but tended to be stable when the pH value was above about 6, such as Figure 1 (B) shown.
[0072] Nitrite nitrogen production: The nitrite nitrogen content generated by nZVI-BC0.6 and nZVI-BC0.8 was significantly higher than that of BC, nZVI-BC0.2 and nZVI-BC0.4, especially under acidic conditions, where the nitrite nitrogen content was the highest, at 16.66, 16.90, 12.76 and 12.41 mg / L, respectively. As the pH value increased, the nitrite nitrogen concentration showed a downward trend, such as Figure 1 (C) shown.
[0073] Removal efficiency and reduction product selectivity:
[0074] Nitrate nitrogen removal rate: The nitrate nitrogen removal rate of all nZVI-BC treatments was significantly higher than that of the control (BC), and the highest removal rate was 83.17%, 87.37%, 95.65% and 97.16% at pH = 2. As the pH value increased, the nitrate nitrogen removal rate gradually decreased, but remained at a high level under neutral and alkaline conditions.
[0075] Selectivity of reduction products: At the same pH value, as the iron-carbon ratio increases, the selectivity of NH4 in the nitrate nitrogen reduction products increases. + The selectivity of -N gradually increased, among which nZVI-BC0.8 had the highest selectivity, with an average of 37.91%. At the same iron-carbon ratio, as the pH increased, the selectivity of nitrate nitrogen reduction products to N2 gradually increased, indicating that the generation of N2 had a higher selectivity under alkaline conditions, such as Figure 2 shown.
[0076] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a zero-valent iron biochar-based repair material, It is characterized in that The following steps are involved: (1) The collected corn stalks were washed with deionized water, dried for 24 hours, crushed and passed through a 20-mesh nylon sieve; (2) Put the crushed corn stalks into the carbonization tank and introduce nitrogen gas into the muffle furnace at a flow rate of 0.1m 3 / h, maintaining pyrolysis for 1.5 to 2.5 hours, collecting the black solid after cooling, washing, drying, and grinding through a 100-mesh nylon sieve to obtain corn straw biochar; (3) mixing the corn straw biochar with potassium ferrate, placing the mixture in a planetary ball mill, rotating forward for 15 minutes and reverse for 15 minutes, for a total of 30 minutes; (4) The mixed solid was placed in a muffle furnace for secondary calcination, and nitrogen gas was introduced at a flow rate of 0.1 m 3 / h, heated to 750°C to 850°C at a heating rate of 3°C / min to 7°C / min, maintained for 1.5 hours to 2.5 hours, collected the black solid after cooling, washed, dried and ground through a 100-mesh nylon sieve to obtain nano-zero-valent iron-loaded biochar.
2. A method for preparing a zero-valent iron biochar-based repair material according to claim 1, It is characterized in that The mass ratio of potassium ferrate to corn straw biochar is 0.2:1 to 0.8:
1.
3. The method for preparing a zero-valent iron biochar-based repair material according to claim 1, It is characterized in that The corn straw biochar is heated to 550° C. to 650° C. in a muffle furnace at a heating rate of 3° C. / min to 7° C. / min.
4. The method for preparing a zero-valent iron biochar-based repair material according to claim 1, It is characterized in that The rotation speed of the potassium ferrate and corn straw biochar mixture in the planetary ball mill is 400 to 600 r / min.
5. The method for preparing a zero-valent iron biochar-based repair material according to claim 1, It is characterized in that The nano-zero-valent iron biochar has a specific surface area of 50 to 200 m 2 / g, pore volume is 0.1 to 0.5cm 3 / g.
6. The method for preparing a zero-valent iron biochar-based repair material according to claim 1, It is characterized in that The content of zero-valent iron in the nano-zero-valent iron-loaded biochar is 10% to 20%.
7. A zero-valent iron biochar-based repair material, It is characterized in that It is prepared by the preparation method according to any one of claims 1 to 6.
8. A zero-valent iron biochar-based repair material according to claim 7, It is characterized in that The repair material has the ability to remove nitrates under the condition of pH value of 2 to 12.
9. The zero-valent iron biochar-based repair material according to claim 1, It is characterized in that The remediation material has a nitrate removal rate of 80% to 98%.
10. Use of the zero-valent iron biochar-based remediation material according to any one of claims 7 to 9 in removing nitrate pollution in water bodies.
Citation Information
Patent Citations
Graphitized porous biochar, and method for degrading organic pollutants in water body by using graphitized porous biochar
CN109292883A
Nanometer copper loaded Myriophyllum biochar, and preparation method and application thereof
CN110270304A
Long-term stable biochar-zero-valent iron composite material and one-step preparation method thereof
CN111569831A
Preparation method and application of highly graphitized biochar-based material
CN113307262A
Preparation method of efficient biomass derived carbon magnetic catalyst