Ruthenium catalyst for alkylanthraquinone hydrogenation and preparation method thereof
The preparation of rare earth metal-modified ruthenium catalysts through microwave hydrothermal-immersion methods has solved the problem of complex and high cost in the preparation process of alkyl anthraquinone hydrogenation catalysts in the prior art, and achieved high activity, stability and low cost hydrogen peroxide production .
Patent Information
- Application Number
- CN202410781720.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, the preparation process of alkyl anthraquinone hydrogenation catalysts is complex, the use of a large number of organic solvents, the catalyst activity is poor, and the Pd catalyst is expensive, which limits the production efficiency and cost control of hydrogen peroxide.
The ruthenium catalyst modified by rare earth metal is prepared by microwave hydrothermal-impregnation method. By reacting the ruthenium precursor with the additive metal salt in a microwave hydrothermal kettle, the additive modified ruthenium nanoparticle colloid is formed, and then impregnated with alumina powder. Wash, dry and reduce activation to obtain a high-activity and low-cost alkylanthraquinone hydroruthenon catalyst.
The activity and stability of the ruthenium catalyst is significantly higher than that of the Pd/Al2O3 catalyst under normal pressure, and the preparation process is energy-saving and environmentally friendly, with low cost. The additive metal of the catalyst shows atomic cluster-level dispersion on the support surface, which significantly improves the catalytic effect.
Smart Images

Figure CN118904333A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalysts, and in particular relates to a ruthenium catalyst for hydrogenation of alkyl anthraquinone and a preparation method thereof. Background Art
[0002] Hydrogen peroxide (H 2 O 2 ) is an important inorganic chemical raw material, which is widely used in chemical synthesis, textiles, medicine, electronics, food and metallurgy. Anthraquinone method has become the mainstream method for producing hydrogen peroxide due to its advantages of large scale, low energy consumption, low cost and easy operation. Anthraquinone method for producing hydrogen peroxide is mainly carried out in two steps of hydrogenation and oxidation of alkyl anthraquinone, in which the selective hydrogenation of alkyl anthraquinone is 2 O 2 The yield is crucial. In order to improve the activation ability of the C=O bond on the alkyl anthraquinone molecule and reduce the production of degradation products, it is particularly important to develop an efficient hydrogenation catalyst.
[0003] As one of the alkyl anthraquinone hydrogenation catalyst systems, Pd catalyst has the characteristics of high activity, operation resistance, long life and easy recovery, and has attracted widespread attention, becoming the mainstream alkyl anthraquinone hydrogenation catalyst on the market. However, the price of Pd has remained high for a long time, which has become a key issue restricting its widespread application. Ru, as the cheapest platinum group metal, has a greater price advantage than Pt, Rh, and Pd. At the same time, it has better stability than industrial Ni-based catalysts (not easy to spontaneously combust), and may be a new generation of anthraquinone hydrogenation catalyst with great development potential. For example, patent CN108057438A also reported that Ru / Al prepared by polyol reduction method 2 O 3 The catalyst was used in the hydrogenation reaction of alkyl anthraquinone, and the results showed that it had high reaction selectivity, but the catalyst activity was relatively low, resulting in the use of Ru metal equivalent to 20 times the amount of industrial palladium catalyst Pd under similar hydrogen efficiency conditions, which greatly increased the production cost.
[0004] In recent years, microwaves have been widely used in industrial production as a special green heating method due to their special energy transfer and conversion methods. Compared with traditional methods, microwave technology has significant advantages such as high efficiency, fast speed, high resource recycling rate, low energy consumption, and no pollution to the environment. For example, patent CN102658207A successfully prepared a highly dispersed Pd catalyst using microwave reaction technology, but the anthraquinone hydrogenation activity of the catalyst was poor, and a large amount of organic tin solvents were introduced during the catalyst preparation process. A large amount of by-products caused great damage to the environment, limiting the development of this method; patent CN105268433A also successfully prepared a series of highly dispersed platinum group catalysts using microwave heating, but this method H 2 O2 The yield is low, and a large amount of alcohol reducing agents and polymer protective agents are introduced during the preparation process, which makes the preparation process complicated and increases the production cost investment, making this solution difficult to industrialize. Summary of the invention
[0005] In view of the problems existing in the prior art such as complex preparation process, large amount of organic solvent used, poor anthraquinone hydrogenation activity, high cost of Pd catalyst, etc., the present invention provides a ruthenium catalyst for alkyl anthraquinone hydrogenation and a preparation method thereof. The present invention successfully prepares a series of rare earth metal modified ruthenium catalysts by microwave hydrothermal-impregnation method. The ruthenium catalyst is used for alkyl anthraquinone hydrogenation reaction, and has a significantly higher Pd / Al ratio under normal pressure. 2 O 3 The catalyst is active and has a very high stability.
[0006] The first aspect of the present invention provides a ruthenium catalyst for hydrogenation of an alkyl anthraquinone, comprising a carrier Al 2 O 3 , active component ruthenium and auxiliary metal elements; The auxiliary metal element is selected from one or more rare earth elements; The loading amount of the active component ruthenium is 0.5-5% of the mass of the carrier, and the loading amount of the active component ruthenium is calculated based on the mass of the ruthenium metal element.
[0007] The second aspect of the present invention provides a method for preparing a ruthenium catalyst for hydrogenation of an alkyl anthraquinone, comprising the following steps: a) mixing a solution of a ruthenium precursor with a solution of an auxiliary metal salt, adding a dispersant and a pH adjuster, and reacting them in a microwave hydrothermal reactor to obtain an auxiliary-modified ruthenium nanoparticle colloidal solution; b) dispersing the carrier alumina powder into water, adding the ruthenium nanoparticle colloidal solution in step a), stirring, impregnating, washing, filtering, and drying to obtain a catalyst precursor; c) reducing and activating the catalyst precursor of step b) in an atmosphere containing a reducing gas to obtain the alkylanthraquinone hydrogenation ruthenium catalyst.
[0008] Optionally, the ruthenium precursor is selected from metal salts of ruthenium, preferably one or more of ruthenium chloride, potassium ruthenate, ruthenium acetate, ruthenium nitrate, carbonyl ruthenium, and the like.
[0009] Optionally, the auxiliary metal salt includes one or more of nitrates, chlorides, sulfates, acetates, etc. of rare earth elements; the rare earth elements include lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium, and yttrium.
[0010] Optionally, the molar ratio of the auxiliary metal salt to the ruthenium precursor is 0.1:1 to 5:1.
[0011] Optionally, the dispersant is selected from one or more of polyethylene glycol, polyvinyl alcohol, polypyrrolidone, sodium hexadecylbenzene sulfonate, sodium dodecyl sulfate, methanol, ethanol, polyacrylamide, and the like.
[0012] Optionally, the molar ratio of the dispersant to Ru atoms is 1:1 to 50:1.
[0013] Optionally, the pH adjuster mainly includes acids and bases such as sulfuric acid, nitric acid, hydrochloric acid, potassium hydroxide, sodium carbonate, potassium bicarbonate, etc., and the pH adjustment range is between 4 and 10.
[0014] Optionally, the microwave hydrothermal conditions include: a temperature of 80-250°C, preferably 150-250°C; a reaction time of 10-48 h, and a reaction pressure of 0.1-2.0 MPa.
[0015] Optionally, the carrier alumina powder is selected from alumina with different phase compositions such as γ, Δ, θ, α, etc.
[0016] Optionally, the catalyst impregnation temperature is between 25 and 50°C, and the impregnation time is between 30 and 120 minutes.
[0017] Optionally, the catalyst is dried at a temperature of 80 to 200 °C for 2 to 6 h.
[0018] Optionally, the activation conditions include: the reducing gas is mainly H 2 , reducing gas accounts for 5~10% of the total volume, and the remaining 95~90% of the gas is N 2 , Ar and other inert gases.
[0019] Optionally, the catalyst activation temperature is 300-700°C and the reaction pressure is normal pressure.
[0020] The ruthenium catalyst of the present invention is used in the alkyl anthraquinone hydrogenation catalytic reaction. The test method is to hydrate the ruthenium catalyst and the working solution in pure hydrogen at 1-5 °C·min -1 The temperature is raised to 50-80 °C to carry out the alkyl anthraquinone hydrogenation catalytic reaction. The working fluid consists of heavy aromatics, 2-ethyl anthraquinone and tetrabutyl urea, and the reaction pressure is 0.1-2.0 MPa.
[0021] The ruthenium catalyst for hydrogenation of alkyl anthraquinone prepared by the preparation method of the present invention has the advantages of high activity, good stability and low cost. Compared with the prior art, the beneficial effects produced by the catalyst provided by the present invention include: 1) With simple impregnation of Pd / Al 2 O 3Compared with the catalyst, the supported ruthenium catalyst provided by the present invention has higher activity under normal pressure and has quite high stability.
[0022] 2) Compared with the general hydrothermal reaction, the preparation method of the ruthenium catalyst for hydrogenation of alkyl anthraquinone provided by the present invention has the advantages of energy saving and environmental protection, high degree of controllability of conditions, and significantly improved interaction between Ru and auxiliary metal.
[0023] 3) The preparation method of the supported ruthenium catalyst provided by the present invention, wherein the auxiliary metal is in the form of Al 2 O 3 The surface of the carrier clearly shows atomic cluster-level dispersion. This form of additive significantly improves the interaction between Ru and the carrier, resulting in an excellent catalytic effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 2 wt.% Ru in Example 1 1 Ce 0.5 / Al 2 O 3 Catalyst and 2% Ru / Al in Comparative Example 1 2 O 3 High-resolution transmission electron microscopy images and particle size distribution results after the catalyst reaction (a is a high-resolution transmission electron microscopy image of Example 1, b is a high-resolution transmission electron microscopy image of Comparative Example 1, c is a statistical result of particle size distribution of Example 1, and d is a statistical result of particle size distribution of Comparative Example 1); Figure 2 2 wt.% Ru in Example 1 1 Ce 0.5 / Al 2 O 3 High-angle annular dark-field elemental imaging of the catalyst; Figure 3 These are the test results of the anthraquinone hydrogenation reaction cycle performance of the catalysts prepared in Example 1 and Comparative Examples 1-3. DETAILED DESCRIPTION
[0025] The present invention is described in detail below with reference to the examples, but is not limited to the examples. Unless otherwise specified, all numbers appearing in the specification and claims of the present invention, such as loading, temperature, time and other numerical values, should not be understood as absolute precise values. Due to the standard deviation of the measurement technology, the measured values will inevitably have certain experimental errors.
[0026] The reaction performance of the prepared catalyst was evaluated using an alkyl anthraquinone hydrogenation device. The device was a 100 mL stainless steel reactor with a polytetrafluoroethylene liner. Before the reaction, N 2 Repeat the replacement several times until the oxygen volume fraction is less than 2%, then introduce H2 The working solution is composed of heavy aromatics, tetrabutyl urea, and 2-ethylanthraquinone. The volume ratio of Ar to TBU is 3:1, and the dissolved amount of 2-ethylanthraquinone is 120 g L -1 ; Add 0.2 g of catalyst to the reactor, maintain the temperature at 65 °C and the hydrogen partial pressure at 0.1 MPa, stop aeration after 30 min of reaction, extract the obtained hydrogen peroxide, and calculate the hydrogenation efficiency by titration with standard potassium permanganate solution.
[0027] A transmission electron microscope (model: JEOL 2100X, purchased from JEOL, Japan) was used to observe the existence form and size of the metal in the catalyst sample.
[0028] The high-angle annular dark-field image of the sample was observed using a spherical aberration-corrected electron microscope of the American ThermoFisher model, and it was equipped with an EDX-Mapping image acquisition function.
[0029] The precious metal loading was tested by inductively coupled plasma instrument.
[0030] Example 1
[0031] Dissolve 0.3 g of ruthenium nitrate in 10 mL of water, then take 0.22 g of Ce(NO 3 ) 3 6H 2 O was dissolved in 10 mL of water, and after the two were mixed evenly, 2 mL of polyethylene glycol solution was added, and 0.1 g of K 2 CO 3 The pH of the mixed solution was adjusted between 5 and 6, and a hydrothermal reaction was carried out in a 50 mL microwave reactor. The reaction temperature was controlled at about 160 ° C and the pressure was about 0.3 MPa. The reaction was then maintained for 8 h. The obtained colloidal solution was stirred evenly at room temperature, 5 g of alumina powder was added and impregnated for 2 h, then washed and filtered, dried at 120 ° C for 4 h, and finally reduced at 500 ° C in a hydrogen atmosphere for 2 h to obtain 2 wt. % Ru 1 Ce 0.5 / Al 2 O 3 catalyst.
[0032] Figure 1 High-resolution transmission electron microscopy (a) and particle size distribution (c) results show that the above 2 wt. % Ru 1 Ce 0.5 / Al 2 O 3 The Ru in the catalyst is highly dispersed, with an average size of 2.3 nm.
[0033] Figure 2Middle: (a) is a local dark field image of the catalyst at shooting angle 1, (b) is a local dark field image of the catalyst at shooting angle 2, and cf is an elemental mapping diagram of the catalyst at shooting angle 2 (b). (a) The high-angle annular dark field image shows that many Ce atomic clusters are dispersed around large particles of Ru metal, demonstrating the strong interaction between Ce and Ru nanoparticles. At the same time, the modification of Ce may lead to better reaction performance of Ru catalysts. In order to further illustrate the elemental species distribution given by this dark field image, from Figure 2 (b) and the following four element mapping diagrams show that in the whole carrier Al 2 O 3 The above graph shows obvious Al and O element characteristics, while the corresponding positions of the large particle bright spots show obvious dense Ru element distribution. The scattered tiny bright spots in the figure correspond to discrete Ce elements, suggesting the existence of Ce species in the form of atomic clusters.
[0034] The reaction performance of the prepared catalyst was then evaluated. Under the reaction conditions of 0.1 MPa pressure and 65 °C temperature, the hydrogenation efficiency was measured to be 11.01 g·L -1 .
[0035] Example 2
[0036] 0.05 g of ruthenium chloride was dissolved in 10 mL of water, and then 0.045 g of La(NO 3 ) 3 6H 2 O was dissolved in 10 mL of water, and after the two were mixed evenly, 1.2 g of polypyrrolidone was added, and 0.1 g of Na 2 CO 3 The pH of the mixed solution was adjusted between 4 and 5, and a hydrothermal reaction was carried out in a 50 mL microwave reactor. The reaction temperature was controlled at about 200 °C and the pressure was about 0.8 MPa. The reaction was then maintained for 24 h. The obtained colloidal solution was stirred evenly at 50 °C, 5 g of alumina powder was added and impregnated for 0.5 h, then washed and filtered, dried at 80 °C for 6 h, and finally reduced at 300 °C in a hydrogen atmosphere for 2 h to obtain 0.5 wt. %Ru 1 La 0.1 / Al 2 O 3 catalyst.
[0037] The reaction performance of the prepared catalyst was then evaluated. Under the reaction conditions of 0.1 MPa reaction pressure and 50 °C temperature, the hydrogenation efficiency was measured to be 4.78 g·L -1 .
[0038] Example 3
[0039] 0.6 g potassium ruthenate was dissolved in 10 mL water, and then 0.39 g Y(NO 3 ) 3 6H 2 O was dissolved in 10 mL of water. After the two were mixed evenly, 1.2 g of polyacrylamide was added, and 0.5 g of NaOH was added dropwise to adjust the pH of the mixture to between 9 and 10. The hydrothermal reaction was carried out in a 50 mL microwave reactor. The reaction temperature was controlled at about 250 °C and the pressure was about 2.0 MPa. Then it was kept for 23 h. The obtained colloidal solution was stirred evenly at 30 °C, 5 g of alumina powder was added and impregnated for 1 h, then washed and filtered, dried at 100 °C for 5 h, and finally reduced at 700 °C in a hydrogen atmosphere for 2 h to obtain 5 wt. % Ru 1 Y 1 / Al 2 O 3 catalyst.
[0040] The reaction performance of the prepared catalyst was then evaluated. Under the reaction conditions of a reaction pressure of 2.0 MPa and a temperature of 80 °C, the hydrogenation efficiency was measured to be 14.88 g·L -1 .
[0041] Example 4
[0042] 0.4 g of ruthenium acetate was dissolved in 10 mL of water, and then 2.5 g of Pr(CH 3 COO 3 Dissolve in 10 mL of water, mix well, add 1.3 mL of sodium hexadecylbenzenesulfonate solution, and then add 2.4 g of K 2 CO 3 The pH of the mixed solution was adjusted between 4 and 5, and a hydrothermal reaction was carried out in a 50 mL microwave reactor. The reaction temperature was controlled at about 80 °C and the pressure was about 0.1 MPa. The reaction was then maintained for 48 h. The obtained colloidal solution was stirred evenly at room temperature, 5 g of alumina powder was added and impregnated for 2 h, then washed and filtered, dried at 120 °C for 4 h, and finally reduced at 600 °C in a hydrogen atmosphere for 2 h to obtain 2 wt. % Ru 1 Pr 5 / Al 2 O 3 catalyst.
[0043] The reaction performance of the prepared catalyst was then evaluated. Under the reaction conditions of 0.1 MPa pressure and 65 °C temperature, the hydrogenation efficiency was measured to be 9.43 g·L -1 .
[0044] Example 5
[0045] Dissolve 0.2 g of carbonylruthenium in 10 mL of tetrahydrofuran solution, then take 0.23 g of SmCl 3 6H 2 O was dissolved in 10 mL of water, and after the two were mixed evenly, 2 mL of methanol solution was added, and 0.6 mL of ammonia water was added dropwise to adjust the pH of the mixture to between 5 and 6. The hydrothermal reaction was carried out in a 50 mL microwave reactor, and the reaction temperature was controlled at about 130 °C and the pressure was about 0.3 MPa. Then it was kept for 8 h. The obtained colloidal solution was stirred evenly at room temperature, 5 g of alumina powder was added and impregnated for 2 h, then washed and filtered, dried at 120 °C for 4 h, and finally reduced at 400 °C in a hydrogen atmosphere for 2 h to obtain 2 wt. % Ru 1 Sm 0.5 / Al 2 O 3 catalyst.
[0046] The reaction performance of the prepared catalyst was then evaluated. Under the reaction conditions of 0.1 MPa pressure and 65 °C temperature, the hydrogenation efficiency was measured to be 10.75 g·L -1 .
[0047] Example 6
[0048] 0.3 g of ruthenium nitrate was dissolved in 10 mL of aqueous solution, and then 0.52 g of Eu 2 (SO 4 ) 3 8H 2 O was dissolved in 10 mL of water, and after the two were mixed evenly, 2 mL of polyvinyl alcohol solution was added, and 1.7 mL of ammonia water was added dropwise to adjust the pH of the mixture to between 8 and 9. The hydrothermal reaction was carried out in a 50 mL microwave reactor, and the reaction temperature was controlled at about 110 ° C and the pressure was about 0.2 MPa, and then maintained for 19 h. The obtained colloidal solution was stirred evenly at 30 ° C, 5 g of alumina powder was added and immersed for 2 h, and then washed and filtered, and dried at 120 ° C for 4 h, and finally reduced at 600 ° C in a hydrogen atmosphere for 2 h to obtain 2wt. % Ru 1 Eu 0.5 / Al 2 O 3 catalyst.
[0049] The reaction performance of the prepared catalyst was then evaluated. Under the reaction conditions of 0.1 MPa pressure and 65 °C temperature, the hydrogenation efficiency was measured to be 8.74 g·L -1 .
[0050] Example 7
[0051] 0.3 g of ruthenium nitrate was dissolved in 10 mL of aqueous solution, and then 0.28 g of Dy(NO 3 ) 3 6H 2 O was dissolved in 10 mL of water. After the two were mixed evenly, 2 mL of sodium dodecyl sulfate solution was added, and 0.4 g of sodium bicarbonate was added dropwise to adjust the pH of the mixture to between 7 and 8. The hydrothermal reaction was carried out in a 50 mL microwave reactor. The reaction temperature was controlled at about 190 °C and the pressure was about 0.8 MPa. Then it was kept for 15 h. The obtained colloidal solution was stirred evenly at 30 °C, 5 g of alumina powder was added and impregnated for 2 h, then washed and filtered, dried at 120 °C for 4 h, and finally reduced at 600 °C in a hydrogen atmosphere for 2 h to obtain 2 wt. % Ru. 1 Dy 0.5 / Al 2 O 3 catalyst.
[0052] The reaction performance of the prepared catalyst was then evaluated. Under the reaction conditions of 0.1 MPa pressure and 65 °C temperature, the hydrogenation efficiency was measured to be 7.49 g·L -1 .
[0053] Example 8
[0054] 0.3 g of ruthenium nitrate was dissolved in 10 mL of aqueous solution, and then 0.21 g of Sc(NO 3 ) 3 6H 2 O was dissolved in 10 mL of water, and after the two were mixed evenly, 2 mL of polyvinyl alcohol solution was added, and 0.6 g of potassium bicarbonate was added dropwise to adjust the pH of the mixture to between 8 and 9. The hydrothermal reaction was carried out in a 50 mL microwave reactor, and the reaction temperature was controlled at about 220 ° C and the pressure was about 1.5 MPa, and then maintained for 10 h. The obtained colloidal solution was stirred evenly at 30 ° C, 5 g of alumina powder was added and immersed for 2 h, and then washed and filtered, and dried at 120 ° C for 4 h. Finally, it was reduced at 600 ° C in a hydrogen atmosphere for 2 h to obtain 2wt. % Ru 1 Sc 0.5 / Al 2 O 3 catalyst.
[0055] The reaction performance of the prepared catalyst was then evaluated. Under the reaction conditions of 0.1 MPa pressure and 65 °C temperature, the hydrogenation efficiency was measured to be 9.98 g·L -1 .
[0056] Example 9
[0057] 0.3 g of ruthenium nitrate was dissolved in 10 mL of aqueous solution, and then 0.24 g of La(NO 3 ) 3 6H 2 O and 0.24g Ce(NO 3 ) 3 6H 2 O was dissolved in 10 mL of water. After the two were mixed evenly, 2 mL of polyvinyl alcohol solution was added, and 0.6 g of potassium bicarbonate was added dropwise to adjust the pH of the mixture to between 7 and 8. The hydrothermal reaction was carried out in a 50 mL microwave reactor. The reaction temperature was controlled at about 180 °C and the pressure was about 1.0 MPa. Then it was kept for 18 h. The obtained colloidal solution was stirred evenly at 30 °C, 5 g of alumina powder was added and impregnated for 2 h, then washed and filtered, dried at 120 °C for 4 h, and finally reduced at 600 °C in a hydrogen atmosphere for 2 h to obtain 2 wt. % Ru 1 La 0.5 Ce 0.5 / Al 2 O 3 catalyst.
[0058] The reaction performance of the prepared catalyst was then evaluated. Under the reaction conditions of 0.1 MPa pressure and 65 °C temperature, the hydrogenation efficiency was measured to be 10.34 g·L -1 .
[0059] Comparative Example 1
[0060] Without adding Ce(NO 3 ) 3 6H 2 O was used as an auxiliary agent, and the rest of the operations were the same as in Example 1.
[0061] The reaction performance of the prepared catalyst was evaluated. Under the reaction conditions of 0.1 MPa pressure and 65 °C temperature, the hydrogenation efficiency was 2.09 g·L -1 .
[0062] from Figure 1 From b and d, it can be found that 2 wt. % Ru / Al without additives 2 O 3 The catalyst particles are relatively large, with an average particle size of 7.3 nm. Due to the lack of the dispersion aid of rare earth elements, the Ru particles grow larger, reducing the reaction performance.
[0063] Comparative Example 2
[0064] The microwave reaction kettle in Example 1 was replaced by a common hydrothermal kettle, and the remaining operations were the same as in Example 1.
[0065] The reaction performance of the prepared catalyst was evaluated. Under the reaction conditions of 0.1 MPa pressure and 65 °C temperature, the hydrogenation efficiency was 1.23 g·L -1 .
[0066] Compared with Example 1,2 wt. % Ru without microwave hydrothermal treatment 1 Ce 0.5 / Al 2 O 3 The catalyst activity decreased by nearly one order of magnitude, suggesting that the microwave hydrothermal process plays an important role in the dispersion of Ru nanoparticles and the formation of strong interactions between Ru nanoparticles and rare earth elements.
[0067] Comparative Example 3
[0068] 0.2 g of sodium chloropalladate was dissolved in 10 mL of water, and 5 g of alumina powder was added and immersed at room temperature for 2 h. Then, it was washed and filtered, dried at 120 °C for 4 h, and finally reduced at 500 °C in a hydrogen atmosphere for 2 h to obtain 2 wt. % Pd / Al 2 O 3 catalyst.
[0069] The reaction performance of the prepared catalyst was evaluated. Under the reaction conditions of 0.1 MPa pressure and 65 °C temperature, the hydrogenation efficiency was 4.21 g·L -1 .
[0070] Table 1 shows the alkyl anthraquinone hydrogenation activity of the catalysts in Examples 1-9 and Comparative Examples 1-3. It can be seen that the activity of the ruthenium nanoparticle catalyst prepared by microwave hydrothermal-impregnation is significantly higher than that of the Pd / Al prepared by impregnation. 2 O 3 and other comparative catalysts.
[0071] Table 1 Comparison of 2-ethylanthraquinone hydrogenation activity over different catalysts
[0072] Example 10 Anthraquinone hydrogenation reaction cycle test The stability test of the catalysts prepared in Example 1 and Comparative Examples 1-3 was carried out in an alkyl anthraquinone hydrogenation device. The catalysts were tested multiple times in a working solution, the working solution was replaced every 30 minutes, and the activity changes were tested cyclically.
[0073] 2 wt.% Ru in Example 1 1 Ce0.5 / Al 2 O 3 The catalyst has high stability ( Figure 3 ), the activity of the catalyst is also greatly improved compared with that of the comparative examples 1-3.
[0074] The above are only several embodiments of the present invention, and are not intended to limit the present invention in any form. Although the present invention is disclosed as above with preferred embodiments, it is not intended to limit the present invention. Any technician familiar with the profession, without departing from the scope of the technical solution of the present invention, using the above disclosed technical content to make some changes or modifications are equivalent to equivalent embodiments and fall within the scope of the technical solution.
Claims
1. A ruthenium catalyst for hydrogenation of alkyl anthraquinone, comprising a carrier Al2O3, an active component ruthenium and a promoter metal element; The auxiliary metal element is selected from one or more rare earth elements; The loading amount of the active component ruthenium is 0.5-5% of the mass of the carrier, and the loading amount of the active component ruthenium is calculated based on the mass of the ruthenium metal element.
2. A method for preparing the ruthenium catalyst for hydrogenation of alkylanthraquinone according to claim 1, comprising the following steps: a) mixing a solution of a ruthenium precursor with a solution of an auxiliary metal salt, adding a dispersant and a pH adjuster, and reacting them in a microwave hydrothermal reactor to obtain an auxiliary-modified ruthenium nanoparticle colloidal solution; b) dispersing the carrier alumina powder into water, adding the ruthenium nanoparticle colloidal solution in step a), stirring, impregnating, washing, filtering, and drying to obtain a catalyst precursor; c) reducing and activating the catalyst precursor of step b) in an atmosphere containing a reducing gas to obtain the alkylanthraquinone hydrogenation ruthenium catalyst.
3. The preparation method according to claim 2, characterized in that: The ruthenium precursor is selected from metal salts of ruthenium.
4. The preparation method according to claim 3, characterized in that: The metal salt of ruthenium is selected from one or more of ruthenium chloride, potassium ruthenate, ruthenium acetate, ruthenium nitrate and carbonyl ruthenium.
5. The preparation method according to claim 2, characterized in that: The auxiliary metal salt is selected from one or more of nitrates, chlorides, sulfates, acetates, etc. of rare earth elements; the rare earth element is one or more of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium, and yttrium.
6. The preparation method according to claim 2, characterized in that: The molar ratio of the auxiliary metal salt to the ruthenium precursor is 0.1:1 to 5:
1.
7. The preparation method according to claim 2, characterized in that: The molar ratio of the dispersant to Ru atoms is 1:1 to 50:
1.
8. The preparation method according to claim 2, characterized in that: The pH regulator is selected from one or more of sulfuric acid, nitric acid, hydrochloric acid, potassium hydroxide, sodium carbonate, and potassium bicarbonate, and the pH adjustment range is between 4 and 10.
9. The preparation method according to claim 2, characterized in that: The microwave hydrothermal conditions include: temperature of 80-250°C, reaction time of 10-48 h, and reaction pressure of 0.1-2.0 MPa.
10. The preparation method according to claim 2, characterized in that: The reducing gas is H2, which accounts for 5-10% of the total volume, and the remaining 95-90% of the gas is inert gas.
Citation Information
Patent Citations
Supported ruthenium-based catalyst, preparation method thereof and application of supported ruthenium-based catalyst in synthesis ammonia reaction
CN116809060A
Anthraquinone process
US5772977A