Cerium-zirconium-neodymium-aluminum composite oxide carrier as well as preparation method and application thereof
The preparation of cerium, zirconium, neodymium aluminum composite oxide support was solved by step-by-step mixing method of cerium, zirconium, neodymium, aluminum composite oxide support was solved, and the particle size and chemical state of precious metal supported catalysts were achieved. The uniform dispersion and efficient catalytic activity of precious metal catalysts were achieved, which reduced the Preparation costs and water pollution.
Patent Information
- Application Number
- CN202411055486.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-08
AI Technical Summary
During the preparation process, existing precious metal-supported catalysts have problems such as difficult to control the particle size and chemical state of the active component, complex operation and water pollution, resulting in poor catalytic effect.
The cerium-zirconium-neodymium-aluminum composite oxide support is prepared by step-by-step mixing method, and the support is prepared by multiple grinding and calcination. After loading the precious metal, a uniformly dispersed catalyst is formed, which improves the catalytic oxidation activity and stability of CO.
The uniform dispersion of precious metal catalysts is achieved, with small particle size, high catalytic activity, and simple preparation process and low cost. The catalyst exhibits excellent catalytic activity and durability under conditions of 100°C to 300°C.
Smart Images

Figure CN118904325A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalysts and air pollution control, and specifically relates to a cerium-zirconium-neodymium-aluminum composite oxide carrier and a preparation method and application thereof. Background Art
[0002] The sintering flue gas in the steel industry contains a large amount of NO x Pollutants such as SO2, CO and solid particles are important gaseous pollutants in atmospheric environmental pollution, which cause great harm to health and the environment. Therefore, the removal of CO in sintering flue gas has important practical application value.
[0003] At present, there are many methods for treating CO, such as direct combustion, cryogenic separation, solution absorption, adsorption and catalytic oxidation. Among them, catalytic oxidation can convert CO and oxygen into carbon dioxide and water at a certain temperature. Compared with other CO treatment processes, catalytic oxidation has the advantages of large treatment capacity, high purification efficiency, no secondary pollution and high safety, making it a feasible sintering flue gas treatment technology.
[0004] The main method for removing CO in industry is catalytic oxidation, and its technical key and core lies in the appropriate catalyst. At present, CO oxidation catalysts are mainly divided into two categories: precious metal and non-precious metal catalysts. Common precious metal catalysts mainly include Pd, Pt, Au and multi-component precious metal catalysts. Precious metal catalysts often have better effects, but they are expensive. Usually, the active components are highly dispersed on the carrier to increase the catalytic active sites, thereby reducing the loading amount of precious metals to control the catalyst cost.
[0005] The commonly used methods for preparing noble metal supported catalysts at present are impregnation, deposition and reduction methods, etc., in which the active component precursor is loaded onto the carrier by impregnation, precipitation and reduction. However, the above-mentioned impregnation and deposition methods easily lead to uncontrollable size and chemical state of the active component metal particles, and the deposition method metal precursor solution is difficult to obtain, and the preparation process is complicated and cumbersome. The reduction method first adds a liquid phase reductant (such as hydrazine hydrate, etc.) to the noble metal source solution to obtain noble metal particles, and then loads the noble metal particles onto the carrier, which is complicated to operate, and the noble metal particle size and distribution are relatively uneven, resulting in poor catalytic effect, and the use of liquid phase reductants, prone to produce a large amount of wastewater, causing water pollution. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing a cerium-zirconium-neodymium-aluminum composite oxide carrier by a distributed mixing method, and the composite oxide prepared by the method, after being used as a catalyst carrier to load precious metals, the obtained catalyst active components have good dispersion and small particle size, can improve CO catalytic oxidation activity and stability, and the preparation method is simple and low-cost.
[0007] Another object of the present invention is to provide a noble metal supported catalyst based on the carrier and its application in CO catalytic oxidation reaction.
[0008] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0009] A method for preparing a cerium-zirconium-neodymium-aluminum composite oxide carrier, characterized in that a cerium precursor, a zirconium precursor, a neodymium precursor and an aluminum precursor are mixed and then calcined to obtain the carrier, comprising the following steps:
[0010] 1) grinding any one of the four precursors for the first time to obtain a first grinding material;
[0011] 2) mixing any one of the remaining three precursors with the first grinding material and grinding the mixture for a second time to obtain a second grinding material;
[0012] 3) mixing the remaining two precursors with the second grinding material and grinding them for a third time to obtain a third grinding material;
[0013] 4) mixing the remaining precursor with the third grinding material and grinding for a fourth time to obtain a fourth grinding material;
[0014] 5) calcining the fourth grind material to obtain the cerium-zirconium-neodymium-aluminum composite oxide support.
[0015] Preferably, the cerium precursor includes but is not limited to one or more of cerium sulfate, cerium acetate, cerium chloride, cerium acetate, cerium oxalate, cerium nitrate, ammonium cerium nitrate, cerium trioxide and cerium oxide; the zirconium precursor includes but is not limited to one or more of zirconium acetate, zirconium oxalate, zirconium nitrate, zirconium acetate, zirconium carbonate and zirconium oxide; the neodymium precursor includes but is not limited to one or more of neodymium chloride, neodymium nitrate, neodymium carbonate, neodymium sulfate, neodymium oxide, neodymium nitride, neodymium boride, neodymium iron boron and neodymium aluminum garnet; the aluminum precursor includes but is not limited to one or more of aluminum carbonate, basic aluminum carbonate, aluminum acetate, aluminum nitrate, aluminum chloride, aluminum oxalate, aluminum acetate and aluminum oxide.
[0016] Preferably, the cerium precursor, zirconium precursor, neodymium precursor and aluminum precursor are respectively added with solvents to form slurries for mixing and grinding, and the solvent in the slurry includes one or more of water, methanol, ethanol, acetonitrile, hexane, cyclohexane, acetone, benzene, toluene and chlorobenzene.
[0017] Furthermore, the first, second, third and fourth grindings are respectively performed by a planetary ball mill, the orbital speed of the planetary ball mill is 50-400 r / min, the rotation speed is 100-800 r / min, and the time is 0.05-24 h.
[0018] Preferably, the revolution speed of the first, second, third and fourth grinding is 100-300 r / min, and the rotation speed is 200-600 r / min.
[0019] Preferably, the particle size of the fourth abrasive is not greater than 5 μm.
[0020] Furthermore, the calcination temperature is 350-800°C, and the time is 10-600 min. Preferably, the calcination temperature is 400-550°C, and the time is 30-180 min.
[0021] The present invention also provides a cerium-zirconium-neodymium-aluminum composite oxide carrier prepared by the above preparation method.
[0022] Furthermore, the cerium-zirconium-neodymium-aluminum composite oxide carrier comprises the following components by mass percentage: 15-70% cerium oxide, 25-70% zirconium oxide, 5-60% aluminum oxide, and 0.5-10% neodymium oxide.
[0023] The present invention also provides a noble metal supported cerium zirconium neodymium aluminum composite oxide catalyst, comprising an active component and a carrier, wherein the active component is selected from one or more of the noble metals Pd, Pt, and Au, and the carrier is the cerium zirconium neodymium aluminum composite oxide carrier.
[0024] In the catalyst, the content of the noble metal is 0.1% to 5% by mass.
[0025] The present invention also provides the use of the noble metal supported cerium-zirconium-neodymium-aluminum composite oxide catalyst in CO catalytic oxidation reaction.
[0026] Beneficial effects: The method for preparing a cerium-zirconium-neodymium-aluminum composite oxide carrier by a step-by-step mixing method of the present invention is simple and low in cost. The prepared cerium-zirconium-neodymium-aluminum composite oxide is used as a precious metal catalyst carrier. After loading the active component, the precious metal is evenly dispersed and has a small particle size. The obtained catalyst has high CO catalytic oxidation activity. -1 ·h -1 ·g -1 Under high space velocity reaction conditions, it exhibits excellent catalytic activity and durability. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 TEM image of the cerium-zirconium-neodymium-aluminum composite oxide supported Pt-based catalyst prepared in Example 1.
[0028] Figure 2 Durability test of the Pt-based catalyst prepared in Example 1 in the CO catalytic combustion reaction. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is described in detail below through specific embodiments. However, it is necessary to point out that the following embodiments are only used to describe the content of the present invention and do not constitute a limitation on the protection scope of the present invention.
[0030] The method for preparing the cerium-zirconium-neodymium-aluminum composite oxide carrier according to the present invention uses four precursors, namely, a cerium precursor, a zirconium precursor, a neodymium precursor and an aluminum precursor, and comprises the following steps:
[0031] 1) grinding any one of the four precursors for the first time to obtain a first grinding material;
[0032] 2) mixing any one of the remaining three precursors with the first grinding material and grinding the mixture for a second time to obtain a second grinding material;
[0033] 3) mixing any one of the remaining two precursors with the second grinding material and grinding the mixture for a third time to obtain a third grinding material;
[0034] 4) mixing the remaining precursor with the third grinding material and grinding for a fourth time to obtain a fourth grinding material;
[0035] 5) calcining the fourth grinding material to obtain the cerium-zirconium-neodymium-aluminum composite oxide support.
[0036] In the present invention, the precursor is preferably a carbonate, acetate, bicarbonate, nitrate or metal oxide of the metal element.
[0037] The cerium precursor includes, but is not limited to, one or more of cerium sulfate, cerium acetate, cerium chloride, cerium acetate, cerium oxalate, cerium nitrate, ammonium cerium nitrate, cerium trioxide and cerium oxide; the zirconium precursor includes, but is not limited to, one or more of zirconium acetate, zirconium oxalate, zirconium nitrate, zirconium acetate, zirconium carbonate and zirconium oxide; the neodymium precursor includes, but is not limited to, one or more of neodymium chloride, neodymium nitrate, neodymium carbonate, neodymium sulfate, neodymium oxide, neodymium nitride, neodymium boride, neodymium iron boron and neodymium aluminum garnet; the aluminum precursor includes, but is not limited to, one or more of aluminum carbonate, basic aluminum carbonate, aluminum acetate, aluminum nitrate, aluminum chloride, aluminum oxalate, aluminum acetate and aluminum oxide.
[0038] When the precursors are mixed step by step in the present invention, any one of the four precursors is firstly ground for the first time to obtain a first grinding material.
[0039] In the present invention, the first grinding is preferably carried out in a planetary ball mill. The revolution speed of the first grinding is preferably 50 to 400 r / min, more preferably 100 to 300 r / min, the rotation speed is preferably 100 to 800 r / min, more preferably 200 to 600 r / min, and the time is preferably 0.05 to 24 h.
[0040] After obtaining the first grinding material, any one of the remaining three precursors is mixed with the first grinding material and then ground for a second time to obtain the second grinding material. After obtaining the second grinding material, any one of the remaining two precursors is mixed with the second grinding material and then ground for a third time to obtain the third grinding material. After obtaining the third grinding material, the last precursor is mixed with the third grinding material and then ground for a fourth time to obtain the fourth grinding material.
[0041] The second, third and fourth grindings are preferably carried out using a planetary ball mill, and the parameters such as the revolution and rotation speeds and time are consistent with the first grinding, but are carried out separately under independent conditions.
[0042] Preferably, after the fourth grinding, the particle size of the fourth grinding material is not greater than 5 μm.
[0043] Preferably, the cerium, zirconium, neodymium and aluminum precursors are mixed and ground in the form of a slurry, and the solvent used in the slurry includes, but is not limited to, one or more of water, methanol, ethanol, acetonitrile, hexane, cyclohexane, acetone, benzene, toluene and chlorobenzene.
[0044] Preferably, the solid-liquid ratio of the slurry is less than or equal to 1:20.
[0045] In the present invention, the order of adding the precursors is preferably: first add the cerium precursor, then add the zirconium precursor, then add the neodymium precursor, and finally add the aluminum precursor.
[0046] A preferred implementation method is that the precursor is added in the form of a slurry, first preparing a cerium precursor slurry, grinding the cerium precursor slurry for the first time to obtain a first grindstone, adding a zirconium precursor slurry for a second grinding, and then adding a neodymium precursor slurry to the obtained second grindstone for a third grinding to obtain a third grindstone, and finally adding an aluminum precursor slurry to the third grindstone for a fourth grinding to obtain a fourth grindstone.
[0047] After the fourth grind material is obtained, the fourth grind material is calcined to obtain the cerium-zirconium-neodymium-aluminum composite oxide support.
[0048] The fourth ground material is dehydrated and dried before being calcined. The specific method of dehydration and drying is not limited and can be a method well known to those skilled in the art.
[0049] The calcination temperature is preferably 350-800° C., more preferably 400-550° C., and the calcination time is preferably 10-600 min, more preferably 30-180 min.
[0050] The present invention also provides a cerium-zirconium-neodymium-aluminum composite oxide carrier prepared by the preparation method. The carrier comprises the following components in weight percentage: 15-70% cerium oxide, 25-70% zirconium oxide, 5-60% aluminum oxide, and 0.5-10% neodymium oxide. Preferably, 30-50% cerium oxide, 30-50% zirconium oxide, 2-7% neodymium oxide, and the rest is aluminum oxide.
[0051] The present invention also provides a noble metal supported cerium zirconium neodymium aluminum composite oxide catalyst, comprising an active component and a carrier, wherein the active component is selected from one or more of the noble metals Pd, Pt, and Au, and the carrier is the cerium zirconium neodymium aluminum composite oxide carrier.
[0052] In the above catalyst, the content of the noble metal is 0.1% to 5% by mass.
[0053] The catalyst can be prepared by adding the noble metal precursor and the carrier into a solvent, aging for a period of time, heating and stirring until the mixture is in a gelatinous state, and then drying; and calcining the obtained solid product to obtain a noble metal-loaded composite metal oxide catalyst.
[0054] In the preparation of the catalyst, the noble metal can be loaded, dried and calcined according to the known methods in the prior art to prepare a powder or a granular catalyst in various shapes, or the prepared slurry can be coated on a porous material such as a honeycomb or foam metal.
[0055] The catalyst obtained by loading the active component noble metal on the cerium-zirconium-neodymium-aluminum composite oxide carrier can be used as a catalyst in CO catalytic oxidation reaction.
[0056] In the following examples, the test method for the activity of the catalyst in the catalytic oxidation reaction of CO is as follows: 1% Pt is loaded on a cerium-zirconium-neodymium-aluminum composite oxide carrier, and the Pt-based catalyst loaded on the obtained cerium-zirconium-neodymium-aluminum composite oxide carrier is pressed, ground, and sieved to obtain 40-60 mesh catalyst small particles. Weigh 0.035g and put it into a quartz tube with an inner diameter of 9mm, and the quartz tube is placed in an electric heating furnace. Use cylinder gas to simulate a CO-containing simulated mixed gas, and the composition of the inlet reaction gas is: O2=21%, CO=5000ppm, N2 balance gas. 300mL / min of the simulated mixed gas is passed into the quartz tube containing the catalyst, and the CO concentration in the outlet gas is analyzed by online chromatography. The reaction temperature of the test is 100-300℃; the air velocity is about 510000mL·g -1 ·h -1The reaction temperature T50 or T90 when the CO conversion rate reaches 50% or 90% is mainly used as the catalyst activity index (the lower the value of T50 or T90, the better the catalyst activity).
[0057] Example 1
[0058] A preparation method of a cerium-zirconium-neodymium-aluminum composite oxide carrier and a Pt-based catalyst is as follows:
[0059] Weigh 23.4g of cerium carbonate, add 117g of water and stir into a slurry, and grind the slurry in a planetary ball mill (model XQM-0.4A) with an orbital speed of 200r / min and a rotation speed of 400r / min for 0.5h. Thereafter, add a pre-configured slurry containing 24.59g of zirconium carbonate and 123g of water to the cerium carbonate slurry, and continue to grind for 0.5h in a planetary ball mill with an orbital speed of 200r / min and a rotation speed of 400r / min after mixing. Then, add a pre-configured slurry containing 2.84g of neodymium nitrate and 1.2g of water, and continue to grind the mixed slurry in a planetary ball mill with an orbital speed of 200r / min and a rotation speed of 400r / min for 0.5h. Finally, a slurry containing 1.75g of aluminum oxide and 8.75g of water was added, and the mixed slurry was further ground for 0.5h in a planetary ball mill with a revolution speed of 200r / min and a rotation speed of 400r / min, until the particle size of the ground material was no more than 5μm. After the grinding was completed, the cerium-zirconium-neodymium-aluminum composite oxide carrier was obtained after drying at 110°C and calcining at 500°C (180min), wherein the mass contents of cerium oxide, zirconium oxide and neodymium oxide were 50%, 35% and 5% respectively, and aluminum oxide was 10%.
[0060] The carrier is ground, platinum nitrate and deionized water are added, Pt accounts for 1% of the total mass of the catalyst, stirred at room temperature (25°C) for 12 hours, and the mixed solution is heated to 80°C until it is boiled dry; the material is dried in a drying oven at 110°C for 12 hours, and then heated to 450°C at 5°C / min and calcined for 2 hours. After the temperature drops to room temperature, it is taken out to obtain a Pt-based catalyst supported on a cerium-zirconium-neodymium-aluminum composite oxide carrier.
[0061] TEM images of the prepared cerium-zirconium-neodymium-aluminum composite oxide support supported on Pt-based catalysts are shown in Figure 2. Figure 1 As shown in the figure, it can be seen that the active component Pt has good dispersion and its average particle size is 2.1nm.
[0062] Example 2
[0063] The method for synthesizing a cerium-zirconium-neodymium-aluminum composite oxide carrier and a Pt-based catalyst based on the carrier is as follows:
[0064] Weigh a certain amount of cerium carbonate, add an appropriate amount of water and stir to form a slurry, and grind the slurry in a planetary ball mill (orbital speed of 200r / min, rotation speed of 400r / min) for 0.5h. Thereafter, add the pre-prepared zirconium carbonate slurry to the cerium carbonate slurry, and continue to grind the mixed slurry in the planetary ball mill for 0.5h. Then, add the neodymium nitrate slurry, and continue to grind the mixed slurry in the planetary ball mill for 0.5h. Finally, add the alumina slurry, and continue to grind the mixed slurry in the planetary ball mill for 0.5h. After grinding, the particle size of the grinding material is no more than 5μm, and the cerium zirconium neodymium aluminum composite oxide carrier is obtained after drying at 110°C and calcining at 500°C (180min).
[0065] The prepared carrier was ground, and platinum nitrate and deionized water were added to control Pt to account for 1% of the total mass of the catalyst. The mixture was stirred at room temperature for 12 hours, and then the mixed solution was heated to 80°C until it was boiled dry. The material was placed in a drying oven at 110°C and dried for 12 hours, and then the temperature was raised to 450°C at 5°C / min and calcined for 2 hours. After the temperature was lowered to room temperature, the catalyst was taken out to obtain a Pt-based catalyst supported on a cerium-zirconium-neodymium-aluminum composite oxide carrier.
[0066] Carriers and catalysts with different cerium-zirconium-neodymium-aluminum contents were prepared, and the catalyst activity was tested. Table 1 shows the catalysts with different cerium-zirconium-neodymium-aluminum contents and their activity data in the CO catalytic combustion reaction. As shown in Table 1, good catalytic effects were achieved on cerium-zirconium-neodymium-aluminum composite oxide catalysts with a cerium oxide mass content of 30-50%, a zirconium oxide mass content of 30-50%, and a neodymium oxide mass content of 2-7%. The Pt-based catalyst supported on a cerium-zirconium-neodymium-aluminum composite oxide carrier with a cerium oxide mass content of 50%, a zirconium oxide mass content of 35%, a neodymium oxide mass content of 5%, and an aluminum oxide mass content of 10% obtained the best catalytic activity.
[0067] Table 1 Catalysts with different Cerium-Zirconium-NdAl contents in the carrier and their activities in CO catalytic oxidation reaction
[0068]
[0069] Example 3
[0070] The cerium zirconium neodymium aluminum composite oxide carrier was prepared by different mixing methods and sequences, and a loaded Pt-based catalyst was prepared to test its activity in the catalytic combustion reaction of CO. In the preparation of the catalyst, the cerium zirconium neodymium aluminum composite oxide carrier contained 50% cerium oxide, 35% zirconium oxide, 5% neodymium oxide and 10% aluminum oxide by mass, and the method of loading Pt on the carrier was the same as that in Example 1.
[0071] Different methods for preparing the vector are as follows:
[0072] (1) Step-by-step wet mixing followed by calcination
[0073] The preparation method is the same as that in Example 1.
[0074] (2) Dry mixing and calcination in steps
[0075] S1: Preparing dry powders of precursors cerium carbonate, zirconium carbonate, neodymium nitrate and aluminum oxide respectively.
[0076] S2: The dry material of the cerium precursor prepared in step S1 is placed in a planetary ball mill with an orbital speed of 200 r / min and an autorotational speed of 400 r / min and ground for 0.5 h.
[0077] S3: Add the dry material of zirconium precursor to the material obtained in step S2, and grind it in a planetary ball mill with an orbital speed of 200 r / min and an autorotation speed of 400 r / min for 0.5 h.
[0078] S4: Add the dry material of the neodymium precursor to the material obtained in step S3, and grind it in a planetary ball mill with an orbital speed of 200 r / min and an autorotation speed of 400 r / min for 0.5 h.
[0079] S5: Add the dry material of aluminum precursor to the material obtained in step S4, and grind it in a planetary ball mill with an orbital speed of 200 r / min and an autorotation speed of 400 r / min for 0.5 h.
[0080] S6: The material obtained in step S5 is calcined at 500° C. for 180 min to obtain a cerium-zirconium-neodymium-aluminum composite oxide carrier.
[0081] In contrast, the precursors were calcined and then mixed in steps, specifically:
[0082] (3) Wet mixing in steps after calcination
[0083] S1: Preparing dry powders of precursors cerium carbonate, zirconium carbonate, neodymium nitrate and aluminum oxide respectively.
[0084] S2: The powdered dry materials of the cerium precursor, zirconium precursor, neodymium precursor and aluminum precursor in step S1 are calcined at 500° C. for 180 min to obtain respective metal oxides, and then water is added to prepare slurries respectively.
[0085] S3: The cerium oxide slurry obtained in step S2 is placed in a planetary ball mill with an orbital speed of 200 r / min and an autorotational speed of 400 r / min and ground for 0.5 h.
[0086] S4: Add the zirconium oxide slurry obtained in step S2 to the material obtained in step S3, and grind for 0.5 h in a planetary ball mill with an orbital speed of 200 r / min and an autorotation speed of 400 r / min.
[0087] S5: Add the slurry of neodymium oxide obtained in step S2 to the material obtained in step S4, and grind for 0.5 h in a planetary ball mill with an orbital speed of 200 r / min and an autorotation speed of 400 r / min.
[0088] S6: Add the aluminum oxide slurry obtained in step S2 to the material obtained in step S5, and grind for 0.5 h in a planetary ball mill with an orbital speed of 200 r / min and an autorotation speed of 400 r / min.
[0089] S7: The material obtained in step S6 is dried at 110° C. for 12 hours and then calcined at 500° C. for 180 minutes to obtain a cerium-zirconium-neodymium-aluminum composite oxide carrier.
[0090] (4) Dry mixing in steps after calcination
[0091] S1: Preparing dry powders of precursors cerium carbonate, zirconium carbonate, neodymium nitrate and aluminum oxide respectively.
[0092] S2: The powdered dry materials of the cerium precursor, zirconium precursor, neodymium precursor and aluminum precursor in step S1 are calcined at 500° C. for 180 min to obtain powdered dry materials of each metal oxide.
[0093] S3: The dry cerium oxide obtained in step S2 is placed in a planetary ball mill with an orbital speed of 200 r / min and an autorotation speed of 400 r / min and ground for 0.5 h.
[0094] S4: Add dry zirconium oxide to the material obtained in step S3, and grind for 0.5 h in a planetary ball mill with an orbital speed of 200 r / min and an autorotation speed of 400 r / min.
[0095] S5: Add dry neodymium oxide to the material obtained in step S4, and grind for 0.5 h in a planetary ball mill with an orbital speed of 200 r / min and an autorotation speed of 400 r / min.
[0096] S6: Add dry aluminum oxide to the material obtained in step S5, and grind for 0.5 h in a planetary ball mill with an orbital speed of 200 r / min and an autorotation speed of 400 r / min.
[0097] S7: The material obtained in step S6 is calcined at 500° C. for 180 min to obtain a cerium-zirconium-neodymium-aluminum composite oxide carrier.
[0098] Table 2 shows the Pt-based catalysts supported on the cerium-zirconium-neodymium-aluminum composite oxide carrier obtained by different preparation methods and their catalytic activities for CO, as well as the Pt particle size (CO pulse analysis) on different catalysts, the H2-TPR minimum reduction peak temperature (α peak position) and its effect on the catalytic activity of CO catalytic combustion reaction. As shown in Table 2, among the Pt-based catalysts prepared by different preparation methods, the catalyst obtained by step-by-step wet mixing and calcination has a Pt particle size of 2.1nm and a H2-TPR minimum reduction peak temperature (α peak position) of 105°C, and the corresponding CO catalytic combustion reaction activity is the best, with T50 of 110°C and T90 of 150°C; step-by-step dry mixing and calcination is second. The catalyst prepared by step-by-step dry mixing after calcination has the largest Pt particle size and H2-TPR minimum reduction peak temperature (α peak position), which are 3.7nm and 120℃ respectively, and its corresponding CO catalytic combustion reaction activity is the worst, with T50 of 137℃ and T90 of 211℃; the catalyst prepared by step-by-step wet mixing after calcination is better than step-by-step dry mixing after calcination, but the Pt particle size, H2-TPR minimum reduction peak temperature (α peak position) and activity are significantly different from those of the step-by-step mixing and calcination method. It can be seen that a catalyst with high dispersion and H2 reduction ability can be prepared by using a suitable preparation method, and thus produces good catalytic activity.
[0099] Table 2 Ce-Zr-Nd-Al composite oxide catalysts prepared by different methods and their catalytic oxidation activity for CO
[0100] Preparation method Pt particle size (nm) α peak position (℃) T50(℃) T90(℃) Step-by-step wet mixing followed by calcination 2.1 105 110 150 Dry mixing followed by calcination 2.9 114 129 161 After roasting, wet mixing in steps 3.6 116 134 204 Dry mixing in steps after calcination 3.7 120 137 211
[0101] Example 4
[0102] Different precursors were used to prepare cerium-zirconium-neodymium-aluminum composite oxide supports and loaded Pt-based catalysts.
[0103] According to the "step-by-step wet mixing" method of Example 1, carbonates, acetates, oxalates and nitrates of cerium, zirconium and neodymium are used as precursors, respectively, and the mass contents of cerium oxide, zirconium oxide and neodymium oxide in the cerium-zirconium-neodymium-aluminum composite oxide carrier after calcination are controlled to be 50%, 35% and 5%, respectively, and the balance is alumina. Table 3 shows the Pt-based catalysts loaded on the cerium-zirconium-neodymium-aluminum composite oxide carrier obtained from different precursors and their effects on CO catalytic activity. It can be seen from Table 3 that the cerium-zirconium-neodymium-aluminum composite oxide carriers prepared using different precursors have different properties. In general, carbonate>acetate>nitrate>oxalate. In addition, the change patterns of properties such as Pt particle size and H2-TPR minimum reduction peak temperature are basically consistent with the change patterns of their activity for CO catalytic combustion reaction.
[0104] Table 3 Ce-Zr-Nd-Al composite oxide catalysts obtained from different precursors and their catalytic oxidation activity for CO
[0105]
[0106]
[0107] Example 5
[0108] Example 5 The durability of the catalyst prepared according to the preparation method of Example 1 for the catalytic combustion reaction of CO at 200°C was tested, wherein the mass contents of cerium oxide, zirconium oxide and neodymium oxide in the cerium-zirconium-neodymium-aluminum composite oxide support were 50%, 35% and 5%, respectively, and the balance was aluminum oxide. The results are as follows: Figure 2 As shown in the figure, within the 100h test, the activity of the catalyst for CO catalytic combustion remained at nearly 100%, and no obvious catalyst activity decay was found, indicating that the catalyst has good durability.
[0109] Comparative Example 1
[0110] The cerium-zirconium-neodymium-aluminum composite oxide carrier is prepared by a "one-step wet mixing" and then calcining method. The specific preparation method is as follows:
[0111] Weigh a certain amount of cerium carbonate, zirconium carbonate, neodymium oxide and aluminum oxide, add appropriate amount of water and stir into slurry, respectively, to obtain slurries of precursors cerium carbonate, zirconium carbonate, neodymium oxide and aluminum oxide. Mix these four precursor slurries together and grind them for 1.5 hours in a planetary ball mill with an orbital speed of 200r / min and a rotation speed of 400r / min. After grinding, dry at 110°C and calcine at 500°C (180min) to obtain a cerium-zirconium-neodymium-aluminum composite oxide carrier. Load 1% Pt on the carrier in the same way as in Example 1 to obtain a catalyst for CO catalytic oxidation.
[0112] The Pt-based catalysts supported on the cerium-zirconium-neodymium-aluminum composite oxide carriers prepared in Comparative Example 1 and Example 1 were applied to the CO catalytic combustion reaction, and their catalytic performance was measured, and the results are shown in Table 4. As can be seen from Table 4, the activity of the catalyst prepared by the preparation method of "step-by-step wet mixing" followed by calcination in Example 1 is significantly better than that of the preparation method of "one-step wet mixing" followed by calcination.
[0113] Table 4 CO catalytic activity of Pt-based catalysts prepared by different methods
[0114] Preparation method Grinding time T50(℃) T90(℃) Comparative Example 1 1.5h 142 202 Example 1 0.5h+0.5h+0.5h 110 150
[0115] The above description is only a preferred embodiment of the present invention, and does not limit the present invention in any substantial or formal sense. It should be noted that, for a person skilled in the art, several improvements can be made without departing from the purpose of the present invention, and these improvements should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing a cerium-zirconium-neodymium-aluminum composite oxide carrier, characterized in that: The method is prepared by mixing a cerium precursor, a zirconium precursor, a neodymium precursor and an aluminum precursor and then calcining the mixture, and comprises the following steps: 1) grinding any one of the four precursors for the first time to obtain a first grinding material; 2) mixing any one of the remaining three precursors with the first grinding material and grinding the mixture for a second time to obtain a second grinding material; 3) mixing the remaining two precursors with the second grinding material and grinding them for a third time to obtain a third grinding material; 4) mixing the remaining precursor with the third grinding material and grinding for a fourth time to obtain a fourth grinding material; 5) calcining the fourth abrasive material to obtain the cerium-zirconium-neodymium-aluminum composite oxide support.
2. The method for preparing the cerium-zirconium-neodymium-aluminum composite oxide support according to claim 1, characterized in that: The cerium precursor is selected from one or more of cerium sulfate, cerium acetate, cerium chloride, cerium acetate, cerium oxalate, cerium nitrate, ammonium cerium nitrate, cerium trioxide and cerium oxide; the zirconium precursor is selected from one or more of zirconium acetate, zirconium oxalate, zirconium nitrate, zirconium acetate, zirconium carbonate and zirconium oxide; the neodymium precursor is selected from one or more of neodymium chloride, neodymium nitrate, neodymium carbonate, neodymium sulfate, neodymium oxide, neodymium nitride, neodymium boride, neodymium iron boron and neodymium aluminum garnet; the aluminum precursor is selected from one or more of aluminum carbonate, basic aluminum carbonate, aluminum acetate, aluminum nitrate, aluminum chloride, aluminum oxalate, aluminum acetate and aluminum oxide.
3. The method for preparing the cerium-zirconium-neodymium-aluminum composite oxide support according to claim 1, characterized in that: The cerium precursor, zirconium precursor, neodymium precursor and aluminum precursor are respectively added with solvents to prepare slurries for mixing and grinding.
4. The method for preparing the cerium-zirconium-neodymium-aluminum composite oxide support according to claim 1, characterized in that: The grinding is carried out using a planetary ball mill, the orbital speed of the planetary ball mill is 50-400 r / min, the rotation speed is 100-800 r / min, and the time is 0.05-24 h.
5. The method for preparing the cerium-zirconium-neodymium-aluminum composite oxide support according to claim 1, characterized in that: The particle size of the fourth abrasive is no greater than 5 μm.
6. The method for preparing the cerium-zirconium-neodymium-aluminum composite oxide support according to claim 1, characterized in that: The calcination temperature is 350-800° C. and the calcination time is 10-600 min.
7. A cerium-zirconium-neodymium-aluminum composite oxide support obtained according to the method for preparing a cerium-zirconium-neodymium-aluminum composite oxide support according to any one of claims 1 to 6.
8. The cerium-zirconium-neodymium-aluminum composite oxide support according to claim 7, characterized in that: Calculated by mass percentage, it contains 15-70% cerium oxide, 25-70% zirconium oxide, 5-60% aluminum oxide, and 0.5-10% neodymium oxide.
9. A noble metal supported cerium-zirconium-neodymium-aluminum composite oxide catalyst, characterized in that: It comprises an active component and a carrier, wherein the active component is selected from one or more of the noble metals Pd, Pt and Au, and the carrier is the cerium-zirconium-neodymium-aluminum composite oxide carrier as described in claim 7.
10. Use of the noble metal supported cerium-zirconium-neodymium-aluminum composite oxide catalyst according to claim 9 in a CO catalytic oxidation reaction.
Citation Information
Patent Citations
Aluminum-cerium-zirconium based composite oxide catalytic material and preparation method thereof
CN102962047A
Ce-Zr-Al-based composite oxide rare earth oxygen-storage material and preparation method thereof
CN103084161A
Cerium-zirconium-aluminium-based composite oxide catalytic material and preparation method thereof
CN103349978A
Preparation method of ternary tail gas catalyst
CN105797708A
Low-temperature high-effective mesoporous Ce-Zr-Al composite oxide supported noble metal nano catalyst, preparation method, and application thereof