High-dispersion noble metal modified indium oxide catalyst as well as preparation method and application thereof

By doping precious metals into hexagonal phase indium oxide, a highly dispersed precious metal modified indium oxide catalyst is formed, which solves the problems of low conversion efficiency and high cost of CO2 hydrogenation to methanol, and achieves efficient CO2 resource utilization.

CN118904332APending Publication Date: 2024-11-08ZHENGZHOU UNIV

Patent Information

Application Number
CN202410959667.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The current conversion efficiency of CO2 hydrogenation to methanol is low and costly, which limits the industrialization process of CO2 resource utilization.

Method used

By doping precious metals such as Pt, Pd, Ru and Rh in hexagonal phase indium oxide to improve their carbon dioxide conversion rate during the preparation of methanol by hydrogenation of carbon dioxide, the hydrothermal method is used to ensure that the precious metals are uniformly dispersed in atomic-level form, forming Highly dispersed precious metal modified indium oxide catalyst.

Benefits of technology

The carbon dioxide conversion rate and hydrogen adsorption and dissociation capacity of the catalyst are significantly improved, catalytic activity and stability are enhanced, preparation costs are reduced, and efficient CO2 resource utilization is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904332A_ABST
    Figure CN118904332A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of new energy and new materials, and discloses a high-dispersion noble metal modified indium oxide catalyst as well as a preparation method and application thereof. The high-dispersion noble metal modified indium oxide catalyst comprises an active component and doped noble metal, the active component is hexagonal phase indium oxide with a nanowire multilevel structure; the doped noble metal is dispersed and doped in the active component in an atomic form, and the doped noble metal is any one of Pt, Pd, Ru and Rh; the doped noble metal accounts for 1%-5% of the mass of the high-dispersion noble metal modified indium oxide catalyst. According to the preparation method disclosed by the invention, the hexagonal phase indium oxide with the nanowire multilevel structure is used as an active component, and various different high-dispersion noble metal modified catalysts with relatively high catalytic activity are obtained by adjusting the variety and doping amount of noble metal atoms; and the high-dispersion noble metal modified catalyst has strong carbon dioxide adsorption and hydrogen dissociation capacities, and the target product selectivity and the catalyst stability are high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of new energy and new materials, and in particular to a highly dispersed noble metal modified indium oxide catalyst and a preparation method and application thereof. Background Art

[0002] Developing efficient CO2 conversion and utilization technologies to make CO2 a resource is a demand for renewable energy utilization and carbon neutrality. Methanol, as a high-quality, efficient, clean and low-carbon basic chemical and fuel, has a wide range of uses in automotive energy, industrial fuel and chemical raw materials. Using industrial by-product H2 and zero-carbon energy to produce hydrogen, such as renewable energy hydrogen production and nuclear energy hydrogen production, catalyzing CO2 directly into green and low-carbon methanol is a feasible process route for CO2 resource utilization.

[0003] As an important chemical raw material and liquid hydrogen storage fuel, methanol has become an important substitute for fossil fuels. At present, the conversion efficiency of CO2 hydrogenation to methanol is still low and the cost is high, which slows down the large-scale industrialization of CO2 to methanol. In recent years, through DFT and experimental studies, it has been found that the (104) crystal plane of hexagonal indium oxide has a high methanol selectivity for methanol, but there are still problems such as low carbon dioxide conversion rate and priority of hydrogenolysis ability. Based on indium oxide with mainly exposed crystal planes, the precise construction and preparation of efficient indium oxide-based catalysts has important research significance for catalyst design and industrial application of carbon dioxide hydrogenation to methanol. Summary of the invention

[0004] In order to solve the above-mentioned deficiencies in the prior art, the present invention provides a highly dispersed noble metal modified indium oxide catalyst and a preparation method and application thereof. A highly dispersed noble metal modified indium oxide catalyst and a preparation method and application thereof of the present invention are achieved by the following technical scheme:

[0005] The first object of the present invention is to provide a highly dispersed noble metal modified indium oxide catalyst. The present invention proposes to improve the carbon dioxide conversion rate of the (104) crystal plane of the hexagonal indium oxide when the carbon dioxide is hydrogenated to produce methanol by doping noble metals in the hexagonal indium oxide, so that the indium oxide-based catalyst can be used in the preparation of methanol by hydrogenation of carbon dioxide. The highly dispersed noble metal modified indium oxide catalyst of the present invention includes an active component and a doped noble metal; wherein the active component is a hexagonal indium oxide with a nanowire multi-level structure; and the doped noble metal is dispersed and doped in the active component in the form of an atomic level.

[0006] It should be noted that in order to improve the carbon dioxide conversion rate of the (104) crystal plane of hexagonal indium oxide in the preparation of methanol by hydrogenation of carbon dioxide, in some preferred embodiments of the present invention, the doped precious metal used is any one of Pt, Pd, Ru and Rh. Since these precious metals have good hydrogen dissociation ability, they can enhance the catalyst's adsorption and dissociation ability for hydrogen and produce more oxygen vacancy active sites, so that the obtained highly dispersed precious metal modified indium oxide catalyst can be used in the preparation of methanol by hydrogenation of carbon dioxide.

[0007] The present invention takes into account that too little doping of the precious metal will result in the inability to effectively improve the catalytic performance of indium oxide; and too much doping of the precious metal will not only fail to further improve the catalytic performance of indium oxide, but will also lead to an increase in preparation costs. Therefore, in some preferred embodiments of the present invention, the doped precious metal accounts for 1% to 5% of the mass of the highly dispersed precious metal modified indium oxide catalyst.

[0008] In order to ensure that in the highly dispersed precious metal-modified indium oxide catalyst of the present invention, the precious metal can be dispersed and doped in the hexagonal indium oxide having a nanowire multi-level structure in the form of an atomic level, in some preferred embodiments of the present invention, the highly dispersed precious metal-modified indium oxide catalyst is obtained by a hydrothermal method by using the doped precious metal to perform bulk doping on the active component.

[0009] The second object of the present invention is to provide a method for preparing the above-mentioned highly dispersed precious metal-modified indium oxide catalyst. In order to ensure that the prepared highly dispersed precious metal-modified indium oxide catalyst, the precious metal can be uniformly doped in the hexagonal phase indium oxide having a nanowire multi-level structure in the form of an atomic level, so as to enhance the hydrogen adsorption and dissociation ability, generate more oxygen vacancies to enhance the catalytic activity, and improve the catalytic activity of the indium oxide-based catalyst, in some preferred embodiments of the present invention, the following steps are adopted to obtain:

[0010] Step 1: according to the ratio of the precious metal component to the total mass of the catalyst of 1% to 5%, weigh the corresponding mass of soluble indium salt and soluble precious metal salt, and disperse them in a solvent to obtain a salt solution.

[0011] It should be noted that the present invention first disperses the indium salt and the noble metal salt uniformly in the solvent, so that the indium ions provided by the indium salt and the noble metal ions provided by the noble metal salt can be evenly mixed in the solution environment, thereby preparing for the subsequent noble metal to be uniformly doped into indium oxide in the form of atomic level.

[0012] The present invention has been found in the process of exploration that when other soluble indium salts are used, hexagonal indium oxide with a nanowire multilevel structure cannot be formed. Therefore, in order to ensure that the soluble indium salt used can form a hexagonal indium oxide with a nanowire multilevel structure in the subsequent reaction process, in some preferred embodiments of the present invention, the indium salt used is indium nitrate. The present invention has been found in the process of further exploration that the bound water contained in indium nitrate will also have a certain influence on the crystal growth and the final indium oxide morphology. In order to further ensure that a hexagonal indium oxide with a nanowire multilevel structure can be formed, in some more preferred embodiments of the present invention, the indium nitrate used can be selected from one or two of tetrahydrated indium nitrate, tetra-point pentahydrated indium nitrate and pentahydrated indium nitrate.

[0013] The present invention does not limit the specific type of precious metal salt, as long as it can provide precious metal ions so that they can form corresponding precious metal atoms and be doped into the hexagonal indium oxide having a nanowire multi-level structure during the subsequent reaction. For example, in some preferred embodiments of the present invention, the precious metal salt used is any one of Pt salt, Pd salt, Ru salt and Rh salt.

[0014] Among them, the present invention found in the process of exploration that the form of Pt salt used has an important influence on the final doping form of Pt in hexagonal indium oxide. In order to ensure that the Pt salt used can disperse Pt in the hexagonal indium oxide in the form of atomic level, in some preferred embodiments of the present invention, when the precious metal salt used is Pt salt, the Pt salt used can be selected from tetraammineplatinum dinitrate. For the sake of ease of expression, the present invention will hereinafter use the chemical formula Pt(NH3)4(NO3)2 to express tetraammineplatinum dinitrate.

[0015] During the research process, the present invention found that the form of Pd salt used has an important influence on the final doping form of Pd in ​​hexagonal indium oxide. In order to ensure that the Pd salt used can disperse Pd in ​​the hexagonal indium oxide in the form of atomic level, in some preferred embodiments of the present invention, when the precious metal salt used is Pd salt, the Pd salt used can be selected from palladium nitrate. For the sake of ease of description, the present invention will hereinafter use the chemical formula Pd(NO3)2·2H2O to describe palladium nitrate.

[0016] During the research process, the present invention found that the form of Ru salt used has an important influence on the final doping form of Ru in hexagonal indium oxide. In order to ensure that the Ru salt used can disperse Ru in the hexagonal indium oxide in the form of atomic level, in some preferred embodiments of the present invention, when the precious metal salt used is Ru salt, the Ru salt used can be selected from ruthenium nitrosyl nitrate. For the sake of ease of description, the present invention will hereinafter use the chemical formula Ru(NO)(NO3)3 to describe ruthenium nitrosyl nitrate.

[0017] During the research process, the present invention found that the form of Rh salt used has an important influence on the final doping form of Rh in hexagonal indium oxide. In order to ensure that the Rh salt used can disperse Rh in the hexagonal indium oxide in the form of atomic level, in some preferred embodiments of the present invention, when the precious metal salt used is Rh salt, the Rh salt used can be selected from rhodium nitrate nitrate. For the sake of ease of description, the present invention will hereinafter use the chemical formula RhCl3 to describe rhodium trichloride.

[0018] In order to ensure that the indium salt and the noble metal salt can be fully mixed in the solution environment, in some preferred embodiments of the present invention, the solvent used is a mixture of deionized water and anhydrous ethanol to ensure that both the indium salt and the noble metal salt have good solubility. The volume ratio of deionized water to anhydrous ethanol is 0.1 to 1.5:1.

[0019] In order to further ensure that the amount of added solvent can fully dissolve and disperse the indium salt and the noble metal salt, in other preferred embodiments of the present invention, the concentration of the indium salt in the salt solution is 0.3-1 mol / L.

[0020] Step 2, adding the precipitant dropwise into the salt solution and mixing well to obtain a precipitated mother solution.

[0021] It should be noted that in order to ensure the in-situ synthesis of unit-site precious metal-doped hexagonal indium oxide, that is, to obtain the highly dispersed precious metal-doped indium oxide catalyst, the present invention investigates the influence of the selection of precipitant on the formation of hexagonal indium oxide with a regular morphology, and in the process of investigation, it is found that the type of precipitant has an important influence on the morphology of hexagonal indium oxide. In order to ensure that hexagonal indium oxide with a regular morphology can be obtained, urea is used as a precipitant in some preferred embodiments of the present invention.

[0022] In order to facilitate the mixing of the precipitant with the above-mentioned salt solution, in some preferred embodiments of the present invention, urea is added dropwise in the salt solution in the form of a solution to mix the precipitant and the salt solution, so that the precipitant can be fully mixed with the salt solution. Since the urea solution is a weak base, it can form an indium hydroxide precipitate with indium ions in the subsequent reaction process. It should be noted that in order to ensure that the components of the salt solution still maintain good solubility after the precipitant and the salt solution are mixed, in some preferred embodiments of the present invention, the solution used to dissolve or disperse the precipitant is a mixed solution of deionized water and anhydrous ethanol, and the precipitant is added in the form of a solution with a concentration of 1 to 6 mol / L, and the volume ratio of deionized water to anhydrous ethanol is 0.2 to 2:1.

[0023] In order to ensure that the precipitant can be mixed with the salt solution after being added, in some preferred embodiments of the present invention, stirring is used to mix and then form a precipitated mother solution. In other preferred embodiments of the present invention, the stirring time is 1 to 7 hours.

[0024] Step 3, subjecting the precipitation mother liquor to a hydrothermal reaction at 100° C. to 180° C., followed by centrifugation, drying and calcination in sequence to obtain the highly dispersed noble metal-modified indium oxide catalyst.

[0025] It should be noted that in order to ensure that the highly dispersed noble metal-doped indium oxide catalyst can be obtained, in some preferred embodiments of the present invention, the above-mentioned precipitation mother liquor is first subjected to a hydrothermal reaction treatment at a temperature of 100 to 180°C, so that the urea in the precipitation mother liquor is decomposed under the high temperature and high pressure conditions of the hydrothermal reaction, providing hydroxide for the reaction system, and the formed hydroxide further reacts with indium ions or noble metal ions to produce hydroxide precipitation. In order to ensure that the above effect can be achieved at this temperature, in some preferred embodiments of the present invention, the hydrothermal reaction time is 10 to 24 hours.

[0026] The present invention takes into account that since the hydrothermal reaction is carried out in a solution environment, the obtained hydrothermal reaction product also exists in the solution environment. In order to facilitate the subsequent further treatment of the hydrothermal reaction product, the hydrothermal reaction product needs to be firstly subjected to solid-liquid separation, such as solid-liquid separation by centrifugation to remove excess filtrate, and the obtained precipitate is the actual desired aging product. At the same time, considering that the reaction solvent and other impurities may remain on the surface of the precipitate, deionized water is used as a detergent during centrifugation, and multiple centrifugation treatments are performed, and the deionized water is centrifuged to a mother liquor with a pH of 7 to 9 to remove the reaction solvent and excess alkaline impurities that may remain on the surface of the precipitate.

[0027] The present invention takes into account that detergent may exist on the surface of the precipitate after washing, which may affect the subsequent calcination effect. Therefore, in some preferred embodiments of the present invention, the precipitate after centrifugation is dried before calcination to remove the deionized water remaining on the surface of the precipitate to avoid its possible influence on the catalyst result. Among them, in other preferred embodiments of the present invention, the drying temperature is 60-120°C and the drying time is 14-26h. It should also be noted that the present invention takes into account the different properties of different precious metals, so the corresponding calcination atmosphere can be selected according to the properties of different precious metals to ensure that a single-atom dispersed catalyst is obtained. For example, the calcination atmosphere used is any one of air, vacuum, pure nitrogen and pure argon.

[0028] Since the noble metal has been doped in the indium hydroxide in the form of hydroxide during the hydrothermal process, in order to obtain a catalyst material doped with the noble metal at the atomic level, the present invention also performs a roasting treatment on it, so as to convert the hydroxide into an oxide through the roasting treatment, thereby obtaining a highly dispersed noble metal-doped indium oxide catalyst doped with the noble metal at the atomic level. In order to ensure that a highly dispersed noble metal-doped indium oxide catalyst doped with the noble metal at the atomic level is obtained through the roasting treatment, the roasting temperature preferably used in the present invention is 300 to 600°C. In order to further ensure that the above-mentioned effect can be achieved at this roasting temperature, in other preferred embodiments of the present invention, the roasting time is 3 to 8 hours.

[0029] The third object of the present invention is to provide an application of the above-mentioned highly dispersed noble metal-doped indium oxide catalyst in the preparation of methanol by hydrogenation of carbon dioxide.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] The present invention uses hexagonal indium oxide with a nanowire multi-level structure as an active component, and obtains a variety of different highly dispersed noble metal modified catalysts by adjusting the type and doping amount of noble metal atoms. The carbon dioxide conversion rate of the indium oxide-based catalyst when carbon dioxide is hydrogenated to prepare methanol can be improved, so that the indium oxide-based catalyst can be used in the preparation of methanol by hydrogenation of carbon dioxide.

[0032] The preparation process of the present invention is simple. The metal salt solution and the precipitant solution dissolved in different ratios of anhydrous ethanol and deionized water are fully mixed and then put into a hydrothermal kettle. A solid phase precursor is obtained by hydrothermal synthesis, centrifugation and drying. A highly dispersed noble metal-doped hexagonal phase indium oxide catalyst with a regular nano multi-level structure is prepared by roasting. The highly dispersed noble metal modified catalyst prepared by the present invention has high catalytic activity, can enhance the ability of indium oxide-based catalysts to adsorb carbon dioxide and dissociate hydrogen, and significantly improves the selectivity of the target product and the stability of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The XRD patterns of the catalysts obtained in Examples 1 to 5 and Comparative Example 1 are shown.

[0034] Figure 2 These are SEM images of the catalysts obtained in Examples 1 to 5 and Comparative Example 1.

[0035] Among them, In2O3 represents the SEM image of comparative example 1, 4Pt-In2O3 represents the SEM image of embodiment 1, 2Pd-In2O3 represents the SEM image of embodiment 2, 2Ru-In2O3 represents the SEM image of embodiment 3, 3Ru-In2O3 represents the SEM image of embodiment 4, and 2Rh-In2O3 represents the SEM image of embodiment 5.

[0036] Figure 3 This is the ac-HAADF-STEM image of 4Pt-In2O3 of Example 1.

[0037] Wherein, (a) and (b) are ac-HAADF-STEM images of 4Pt-In2O3 at different positions in Example 1, and the inset in (b) is the linear scanning profile and corresponding atomic intensity along the yellow rectangular area in (b). DETAILED DESCRIPTION

[0038] The technical solutions in the embodiments of the present invention will be described clearly and completely below.

[0039] Example 1

[0040] This embodiment provides a highly dispersed noble metal-doped indium oxide catalyst, which is prepared by the following steps:

[0041] 1) Prepare salt solution:

[0042] Weigh 2g In(NO3)3·4H2O and 2g In(NO3)3·5H2O and fully dissolve them in 16mL deionized water, then weigh 0.303g Pt(NH3)4(NO3)2 and add it to the above solution and continue stirring. After clarification, add 16mL anhydrous ethanol and stir thoroughly to form a salt solution in which the metal indium ion concentration is 0.824mol / L.

[0043] 2) Preparation of precipitant solution:

[0044] 6.11 g of urea was fully stirred and dissolved in 10 mL of anhydrous ethanol and 15 mL of deionized water to obtain a precipitant solution, wherein the concentration of the precipitant solution was 4 mol / L.

[0045] 3) Mixing to form a precipitation mother solution:

[0046] At room temperature, the precipitant solution was added dropwise to the salt solution, and then stirred thoroughly for 6 h to obtain a precipitate mother solution.

[0047] 4) Aging treatment:

[0048] The obtained precipitation mother liquor was poured into a polytetrafluoroethylene-lined hydrothermal synthesis kettle, and placed in a forced air drying oven at a temperature of 180°C for static aging for 20 hours. After the reaction was completed, the hydrothermal kettle was naturally cooled to room temperature, and the mother liquor was centrifuged with deionized water to a pH of 8 to obtain a precipitate. The obtained precipitate was placed in an oven and dried at 120°C for 22 hours under a nitrogen atmosphere to obtain a dry product.

[0049] 5) Calcination treatment:

[0050] The dried product obtained above was placed in a muffle furnace and calcined at 550°C for 5 hours in an air atmosphere to obtain a highly dispersed precious metal-doped indium oxide catalyst. It was tested that in the highly dispersed precious metal-doped indium oxide catalyst of this embodiment, the Pt atom accounted for 4% of the total mass of the catalyst. Therefore, the highly dispersed precious metal-doped indium oxide catalyst obtained in this embodiment was named 4Pt-In2O3.

[0051] Example 2

[0052] This embodiment provides a highly dispersed noble metal-doped indium oxide catalyst, which is prepared by the following steps:

[0053] 1) Prepare salt solution:

[0054] Weigh 3g In(NO3)3·4.5H2O and 4.8g In(NO3)3·5H2O and fully dissolve them in 8mL deionized water, then weigh 0.138g Pd(NO3)2·2H2O and add it to the above solution and continue stirring. After clarification, add 24mL anhydrous ethanol and stir thoroughly to form a salt solution in which the metal indium ion concentration is 0.607mol / L.

[0055] 2) Preparation of precipitant solution:

[0056] 7.75 g of urea was fully stirred and dissolved in 6 mL of anhydrous ethanol and 19 mL of deionized water to obtain a precipitant solution, wherein the precipitant concentration was 5 mol / L.

[0057] 3) Mixing to form a precipitation mother solution:

[0058] At room temperature, the precipitant solution was added dropwise to the salt solution, and then stirred sufficiently for 3 h to obtain a precipitate mother solution.

[0059] 4) Aging treatment:

[0060] The mother liquor obtained by precipitation was poured into a hydrothermal synthesis kettle lined with polytetrafluoroethylene, and placed in a forced air drying oven at a temperature of 130°C for static aging for 24 hours. After the reaction was completed, the mother liquor was centrifuged with deionized water to a pH of 9 after the hydrothermal kettle naturally cooled to room temperature to obtain a precipitate. The obtained precipitate was placed in an oven and dried at 90°C for 24 hours under an argon atmosphere to obtain a dry product.

[0061] 5) Calcination treatment:

[0062] The dried product obtained above was placed in a muffle furnace and calcined at 450°C for 5 hours in an air atmosphere to obtain a highly dispersed precious metal-doped indium oxide catalyst. It was tested that in the highly dispersed precious metal-doped indium oxide catalyst of this embodiment, the Pd atom accounted for 2% of the total mass of the catalyst. Therefore, the highly dispersed precious metal-doped indium oxide catalyst obtained in this embodiment was named 2Pd-In2O3.

[0063] Example 3

[0064] This embodiment provides a highly dispersed noble metal-doped indium oxide catalyst, which is prepared by the following steps:

[0065] 1) Prepare salt solution:

[0066] Weigh 4 g In(NO3)3·4.5H2O and 4.5 g In(NO3)3·5H2O and fully dissolve them in 6 mL deionized water. Then weigh 0.189 g Ru(NO)(NO3)3 and add it to the above solution and continue stirring. After clarification, add 24 mL of anhydrous ethanol and stir thoroughly to form a salt solution in which the metal indium ion concentration is 0.661 mol / L.

[0067] 2) Preparation of precipitant solution:

[0068] 6.76 g of urea was fully stirred and dissolved in 18 mL of anhydrous ethanol and 7 mL of deionized water to obtain a precipitant solution, wherein the concentration of the precipitant solution was 4.5 mol / L.

[0069] 3) Mixing to form a precipitation mother solution:

[0070] At room temperature, the precipitant solution was added dropwise to the salt solution, and then stirred sufficiently for 4 h to obtain a precipitate mother solution.

[0071] 4) Aging treatment:

[0072] The mother liquor of precipitation obtained above was poured into a hydrothermal synthesis kettle lined with polytetrafluoroethylene, and placed in a forced air drying oven at a temperature of 160°C for static aging for 17 hours. After the reaction was completed, the mother liquor was centrifuged with deionized water to a pH of 8 after the hydrothermal kettle naturally cooled to room temperature to obtain a precipitate. The obtained precipitate was placed in an oven and dried at 100°C for 20 hours under a vacuum environment to obtain a dry product.

[0073] 5) Calcination treatment:

[0074] The dried product obtained above was placed in a muffle furnace and calcined at 500°C for 6 hours in an air atmosphere to obtain a highly dispersed precious metal-doped indium oxide catalyst. It was tested that in the highly dispersed precious metal-doped indium oxide catalyst of this embodiment, the Ru atom accounted for 2% of the total mass of the catalyst. Therefore, the highly dispersed precious metal-doped indium oxide catalyst obtained in this embodiment was named 2Ru-In2O3.

[0075] Example 4

[0076] This embodiment provides a highly dispersed noble metal-doped indium oxide catalyst, which is prepared by the following steps:

[0077] 1) Prepare salt solution:

[0078] Weigh 6g In(NO3)3·4H2O and 6g In(NO3)3·5H2O and fully dissolve them in 17mL deionized water. Then weigh 0.404g Ru(NO)(NO3)3 and add it to the above solution and continue stirring. After clarification, add 15mL anhydrous ethanol and stir thoroughly to form a salt solution with a metal indium ion concentration of 0.933mol / L.

[0079] 2) Preparation of precipitant solution:

[0080] 9.46 g of urea was fully stirred and dissolved in 12 mL of anhydrous ethanol and 13 mL of deionized water to obtain a precipitant solution, wherein the concentration of the precipitant solution was 6 mol / L.

[0081] 3) Mixing to form a precipitation mother solution:

[0082] At room temperature, the precipitant solution was added dropwise to the salt solution, and then stirred sufficiently for 5 h to obtain a precipitate mother solution.

[0083] 4) Aging treatment:

[0084] The mother liquor of precipitation obtained above was poured into a hydrothermal synthesis kettle lined with polytetrafluoroethylene, and placed in a forced air drying oven at a temperature of 160°C for static aging for 19 hours. After the reaction was completed, the mother liquor was centrifuged with deionized water to a pH of 7 after the hydrothermal kettle naturally cooled to room temperature to obtain a precipitate. The obtained precipitate was placed in an oven and dried at 100°C for 16 hours in an air atmosphere to obtain a dry product.

[0085] 5) Calcination treatment:

[0086] The dried product obtained above was placed in a muffle furnace and calcined at 600°C for 7 hours in an air atmosphere to obtain a highly dispersed precious metal-doped indium oxide catalyst. It was tested that in the highly dispersed precious metal-doped indium oxide catalyst of this embodiment, the Ru atom accounted for 3% of the total mass of the catalyst. Therefore, the highly dispersed precious metal-doped indium oxide catalyst obtained in this embodiment was named 3Ru-In2O3.

[0087] Example 5

[0088] This embodiment provides a highly dispersed noble metal-doped indium oxide catalyst, which is prepared by the following steps:

[0089] 1) Prepare salt solution:

[0090] Weigh 2g In(NO3)3·4H2O and 2g In(NO3)3·4.5H2O and fully dissolve them in 10mL deionized water, then weigh 0.057g RhCl3 and add it to the above solution and continue stirring. After clarification, add 22mL anhydrous ethanol and stir thoroughly to form a salt solution, in which the metal indium ion concentration is 0.311mol / L.

[0091] 2) Preparation of precipitant solution:

[0092] 2.25 g of urea was fully stirred and dissolved in 15 mL of anhydrous ethanol and 10 mL of deionized water to obtain a precipitant solution, wherein the concentration of the precipitant solution was 1.5 mol / L.

[0093] 3) Mixing to form a precipitation mother solution:

[0094] At room temperature, the precipitant solution was added dropwise to the salt solution, and then stirred sufficiently for 2 h to obtain a precipitate mother solution.

[0095] 4) Aging treatment:

[0096] The mother liquor obtained by precipitation was poured into a hydrothermal synthesis kettle lined with polytetrafluoroethylene, and placed in a forced air drying oven at a temperature of 120°C for static aging for 16 hours. After the reaction was completed, the mother liquor was centrifuged with deionized water to a pH of 7 after the hydrothermal kettle naturally cooled to room temperature to obtain a precipitate. The obtained precipitate was placed in an oven and dried at 60°C in a vacuum environment for 18 hours to obtain a dry product.

[0097] 5) Calcination treatment:

[0098] The dried product obtained above was placed in a muffle furnace and calcined at 400°C for 8 hours in an air atmosphere to obtain a highly dispersed precious metal-doped indium oxide catalyst. It was tested that in the highly dispersed precious metal-doped indium oxide catalyst of this embodiment, Rh atoms accounted for 2% of the total mass of the catalyst. Therefore, the highly dispersed precious metal-doped indium oxide catalyst obtained in this embodiment was named 2Rh-In2O3.

[0099] Comparative Example 1

[0100] This embodiment provides a highly dispersed noble metal-doped indium oxide catalyst, which is prepared by the following steps:

[0101] 1) Prepare salt solution:

[0102] Weigh 6 g of In(NO3)3·4.5H2O and fully dissolve it in 12 mL of deionized water. Then add 20 mL of anhydrous ethanol and stir thoroughly to form a salt solution in which the concentration of metal indium ions is 0.467 mol / L.

[0103] 2) Preparation of precipitant solution:

[0104] 4.5 g of urea was fully stirred and dissolved in 20 mL of anhydrous ethanol and 5 mL of deionized water to obtain a precipitant solution, wherein the precipitant concentration was 3 mol / L.

[0105] 3) Mixing to form a precipitation mother solution:

[0106] At room temperature, the precipitant solution was added dropwise to the salt solution, and then stirred sufficiently for 2 h to obtain a precipitate mother solution.

[0107] 4) Aging treatment:

[0108] The mother liquor obtained by precipitation was poured into a hydrothermal synthesis kettle lined with polytetrafluoroethylene, and placed in a forced air drying oven at a temperature of 100°C under air atmosphere for static aging for 14 hours. After the reaction was completed, the mother liquor was centrifuged with deionized water to a pH of 7 after the hydrothermal kettle naturally cooled to room temperature to obtain a precipitate. The obtained precipitate was placed in a forced air drying oven at a temperature of 80°C and dried for 16 hours to obtain a dry product.

[0109] 5) Calcination treatment:

[0110] The dried product obtained above was placed in a muffle furnace and calcined at 550° C. for 5 h in an air atmosphere to obtain an indium oxide catalyst. Since the catalyst material of this comparative example is not doped with any precious metal atoms, the catalyst obtained in this comparative example is named In2O3.

[0111] Experimental Section

[0112] (I) XRD test

[0113] The present invention takes 4Pt-In2O3 of Example 1, 2Pd-In2O3 of Example 2, 2Ru-In2O3 of Example 3, 3Ru-In2O3 of Example 4 and 2Rh-In2O3 of Example 5 as examples, and takes In2O3 of Comparative Example 1 as a control, and performs XRD tests respectively, and the test results are as follows: Figure 1 shown. Figure 1 The XRD patterns of the catalysts obtained in Examples 1 to 5 and Comparative Example 1 are shown.

[0114] Depend on Figure 1 It can be seen that the In2O3 of Comparative Example 1 has good crystallinity and is a hexagonal phase (JCPDS22-0336), without impurities. The 4Pt-In2O3 catalyst of Example 1 has good crystallinity and is a hexagonal phase (JCPDS22-0336), and no relevant diffraction peak of any Pt phase is detected, indicating that Pt is highly dispersed. The 2Pd-In2O3 of Example 2 has good crystallinity and is a hexagonal phase (JCPDS22-0336), and no relevant diffraction peak of any Pd phase is detected, indicating that Pd is highly dispersed. The 2Ru-In2O3 of Example 3 has good crystallinity and is a hexagonal phase (JCPDS22-0336), and no relevant diffraction peak of any Ru phase is detected, indicating that Ru is highly dispersed. The 3Ru-In2O3 of Example 4 has good crystallinity and is a hexagonal phase (JCPDS22-0336), and no relevant diffraction peak of any Ru phase is detected, indicating that Ru is highly dispersed. The 2Rh-In2O3 of Example 5 has good crystallinity and is a hexagonal phase (JCPDS22-0336), and no diffraction peaks related to any Rh phase are detected, indicating that Rh is highly dispersed.

[0115] The above shows that the preparation method of the present invention can uniformly dope different precious metals into hexagonal indium oxide in a highly dispersed form without destroying the original structure of hexagonal indium oxide, so that the doped sample still retains the crystal phase of hexagonal indium oxide.

[0116] (ii) SEM test

[0117] The present invention takes 4Pt-In2O3 of Example 1, 2Pd-In2O3 of Example 2, 2Ru-In2O3 of Example 3, 3Ru-In2O3 of Example 4 and 2Rh-In2O3 of Example 5 as examples, and takes In2O3 of Comparative Example 1 as a control, and performs SEM tests respectively, and the test results are as follows: Figure 2 shown. Figure 2 The following are SEM images of the catalysts obtained in Examples 1 to 5 and Comparative Example 1.

[0118] Depend on Figure 2 It can be seen that the In2O3 of Comparative Example 1 is a regular flower-like structure composed of nanowires. The 4Pt-In2O3 of Example 1 is a regular flower-like structure composed of nanowires, indicating that the doping of Pt does not affect the morphology of indium oxide nanoparticles. The 2Pd-In2O3 of Example 2 is a regular flower-like structure composed of nanowires, indicating that the doping of Pd does not affect the morphology of indium oxide nanoparticles. The 2Ru-In2O3 of Example 3 is a regular flower-like structure composed of nanowires, indicating that the doping of Ru does not affect the morphology of indium oxide nanoparticles. The 3Ru-In2O3 of Example 4 is a regular flower-like structure composed of nanowires, indicating that the doping of Ru does not affect the morphology of indium oxide nanoparticles. The 2Rh-In2O3 of Example 5 is a regular flower-like structure composed of nanowires, indicating that the doping of Rh does not affect the morphology of indium oxide nanoparticles.

[0119] The above further shows that the preparation method of the present invention can uniformly dope different precious metals into hexagonal indium oxide in a highly dispersed form without destroying the original structure of hexagonal indium oxide, so that the doped sample still retains the nanoparticle morphology of hexagonal indium oxide.

[0120] (III) TEM test

[0121] The present invention takes 4Pt-In2O3 of Example 1 as an example, and performs ac-HAADF-STEM tests on different positions thereof, and the test results are as follows: Figure 3 shown. Figure 3 (a) and (b) are ac-HAADF-STEM images of different positions of 4Pt-In2O3 in Example 1.

[0122] Depend on Figure 3 It can be seen that in 4Pt-In2O3 of Example 1, Pt is doped in In2O3 in the form of single-atom dispersion.

[0123] (IV) Experimental test of carbon dioxide hydrogenation activity

[0124] The present invention uses 4Pt-In2O3 of Example 1, 2Pd-In2O3 of Example 2, 2Ru-In2O3 of Example 3, 3Ru-In2O3 of Example 4, 2Rh-In2O3 of Example 5 and In2O3 of Comparative Example 1 as catalysts, and conducts carbon dioxide hydrogenation activity experimental tests respectively, and the test results are shown in Table 1.

[0125] The test method is:

[0126] 1) The 4Pt-In2O3 of Example 1, the 2Pd-In2O3 of Example 2, the 2Ru-In2O3 of Example 3, the 3Ru-In2O3 of Example 4, the 2Rh-In2O3 of Example 5 and the In2O3 of Comparative Example 1 were respectively tableted and granulated to obtain catalyst particles with a particle size of 80 to 120 mesh corresponding to Examples 1 to 5 and Comparative Example 1.

[0127] 2) Weigh 0.2 g of catalyst particles corresponding to Examples 1 to 5 and Comparative Example 1 respectively, mix with equal volumes of 80-120 mesh quartz sand and load into a stainless steel reaction tube, introduce 10H2 / Ar gas at 300°C for in-situ reduction for 1 h under atmospheric pressure, introduce feed gas for carbon dioxide hydrogenation reaction, and heat at 3.0 MPa and mass space velocity 9000 mL / g cat h, and the reaction products were detected by TCD and FID detectors under the reaction conditions of 260-300°C. The raw gas was a mixed gas of H2:CO2:N2=73:24:3. The evaluation results are shown in Table 1.

[0128] Table 1 Test results of catalyst catalytic carbon dioxide hydrogenation performance

[0129]

[0130] from Figure 1 , 2 As can be seen from Table 1, Examples 1 to 5 use the method provided by the present invention to prepare highly dispersed precious metal-doped indium oxide catalysts without changing the crystal phase and morphology of indium oxide. When used to catalyze the hydrogenation of carbon dioxide to produce methanol, the carbon dioxide conversion rate is significantly increased compared with the catalyst prepared in Comparative Example 1. Among them, 2Pd-In2O3 has a methanol selectivity of up to 80.2% at a reaction temperature of 300°C, and has the best catalytic performance.

[0131] Obviously, the above embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

Claims

1. A highly dispersed noble metal modified indium oxide catalyst, characterized in that: Used for preparing methanol by hydrogenating carbon dioxide, the highly dispersed noble metal-modified indium oxide catalyst comprises an active component and a doped noble metal; The active component is hexagonal indium oxide with a nanowire multi-level structure; The doped noble metal is dispersedly doped in the active component in the form of atomic level, and the doped noble metal is any one of Pt, Pd, Ru and Rh; The doped noble metal accounts for 1% to 5% of the mass of the highly dispersed noble metal-modified indium oxide catalyst.

2. The highly dispersed noble metal modified indium oxide catalyst according to claim 1, characterized in that The highly dispersed noble metal-modified indium oxide catalyst is obtained by introducing the doped noble metal into the active component through a hydrothermal method.

3. A method for preparing a highly dispersed noble metal-modified indium oxide catalyst according to any one of claims 1 to 2, characterized in that: The following steps are involved: According to the ratio of the noble metal component to the total mass of the catalyst of 1% to 5%, the corresponding mass of soluble indium salt and soluble noble metal salt are weighed and dispersed in a solvent to obtain a salt solution; Adding a precipitant dropwise into the salt solution and mixing well to obtain a precipitated mother solution; The precipitation mother solution is subjected to a hydrothermal reaction at 100° C. to 180° C., followed by centrifugation, drying and calcination in sequence to obtain the highly dispersed noble metal-modified indium oxide catalyst; Wherein, the soluble precious metal salt is any one of a soluble Pt salt, a soluble Pd salt, a soluble Ru salt and a soluble Rh salt.

4. The preparation method according to claim 3, characterized in that: The soluble indium salt is one or two of indium nitrate tetrahydrate, indium nitrate tetra-point pentahydrate and indium nitrate pentahydrate.

5. The preparation method according to claim 3, characterized in that: The precipitant is urea solution.

6. The preparation method according to claim 3, characterized in that: In the salt solution, the concentration of the soluble indium salt is 0.3 mol / L to 1 mol / L.

7. The preparation method according to claim 3, characterized in that: The calcination temperature is 300°C to 600°C.

8. The preparation method according to claim 3, characterized in that: The hydrothermal reaction time is 10 h to 24 h.

9. The preparation method according to claim 3, characterized in that: The calcination time is 3h to 8h.

10. Use of the highly dispersed noble metal-doped indium oxide catalyst according to any one of claims 1 to 2 in the preparation of methanol by hydrogenation of carbon dioxide.

Citation Information

Patent Citations

  • Indium oxide catalyst and preparation method and application thereof

    CN110479235A

  • Platinum-modified indium-based oxide catalyst as well as preparation method and application thereof

    CN114405505A

  • Preparation and application of metal oxide doped monatomic catalyst for preparing ethanol through CO2 hydrogenation

    CN115254100A

  • Indium oxide loaded monatomic catalyst as well as preparation method and application thereof

    CN115945191A

  • Monatomic Pt-doped indium oxide catalyst as well as preparation method and application thereof

    CN118179498A

Cited By

  • Monatomic noble metal catalyst as well as preparation method and application thereof

    CN119746851A