Ruthenium-based catalyst for preferential oxidation of carbon monoxide and preparation method of ruthenium-based catalyst
Ruthenium-based catalysts were prepared by chemical reduction. By combining titanium dioxide support and reducing agent, the problem of high temperature in the preferential oxidation reaction of carbon monoxide was solved, achieving efficient CO conversion over a wide temperature range and promoting the development of proton exchange membrane fuel cells.
Patent Information
- Application Number
- CN202310506735.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-08
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing ruthenium-based catalysts suffer from high optimal reaction temperatures in the preferential oxidation of carbon monoxide, making it difficult to achieve efficient CO conversion over a wide temperature range and limiting their application in proton exchange membrane fuel cells.
Ruthenium-based catalysts were prepared by chemical reduction using titanium dioxide as a support. By adding a reducing agent and controlling the calcination process, ruthenium was uniformly dispersed, forming a strong metal-support interaction, which improved the low-temperature activity and stability of the catalyst.
It achieves efficient CO removal over a wide temperature range (70-210℃), significantly improving the catalyst's activity and stability, and is suitable for the application requirements of proton exchange membrane fuel cells.
Smart Images

Figure CN118904330A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, and in particular to a titanium dioxide-supported ruthenium catalyst for preferential oxidation of carbon monoxide and a preparation method thereof. Background Art
[0002] Hydrogen energy is a secondary energy source with the advantages of abundant sources, green and low carbon, and huge development potential and development market. With the increase in market demand, the development and utilization of H2 has become an important theme in line with the development of the times. An important application of H2 is as a fuel for proton exchange membrane fuel cells (PEMFC). PEMFC has the advantages of being environmentally friendly, high energy conversion efficiency, and no pollutant emissions. It is in a booming stage in various fields, especially in the transportation field, and is one of the main development directions of new energy clean power vehicles in the future. At present, the industrial production technology route of H2 is mainly to reform hydrogen from fossil energy, and the produced H2 contains about 10% CO. However, even if there is only a trace amount of CO, it will seriously poison the platinum electrode, thereby reducing the battery performance and service life, and restricting the development and popularization of PEMFC. Therefore, before H2 enters PEMFC, it is necessary to remove the trace CO in it so that it meets the application requirements of PEMFC and ensures the normal operation of the battery.
[0003] The preferential oxidation of carbon monoxide is an important method for eliminating trace amounts of CO in H2. At present, catalysts for the preferential oxidation of carbon monoxide are mainly based on precious metal platinum, gold and ruthenium. Among them, the price of ruthenium-based catalyst raw materials is relatively low, and CO can be completely eliminated by simultaneously catalyzing the CO oxidation and methanation reactions during the preferential oxidation of carbon monoxide. However, the catalyst has the problem of a high optimal reaction temperature. Therefore, it is an urgent goal to provide an efficient ruthenium-based catalyst for the preferential oxidation of carbon monoxide with excellent low-temperature activity and a wide CO complete conversion temperature range. Summary of the invention
[0004] The purpose of the present invention is to overcome the deficiencies of the prior art and to provide a ruthenium-based catalyst for the preferential oxidation of carbon monoxide and a method for preparing the same. The catalyst has the characteristics of high activity and high stability. The method has a simple process, good reliability, strong repeatability and high universality.
[0005] The technical purpose of the present invention is achieved through the following technical solutions.
[0006] A ruthenium-based catalyst for preferential oxidation of carbon monoxide and a preparation method thereof. The synthesis method (preparation method) of the catalyst is a chemical reduction method. The catalyst is composed of a ruthenium active component and a titanium dioxide carrier. The ruthenium content is 0.05-5wt%, preferably 0.5-5wt%, based on the total mass of the catalyst. The steps are as follows:
[0007] Step 1, dispersing a ruthenium precursor in water to form a uniform solution, adding a titanium dioxide carrier, and stirring to form a uniform suspension, marking the suspension as A;
[0008] In step 1, the ruthenium precursor is selected from ruthenium trichloride, ruthenium nitrosyl nitrate, ruthenium acetate, ruthenium acetate or ruthenium acetylacetonate.
[0009] In step 1, the stirring is selected by mechanical stirring or magnetic stirring, and the speed is 300-500 revolutions per minute.
[0010] Step 2, adding a reducing agent to the suspension obtained in step 1, heating and stirring, to obtain a new suspension, marked as suspension B; the molar ratio of the reducing agent to ruthenium is (1-4):1;
[0011] In step 2, the reducing agent is sodium borohydride, potassium borohydride, formic acid or hydrazine hydrate, and the reducing agent is added to the suspension obtained in step 1 in the form of an aqueous solution thereof.
[0012] In step 2, the molar ratio of the reducing agent to ruthenium is (1-3):1.
[0013] In step 2, the reaction time after adding the reducing agent is 1-5 hours, preferably 3-5 hours, so that the ruthenium precursor and the reducing agent can fully react; the heating temperature is 60-90°C, and the stirring is mechanical stirring or magnetic stirring at a speed of 300-500 revolutions per minute.
[0014] Step 3, after solid-liquid separation of the suspension obtained in step 2, the obtained solid material is washed and dried, and then roasted, and then the roasted material is reduced to obtain a ruthenium-based catalyst for preferential oxidation of carbon monoxide; when roasting, the roasting temperature is 200-500°C, the roasting time is 1-5 hours, and the roasting atmosphere is air or an inert protective gas; when reducing, the reduction temperature is 200-600°C, the reduction time is 1-5 hours, and the reducing atmosphere is a mixed gas of carbon monoxide and an inert protective atmosphere, or a mixed gas of hydrogen and an inert protective atmosphere.
[0015] In step 3, during the calcination, the temperature is raised from room temperature 20-25 degrees Celsius at a rate of 5-10 degrees Celsius per minute to the calcination temperature of 200-300°C, the calcination time is 3-5 hours, and after calcination, it is naturally cooled to room temperature.
[0016] In step 3, during reduction, the temperature is raised from room temperature 20-25 degrees Celsius to the reduction temperature at a rate of 5-10 degrees Celsius per minute, the reduction temperature is 200-400°C, the reduction time is 1-3 hours, and the carbon monoxide preferential oxidation reaction is directly carried out after reduction.
[0017] In step 3, the inert protective gas is nitrogen, helium or argon.
[0018] In step 3, in the mixed gas of carbon monoxide and inert protective atmosphere, the volume percentage of carbon monoxide is 5-10%; in the mixed gas of hydrogen and inert protective atmosphere, the volume percentage of hydrogen is 8-12%.
[0019] The catalyst of the present invention is used for the carbon monoxide preferential oxidation reaction, shows excellent low-temperature activity and high stability, and can effectively eliminate CO in a wide temperature range. The active component Ru is highly dispersed, the metal utilization rate is high, and the catalyst significantly improves the activity of the carbon monoxide preferential oxidation reaction.
[0020] Compared with the prior art, the present invention uses titanium dioxide as a carrier and prepares a catalyst by a chemical reduction method. During the synthesis process, a reducing agent is used to pre-reduce the active component ruthenium, which effectively promotes the uniform dispersion of the active component ruthenium and improves the activity of the catalyst, thereby promoting the development and wide application of PEMFC. The catalyst preparation method provided by the present invention is simple to operate, reliable, highly repeatable, uses less ruthenium, is simple to prepare, has low cost, is easy to repeat, has good stability, significantly improves the activity of carbon monoxide preferential oxidation, is conducive to large-scale production and use, and has good prospects for promoting the wide application of proton exchange membrane fuel cells. The catalyst provided by the present invention has highly dispersed Ru and excellent stability, and high metal utilization. The catalyst provided by the present invention is used for the preferential oxidation reaction of carbon monoxide, and can achieve complete elimination of CO in a wide temperature range, so that the H2 in the raw material is suitable for the application requirements of PEMFC. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is the CO conversion curve of the 0.05RuTi-R200 catalyst prepared in Example 1 for the preferential oxidation of carbon monoxide.
[0022] Figure 2 This is the CO conversion curve of the 0.3RuTi-R200 catalyst prepared in Example 2 for the preferential oxidation of carbon monoxide.
[0023] Figure 3 This is the CO conversion curve of the 0.5RuTi-R200 catalyst prepared in Example 3 for the preferential oxidation of carbon monoxide.
[0024] Figure 4 This is the CO conversion curve of the 0.5RuTi-R400 catalyst prepared in Example 4 for the preferential oxidation of carbon monoxide.
[0025] Figure 5 This is the CH4 selectivity curve for the preferential oxidation of carbon monoxide using the 0.5RuTi-R600 catalyst prepared in Example 5.
[0026] Figure 6 This is the CO conversion curve of the 1RuTi-R600 catalyst prepared in Example 6 for the preferential oxidation of carbon monoxide.
[0027] Figure 7 This is the CO conversion curve of the 1.5RuTi-R200 catalyst prepared in Example 7 for the preferential oxidation of carbon monoxide.
[0028] Figure 8 This is the CO conversion curve of the 2RuTi-R200 catalyst prepared in Example 8 for the preferential oxidation of carbon monoxide.
[0029] Fig. 9 This is the CO conversion curve of the 5RuTi-R200 catalyst prepared in Example 9 for the preferential oxidation of carbon monoxide.
[0030] Fig.10 The XPS spectra of the catalysts prepared in Example 3 and Comparative Example 1 in the C1s and Ru 3d regions.
[0031] Fig.11 In-situ DRIFTS spectra of CO adsorption of the catalysts prepared in Example 3 and Comparative Example 1 at 90°C. DETAILED DESCRIPTION
[0032] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0033] Example 1
[0034] Preparation of Ru-based catalyst: According to the theoretical loading of 0.05wt%, weigh 0.0005g of nitrosyl ruthenium nitrate precursor with a metal Ru content of 70mL, dissolve it in 70mL of water, and stir to mix evenly. Weigh 0.999g of TiO2 powder, add it to the mixed solution, and stir to form a mixed suspension. Weigh potassium borohydride with a molar ratio of 1 to the Ru, dissolve it in water to form a solution, and add the solution to the above suspension, and heat and stir at 60°C for 3h. The suspension is filtered or centrifuged to obtain a solid material, and the solid is washed. The treated solid is dried in a 70°C oven for 12h, and then calcined in a tubular furnace at 200°C in an air atmosphere for 3h to obtain the catalyst 0.05RuTi. The catalyst is reduced at 200°C in a CO / N2 atmosphere (5% CO, 95% N2 by volume) for 1h to obtain 0.05RuTi-R200 (reduction temperature 200 degrees Celsius).
[0035] The catalyst is used for the preferential oxidation reaction of carbon monoxide. 0.1 g of the catalyst (40-60 mesh) prepared in Example 1 is taken and loaded into a fixed bed quartz tube reactor. The reaction tube used is 50 cm long and has an inner diameter of 8 mm. The raw gas composition of the preferential oxidation reaction of carbon monoxide is: 1% CO, 1% O2, 50% H2, 48% N2 (this gas composition simulates the components of the gas in the proton exchange membrane fuel cell, volume percentage), the reaction temperature is 50-210°C (the operating temperature of the proton exchange membrane fuel cell is about 80-180 degrees. In order to characterize the performance of the catalyst of the present invention, the upper and lower limits are appropriately expanded based on this reaction temperature range), and the reaction mass space velocity is 60000 mL·h -1 ·g cat -1 The raw gas and reaction tail gas were analyzed online using Agilent 7890A gas chromatograph. Figure 1 As shown, the CO conversion rate of 0.05RuTi-R200 reaches the highest at 190°C, which is 51%.
[0036] Example 2
[0037] Preparation of Ru-based catalyst: According to the theoretical loading of 0.3wt%, weigh 0.003g of ruthenium acetate precursor with a metal Ru content, dissolve it in 70mL of water, and stir to mix evenly. Weigh 0.997g TiO2 powder, add it to the mixed solution, and form a mixed suspension at room temperature. Weigh formic acid with a molar ratio of 4 to the Ru, dissolve it in water to form a solution, and add the aqueous solution to the above suspension, and heat and stir at 90°C for 3h. The suspension is filtered or centrifuged to obtain a solid material, and the solid is washed. The treated solid is dried in a 70°C oven for 12h, and then calcined in a tubular furnace at 500°C in a nitrogen atmosphere for 3h to obtain the catalyst 0.3RuTi. The catalyst is reduced at 200°C for 1h in a H2 / N2 atmosphere (volume percentage 8% H2, 92% N2, the same below) to obtain 0.3RuTi-R200.
[0038] The catalyst is used for the carbon monoxide preferential oxidation reaction. 0.1 g of the catalyst (40-60 mesh) prepared in Example 2 is taken and loaded into a fixed bed quartz tube reactor. The reaction tube used is 50 cm long and has an inner diameter of 8 mm. The raw gas composition of the carbon monoxide preferential oxidation reaction is: 1% CO, 1% O2, 50% H2, 48% N2, the reaction temperature is 50-210°C, and the reaction mass space velocity is 60000 mL·h -1 ·g cat -1 The raw gas and reaction tail gas were analyzed online using Agilent 7890A gas chromatograph. Figure 2As shown, the CO conversion of 0.3RuTi-R200 reaches 100% at 150°C.
[0039] Example 3
[0040] Preparation of Ru-based catalyst: According to the theoretical loading of 0.5wt%, weigh 0.005g of ruthenium trichloride precursor with a metal Ru content, dissolve it in 70mL of water, and stir to mix evenly. Weigh 0.995g of TiO2 powder, add it to the mixed solution, and stir to form a mixed suspension. Weigh sodium borohydride with a molar ratio of 1.5 to the Ru, dissolve it in water to form a solution, and add the solution to the above suspension, and heat and stir at 90°C for 3h. The suspension is filtered or centrifuged to obtain a solid material, and the solid is washed. The treated solid is dried in a 70°C oven for 12h, and then calcined in a tubular furnace at 300°C in a nitrogen atmosphere for 3h to obtain the catalyst 0.5RuTi. The catalyst is reduced at 200°C in a H2 / N2 atmosphere for 1h to obtain 0.5RuTi-R200.
[0041] The catalyst is used for the carbon monoxide preferential oxidation reaction. 0.1 g of the catalyst (40-60 mesh) prepared in Example 3 is taken and loaded into a fixed bed quartz tube reactor. The reaction tube used is 50 cm long and 8 mm in inner diameter. The raw gas composition of the carbon monoxide preferential oxidation reaction is: 1% CO, 1% O2, 50% H2, 48% N2, the reaction temperature is 50-210°C, and the reaction mass space velocity is 60000 mL·h -1 ·g cat -1 The raw gas and reaction tail gas were analyzed online using Agilent 7890A gas chromatograph. Figure 5 As shown in Figure 5, the CO conversion of 0.5RuTi-R200 reaches 100% at 90 °C, and 100% CO conversion is achieved in the temperature range of 90–150 °C.
[0042] Example 4
[0043] Preparation of Ru-based catalyst: According to the theoretical loading of 0.5wt%, weigh 0.005g of ruthenium trichloride precursor with a metal Ru content, dissolve it in 70mL of water, and stir to mix evenly. Weigh 0.995g of TiO2 powder, add it to the mixed solution, and stir to form a mixed suspension. Weigh sodium borohydride with a molar ratio of 1.5 to the Ru, dissolve it in water to form a solution, and add the solution to the above suspension, and heat and stir at 90°C for 3h. The suspension is filtered or centrifuged to obtain a solid material, and the solid is washed. The treated solid is dried in a 70°C oven for 12h, and then calcined in a tubular furnace at 300°C in a nitrogen atmosphere for 3h to obtain the catalyst 0.5RuTi. The catalyst is reduced at 400°C in a H2 / N2 atmosphere for 1h to obtain 0.5RuTi-R400.
[0044] The catalyst is used for the carbon monoxide preferential oxidation reaction. 0.1 g of the catalyst (40-60 mesh) prepared in Example 4 is taken and loaded into a fixed bed quartz tube reactor. The reaction tube used is 50 cm long and 8 mm in inner diameter. The raw gas composition of the carbon monoxide preferential oxidation reaction is: 1% CO, 1% O2, 50% H2, 48% N2, the reaction temperature is 50-210°C, and the reaction mass space velocity is 60000 mL·h -1 ·g cat -1 The raw gas and reaction tail gas were analyzed online using Agilent 7890A gas chromatograph. Figure 6 As shown in Figure 5, the CO conversion of 0.5RuTi-R400 reaches 100% at 130 °C, and 100% CO conversion is achieved in the temperature range of 130–210 °C.
[0045] Example 5
[0046] Preparation of Ru-based catalyst: According to the theoretical loading of 0.5wt%, weigh 0.005g of ruthenium trichloride precursor with a metal Ru content, dissolve it in 70mL of water, and stir to mix evenly. Weigh 0.995g of TiO2 powder, add it to the mixed solution, and stir to form a mixed suspension. Weigh hydrazine hydrate with a molar ratio of 1.5 to the Ru, dissolve it in water to form a solution, and add the solution to the above suspension, and heat and stir at 90°C for 3h. The suspension is filtered or centrifuged to obtain a solid material, and the solid is washed. The treated solid is dried in a 70°C oven for 12h, and then calcined in a tubular furnace at 300°C in a nitrogen atmosphere for 3h to obtain the catalyst 0.5RuTi. The catalyst is reduced at 600°C in a H2 / N2 atmosphere for 1h to obtain 0.5RuTi-R600.
[0047] The catalyst is used for the carbon monoxide preferential oxidation reaction. 0.1 g of the catalyst (40-60 mesh) prepared in Example 5 is taken and loaded into a fixed bed quartz tube reactor. The reaction tube used is 50 cm long and 8 mm in inner diameter. The raw gas composition of the carbon monoxide preferential oxidation reaction is: 1% CO, 1% O2, 50% H2, 48% N2, the reaction temperature is 50-210°C, and the reaction mass space velocity is 60000 mL·h -1 ·g cat -1 The raw gas and reaction tail gas were analyzed online using Agilent 7890A gas chromatograph. Figure 7 As shown in Figure 5, the CO conversion of 0.5RuTi-R600 reaches 100% at 130 °C, and 100% CO conversion is achieved in the temperature range of 130–210 °C.
[0048] Example 6
[0049] Preparation of Ru-based catalyst: According to the theoretical loading of 1wt%, weigh 0.01g of ruthenium acetylacetonate precursor with a metal Ru content, dissolve it in 70mL of water, and stir to mix evenly. Weigh 0.99g of TiO2 powder, add it to the mixed solution and stir to form a mixed suspension. Weigh 1.5 moles of sodium borohydride with the Ru, dissolve it in water to form a solution, and add the solution to the above suspension, and heat and stir at 90°C for 3h. The suspension is filtered or centrifuged to obtain a solid material, and the solid is washed. The treated solid is dried in a 70°C oven for 12h, and then calcined in a tubular furnace at 300°C in a nitrogen atmosphere for 3h to obtain the catalyst 1RuTi. The catalyst is reduced at 200°C in a H2 / N2 atmosphere for 1h to obtain 1RuTi-R200.
[0050] The catalyst is used for the carbon monoxide preferential oxidation reaction. 0.1 g of the catalyst (40-60 mesh) prepared in Example 6 is taken and loaded into a fixed bed quartz tube reactor. The reaction tube used is 50 cm long and 8 mm in inner diameter. The raw gas composition of the carbon monoxide preferential oxidation reaction is: 1% CO, 1% O2, 50% H2, 48% N2, the reaction temperature is 50-210°C, and the reaction mass space velocity is 60000 mL·h -1 ·g cat -1 The raw gas and reaction tail gas were analyzed online using Agilent 7890A gas chromatograph. Figure 8 As shown in Figure 5, the CO conversion of 1RuTi-R200 reaches 100% at 90 °C, and 100% CO conversion is achieved in the temperature range of 90–150 °C.
[0051] Example 7
[0052] Preparation of Ru-based catalyst: According to the theoretical loading of 1.5wt%, weigh 0.015g of ruthenium acetate precursor with a metal Ru content, dissolve it in 70mL of water, and stir to mix evenly. Weigh 0.985g of TiO2 powder, add it to the mixed solution, and stir to form a mixed suspension. Weigh sodium borohydride with a molar ratio of 1.5 to the Ru, dissolve it in water to form a solution, and add the solution to the above suspension, and heat and stir at 90°C for 3h. The suspension is filtered or centrifuged to obtain a solid material, and the solid is washed. The treated solid is dried in a 70°C oven for 12h, and then calcined in a tubular furnace at 300°C in a nitrogen atmosphere for 3h to obtain the catalyst 1.5RuTi. The catalyst is reduced at 200°C in a H2 / N2 atmosphere for 1h to obtain 1.5RuTi-R200.
[0053] The catalyst is used for the carbon monoxide preferential oxidation reaction. 0.1 g of the catalyst (40-60 mesh) prepared in Example 7 is taken and loaded into a fixed bed quartz tube reactor. The reaction tube used is 50 cm long and 8 mm in inner diameter. The raw gas composition of the carbon monoxide preferential oxidation reaction is: 1% CO, 1% O2, 50% H2, 48% N2, the reaction temperature is 50-210°C, and the reaction mass space velocity is 60000 mL·h -1 ·g cat -1 The raw gas and reaction tail gas were analyzed online using Agilent 7890A gas chromatograph. Fig. 9 As shown in Figure 5, the CO conversion of 1.5RuTi-R200 reaches 100% at 90 °C, and 100% CO conversion is achieved in the temperature range of 90–210 °C.
[0054] Example 8
[0055] Preparation of Ru-based catalyst: According to the theoretical loading of 2wt%, weigh 0.02g of ruthenium trichloride precursor with a metal Ru content, dissolve it in 70mL of water, and stir to mix evenly. Weigh 0.98g of TiO2 powder, add it to the mixed solution, and stir to form a mixed suspension. Weigh sodium borohydride with a molar ratio of 1.5 to the Ru, dissolve it in water to form a solution, and add the solution to the above suspension, and heat and stir at 90°C for 3h. The suspension is filtered or centrifuged to obtain a solid material, and the solid is washed. The treated solid is dried in a 70°C oven for 12h, and then calcined in a tubular furnace at 300°C in a nitrogen atmosphere for 3h to obtain the catalyst 2RuTi. The catalyst is reduced at 200°C in a H2 / N2 atmosphere for 1h to obtain 2RuTi-R200.
[0056] The catalyst is used for the carbon monoxide preferential oxidation reaction. 0.1 g of the catalyst (40-60 mesh) prepared in Example 8 is taken and loaded into a fixed bed quartz tube reactor. The reaction tube used is 50 cm long and 8 mm in inner diameter. The raw gas composition of the carbon monoxide preferential oxidation reaction is: 1% CO, 1% O2, 50% H2, 48% N2, the reaction temperature is 50-210°C, and the reaction mass space velocity is 60000 mL·h -1 ·g cat -1 The raw gas and reaction tail gas were analyzed online using Agilent 7890A gas chromatograph. Fig.10 As shown in Figure 5, the CO conversion of 2RuTi-R200 reaches 100% at 90 °C, and 100% CO conversion is achieved in the temperature range of 90–210 °C.
[0057] Example 9
[0058] Preparation of Ru-based catalyst: According to the theoretical loading of 5wt%, weigh 0.05g of ruthenium trichloride precursor with a metal Ru content, dissolve it in 70mL of water, and stir to form a uniform mixture. Weigh 0.95g of TiO2 powder, add it to the mixed solution, and stir to form a uniformly mixed suspension. Weigh sodium borohydride with a molar ratio of 1.5 to the Ru, dissolve it in water to form a solution, and add the aqueous solution to the above suspension, and heat and stir at 90°C for 3h. The suspension is filtered or centrifuged to obtain a solid material, and the solid is washed. The treated solid is dried in a 70°C oven for 12h, and then calcined in a tubular furnace at 300°C in a nitrogen atmosphere for 3h to obtain the catalyst 5RuTi. The catalyst is reduced at 200°C in a H2 / N2 atmosphere for 1h to obtain 2RuTi-R200.
[0059] The catalyst is used for the carbon monoxide preferential oxidation reaction. 0.1 g of the catalyst (40-60 mesh) prepared in Example 9 is taken and loaded into a fixed bed quartz tube reactor. The reaction tube used is 50 cm long and 8 mm in inner diameter. The raw gas composition of the carbon monoxide preferential oxidation reaction is: 1% CO, 1% O2, 50% H2, 48% N2, the reaction temperature is 50-210°C, and the reaction mass space velocity is 60000 mL·h -1 ·g cat -1 The raw gas and reaction tail gas were analyzed online using Agilent 7890A gas chromatograph. Fig.11 As shown in Figure 5, the CO conversion of 5RuTi-R200 reaches 100% at 90 °C, and 100% CO conversion is achieved in the temperature range of 90–210 °C.
[0060] Comparative Example 1
[0061] Preparation of Ru-based catalyst: According to the theoretical loading of 0.5wt%, weigh 0.05g of ruthenium trichloride precursor with a metal Ru content, dissolve it in 70mL of water, and stir to form a uniform mixture. Weigh 0.95g of TiO2 powder, add it to the mixed solution, stir to form a uniformly mixed suspension, and heat and stir at 90°C for 3h. The suspension is filtered or centrifuged to obtain a solid material, and the solid is washed. The treated solid is dried in a 70°C oven for 12h, and then calcined in a tubular furnace at 300°C in a nitrogen atmosphere for 3h to obtain the catalyst 5RuTi-IM. The catalyst is reduced at 200°C in a H2 / N2 atmosphere for 1h to obtain 0.5RuTi-IM-R200.
[0062] The catalyst is used for the carbon monoxide preferential oxidation reaction. 0.1 g of the catalyst (40-60 mesh) prepared in Comparative Example 1 is taken and loaded into a fixed bed quartz tube reactor. The reaction tube used is 50 cm long and 8 mm in inner diameter. The raw gas composition of the carbon monoxide preferential oxidation reaction is: 1% CO, 1% O2, 50% H2, 48% N2, the reaction temperature is 50-210°C, and the reaction mass space velocity is 60000 mL·h -1 ·g cat -1 The raw gas and the reaction tail gas were analyzed online by Agilent 7890A gas chromatograph. As shown in Table 1, the CO conversion rate of 0.5RuTi-IM-R200 reached a maximum conversion rate of 73% at 170°C, and CO could not be completely eliminated below 210°C.
[0063] Table 1: Catalysts' carbon monoxide preferential oxidation performance tabulated.
[0064]
[0065]
[0066] from Fig.10 It can be seen that compared with the catalyst prepared by the conventional impregnation method (Comparative Example 1, 0.5RuTi-IM-R200), the Ru 3d 5 / 2 The peak shifts toward the low binding energy direction, indicating that TiO2 on the catalyst provided by the present invention transfers more electrons to Ru, thereby forming a stronger metal-support interaction. Fig.11It can be seen that compared with the catalyst prepared by the traditional impregnation method (Comparative Example 1, 0.5RuTi-IM-R200), the CO adsorption peak on the catalyst provided by the present invention (Example 3, 0.5RuTi-R200) is red-shifted to a low wave number, indicating that the catalyst provided by the present invention has a stronger electronic metal-support interaction. Combined with the activity data in Table 1, it can be seen that compared with the catalyst prepared by the traditional impregnation method, due to the stronger electronic metal-support interaction, the catalyst provided by the present invention exhibits a more excellent catalytic activity, and can achieve complete elimination of CO in a wide temperature range (70-210 degrees Celsius, that is, the upper limit can reach 210 degrees Celsius, and the lower limit can reach 70 degrees Celsius), which is suitable for proton exchange membrane fuel cells, and preferentially oxidizes trace carbon monoxide in the gas used therein.
[0067] According to the content of the present invention, the process parameters can be adjusted to achieve the preparation of the catalyst of the present invention, and the performance substantially consistent with the present invention is shown after testing. The present invention is described exemplarily above, and it should be noted that any simple deformation, modification or equivalent replacement that can be made by other technicians in this field without spending creative labor falls within the protection scope of the present invention without departing from the core of the present invention.
Claims
1. A ruthenium-based catalyst for preferential oxidation of carbon monoxide, characterized in that: The catalyst is composed of a ruthenium active component and a titanium dioxide carrier. The ruthenium content is 0.05-5wt% based on the total mass of the catalyst. The steps are as follows: Step 1, dispersing a ruthenium precursor in water to form a uniform solution, adding a titanium dioxide carrier, and stirring to form a uniform suspension, which is labeled as A; in step 1, the ruthenium precursor is selected from ruthenium trichloride, ruthenium nitrosyl nitrate, ruthenium acetate, ruthenium acetate or ruthenium acetylacetonate; Step 2, adding a reducing agent to the suspension obtained in step 1, heating and stirring, to obtain a new suspension, marked as suspension B; the molar ratio of the reducing agent to ruthenium is (1-4):1; the reducing agent is sodium borohydride, potassium borohydride, formic acid or hydrazine hydrate; the reaction time after adding the reducing agent is 1-5 hours Step 3, after solid-liquid separation of the suspension obtained in step 2, the obtained solid material is washed and dried, and then roasted, and then the roasted material is reduced to obtain a ruthenium-based catalyst for preferential oxidation of carbon monoxide; when roasting, the roasting temperature is 200-500°C, the roasting time is 1-5 hours, and the roasting atmosphere is air or an inert protective gas; when reducing, the reduction temperature is 200-600°C, the reduction time is 1-5 hours, and the reducing atmosphere is a mixed gas of carbon monoxide and an inert protective atmosphere, or a mixed gas of hydrogen and an inert protective atmosphere.
2. A ruthenium-based catalyst for preferential oxidation of carbon monoxide according to claim 1, characterized in that: The content of ruthenium is 0.5-5wt% based on the total mass of the catalyst.
3. A ruthenium-based catalyst for preferential oxidation of carbon monoxide according to claim 1, characterized in that: In step 1, the stirring is selected by mechanical stirring or magnetic stirring, and the speed is 300-500 revolutions per minute.
4. A ruthenium-based catalyst for preferential oxidation of carbon monoxide according to claim 1, characterized in that: In step 2, the reducing agent is added to the suspension obtained in step 1 in the form of an aqueous solution; the molar ratio of the reducing agent to ruthenium is (1-3):1, and the reaction time after adding the reducing agent is 3-5 hours to allow the ruthenium precursor and the reducing agent to fully react; the heating temperature is 60-90°C, and the stirring is selected by mechanical stirring or magnetic stirring at a speed of 300-500 revolutions per minute.
5. A ruthenium-based catalyst for preferential oxidation of carbon monoxide according to claim 1, characterized in that: In step 3, during calcination, the temperature is raised from room temperature 20-25 degrees Celsius at a rate of 5-10 degrees Celsius per minute to a calcination temperature of 200-300°C, the calcination time is 3-5 hours, and the calcination is naturally cooled to room temperature; during reduction, the temperature is raised from room temperature 20-25 degrees Celsius at a rate of 5-10 degrees Celsius per minute to a reduction temperature of 200-400°C, the reduction time is 1-3 hours, and carbon monoxide is directly preferentially oxidized after reduction; the inert protective gas is nitrogen, helium or argon; in the mixed gas of carbon monoxide and the inert protective atmosphere, the volume percentage of carbon monoxide is 5-10%; in the mixed gas of hydrogen and the inert protective atmosphere, the volume percentage of hydrogen is 8-12%.
6. A method for preparing a ruthenium-based catalyst for preferential oxidation of carbon monoxide, characterized in that: The catalyst is composed of a ruthenium active component and a titanium dioxide carrier. The ruthenium content is 0.05-5wt% based on the total mass of the catalyst. The steps are as follows: Step 1, dispersing a ruthenium precursor in water to form a uniform solution, adding a titanium dioxide carrier, and stirring to form a uniform suspension, which is labeled as A; in step 1, the ruthenium precursor is selected from ruthenium trichloride, ruthenium nitrosyl nitrate, ruthenium acetate, ruthenium acetate or ruthenium acetylacetonate; Step 2, adding a reducing agent to the suspension obtained in step 1, heating and stirring, to obtain a new suspension, marked as suspension B; the molar ratio of the reducing agent to ruthenium is (1-4):1; the reducing agent is sodium borohydride, potassium borohydride, formic acid or hydrazine hydrate; the reaction time after adding the reducing agent is 1-5 hours Step 3, after solid-liquid separation of the suspension obtained in step 2, the obtained solid material is washed and dried, and then roasted, and then the roasted material is reduced to obtain a ruthenium-based catalyst for preferential oxidation of carbon monoxide; when roasting, the roasting temperature is 200-500°C, the roasting time is 1-5 hours, and the roasting atmosphere is air or an inert protective gas; when reducing, the reduction temperature is 200-600°C, the reduction time is 1-5 hours, and the reducing atmosphere is a mixed gas of carbon monoxide and an inert protective atmosphere, or a mixed gas of hydrogen and an inert protective atmosphere.
7. The method for preparing a ruthenium-based catalyst for preferential oxidation of carbon monoxide according to claim 6, characterized in that: In step 1, the stirring is selected by mechanical stirring or magnetic stirring, and the speed is 300-500 revolutions per minute.
8. The method for preparing a ruthenium-based catalyst for preferential oxidation of carbon monoxide according to claim 6, characterized in that: In step 2, the reducing agent is added to the suspension obtained in step 1 in the form of an aqueous solution; the molar ratio of the reducing agent to ruthenium is (1-3):1, and the reaction time after adding the reducing agent is 3-5 hours to allow the ruthenium precursor and the reducing agent to fully react; the heating temperature is 60-90°C, and the stirring is selected by mechanical stirring or magnetic stirring at a speed of 300-500 revolutions per minute.
9. The method for preparing a ruthenium-based catalyst for preferential oxidation of carbon monoxide according to claim 6, characterized in that: In step 3, during calcination, the temperature is raised from room temperature 20-25 degrees Celsius at a rate of 5-10 degrees Celsius per minute to a calcination temperature of 200-300°C, the calcination time is 3-5 hours, and the calcination is naturally cooled to room temperature; during reduction, the temperature is raised from room temperature 20-25 degrees Celsius at a rate of 5-10 degrees Celsius per minute to a reduction temperature of 200-400°C, the reduction time is 1-3 hours, and carbon monoxide is directly preferentially oxidized after reduction; the inert protective gas is nitrogen, helium or argon; in the mixed gas of carbon monoxide and the inert protective atmosphere, the volume percentage of carbon monoxide is 5-10%; in the mixed gas of hydrogen and the inert protective atmosphere, the volume percentage of hydrogen is 8-12%.
10. Use of the ruthenium-based catalyst for preferential oxidation of carbon monoxide as claimed in any one of claims 1 to 5 in a proton exchange membrane fuel cell.
Citation Information
Patent Citations
Method for preparing proton exchange membrane fuel cell supported catalyst
CN101890347A
High dispersion type ruthenium oxide catalyst as well as preparation method and application thereof
CN108212149A
Supported nano multi-metal catalyst, preparation method thereof and application of supported nano multi-metal catalyst to CO oxidation
CN111266116A
Ru-based catalyst for synthesizing 3-pentanone through ethylene conversion and preparation method and application thereof
CN111420657A
Ru-based catalyst as well as preparation method and application thereof
CN114570360A
Cited By
Platinum-based catalyst for CO preferential oxidation in hydrogen-rich atmosphere as well as preparation method and application of platinum-based catalyst
CN122124815A