Neodymium-doped cobalt-based catalyst capable of resisting interference of water vapor and impurity gas, preparation and application

By doping neodymium to cobalt tetraoxide catalyst, a neodymium-doped cobalt-based catalyst with a mesoporous structure solves the problem of poor thermal stability of the catalyst in industrial exhaust gas, and achieves efficient nitrous oxide decomposition and resistance to water vapor and impurity interference. It is suitable for Industrial production.

CN118904349APending Publication Date: 2024-11-08CHINA JILIANG UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411406406.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-10
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When existing catalysts are interfered with water vapor and impurity gas in industrial exhaust gas, their thermal stability is poor, their catalytic efficiency is reduced, and they are difficult to apply on a large scale.

Method used

By doping neodymium (Nd) into a cobalt tetraoxide (Co3O4) catalyst, a neodymium-doped cobalt-based catalyst with a mesoporous structure was prepared by sol-gel method to enhance the water resistance and impurity interference resistance of the catalyst.

Benefits of technology

It reduces the reaction temperature of catalytic decomposition of nitrous oxide, improves the stability and conversion rate of the catalyst in complex environments, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904349A_ABST
    Figure CN118904349A_ABST
Patent Text Reader

Abstract

The invention discloses a neodymium-doped cobalt-based catalyst capable of resisting interference of water vapor and impurity gas, a preparation method of the neodymium-doped cobalt-based catalyst and application of the neodymium-doped cobalt-based catalyst in catalytic decomposition of nitrous oxide. The neodymium-doped cobalt-based catalyst is a neodymium lattice-doped cobaltosic oxide catalyst with a mesoporous structure, wherein the molar ratio of neodymium to cobalt is (0.02-0.14): 1. The preparation method comprises the following steps: preparing a mixed solution containing cobalt nitrate, neodymium nitrate, urea and citric acid, stirring and heating to form gel, and then drying and roasting to obtain the neodymium-doped cobalt-based catalyst. Through lattice doping of neodymium, the activity of the cobaltosic oxide-based catalyst is enhanced, the reaction temperature of the catalyst for catalytic decomposition of nitrous oxide is reduced, and the anti-interference performance of the catalyst in a complex environment in which NO, O2 and other foreign gases and water vapor exist is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of environmental protection catalytic materials and air pollution control, and in particular to a neodymium-doped cobalt-based catalyst resistant to interference from water vapor and impurity gases, and a preparation method and application thereof. Background Art

[0002] Nitrous oxide (also known as nitrous oxide, N2O) is a type of greenhouse gas with an emission impact second only to carbon dioxide (CO2) and methane (CH4). Its global warming potential is 21 times that of CH4 and 310 times that of CO2. Its harm to the environment has received increasing attention. In addition to its extremely strong greenhouse effect, due to its stable structural characteristics, N2O can stably exist in the atmospheric troposphere, and when it moves to the stratosphere with the atmosphere, it can have a strong destructive effect on the ozone layer. Currently, N2O has become one of the substances that most seriously damage ozone, and the degree of damage is increasing year by year.

[0003] At present, the main sources of N2O emissions are agricultural and industrial. Compared with other sources, the emissions from industrial sources are controllable. Among industrial sources, N2O in the tail gas from nitric acid and adipic acid production is the main source of industrial production emissions, accounting for more than 97%. Therefore, the focus of research on reducing N2O emissions is to reduce the emission of N2O in the tail gas from nitric acid and adipic acid production. The components of the tail gas from nitric acid and adipic acid production are relatively complex, with the main components being N2O, NO x (nitrogen oxides), CO2, O2 (oxygen), SO2 (sulfur dioxide), water vapor and some trace gas impurities.

[0004] At present, there are mainly direct catalysis, thermal decomposition and selective catalytic reduction for reducing N2O emissions in industrial tail gas. Among them, direct catalysis is the current mainstream N2O emission reduction technology, which has the advantages of simple technical route, low economic cost and no by-products. The catalyst is the key to direct catalyst N2O, which can directly catalyze and decompose N2O into N2 and O2. At present, researchers have developed many types of catalysts for direct catalysis of N2O, which are mainly divided into three categories, namely precious metal catalysts, molecular sieve catalysts and metal oxide catalysts.

[0005] Precious metals such as gold (Au), silver (Ag), palladium (Pd), platinum (Pt), and rhodium (Rh) are used as active components and loaded on carriers such as metal oxides or molecular sieves. They have the characteristics of strong activity and high conversion rate. For example, Patent Document 1 discloses the use of precious metal iridium (Ir) as the main active component, loaded on CHA type microporous molecular sieve SSZ-13, to obtain a catalyst and catalytically decompose N2O. However, it is inevitable that precious metals are not suitable for large-scale application in industrial production due to their high prices and scarce storage.

[0006] Molecular sieve catalysts are mainly prepared by selecting transition metals (such as iron, cobalt, nickel and copper) and exchanging ions with molecular sieves (mainly ZSM-5) to obtain catalysts. For example, Patent Document 2 discloses a molecular sieve catalyst that uses copper as an active component and performs ion exchange with MFI molecular sieves to prepare a catalyst with high catalytic efficiency. Although molecular sieve catalysts have the advantage of high conversion efficiency, molecular sieves are prone to irreversible deactivation in a hydrothermal environment, and industrial production tail gas often contains water vapor, which can cause serious interference to the catalytic efficiency of molecular sieve catalysts.

[0007] Metal oxide catalysts are the most widely used and studied catalysts at present. They have the advantages of simple preparation, low cost, easy structure control, and high conversion efficiency in the medium and low temperature stages. In particular, cobalt-based catalysts, whose spinel structure helps to increase the rate of catalytic decomposition of N2O. For example, Patent 3 cited discloses a cobalt-based catalyst, which uses Co3O4 as an active component and cerium dioxide as an auxiliary agent, and uses an impregnation method to prepare a catalyst with high N2O catalytic decomposition efficiency. However, due to the characteristics of its own structure, cobalt-based catalysts have poor thermal stability and are easily deactivated by impurities such as O2, H2O and NO contained in real exhaust gas.

[0008] Based on the above situation, in combination with industrial tail gas, the preparation of metal oxide catalysts with high activity, high medium and low temperature conversion rate, water resistance and resistance to impurity interference will be the focus of future research.

[0009] Existing patent technology literature: Patent document 1: CN112973777A; Patent document 2: CN105749959A; Patent document 3: CN105289654A. Summary of the invention

[0010] In view of the above technical problems and the shortcomings in the art, the present invention provides a neodymium (Nd)-doped cobalt-based catalyst that can directly catalyze and decompose nitrous oxide and resist the interference of water vapor and impurity gases, as well as a preparation method and application thereof. The present invention enhances the activity of cobalt tetraoxide (Co3O4)-based catalysts by lattice doping with neodymium, reduces the reaction temperature of the catalyst for catalytic decomposition of nitrous oxide, and improves the anti-interference ability of the catalyst in complex environments where impurity gases such as NO and O2 and water vapor exist. The present invention discloses the application of a catalyst for removing nitrous oxide in a scenario where water vapor and impurity gases exist.

[0011] In the first aspect, the present invention provides a neodymium-doped cobalt-based catalyst that can directly catalyze the decomposition of nitrous oxide and is resistant to interference from water vapor and impurity gases. The neodymium-doped cobalt-based catalyst is a cobalt tetroxide catalyst doped with a neodymium lattice having a mesoporous structure, wherein the molar ratio of neodymium to cobalt is 0.02~0.14:1, for example, 0.04:1, 0.06:1, 0.08:1, 0.1:1, 0.12:1, etc., preferably 0.08~0.1:1, and further preferably 0.08:1.

[0012] In some embodiments, the average particle size of the neodymium-doped cobalt-based catalyst described in the first aspect is less than 15 nm, and further less than 10 nm.

[0013] In some embodiments, the specific surface area of ​​the neodymium-doped cobalt-based catalyst of the first aspect is greater than 20 m 2 / g, further greater than 60 m 2 / g.

[0014] In a second aspect, the present invention provides a method for preparing the neodymium-doped cobalt-based catalyst described in the first aspect, comprising: preparing a mixed solution containing cobalt nitrate, neodymium nitrate, urea (which can act as a fuel to promote oxidative combustion) and citric acid (which can act as a chelating agent), stirring and heating to form a gel, and then drying and calcining to obtain the neodymium-doped cobalt-based catalyst.

[0015] The present invention uses Co3O4 as an active component, doped with Nd, and adopts a sol-gel method to prepare a catalyst, which ensures high activity of the catalyst while enabling the catalyst to maintain a high conversion rate and anti-interference and resurrection performance in an environment of O2, H2O and NO.

[0016] In some embodiments, in the method for preparing a neodymium-doped cobalt-based catalyst described in the second aspect, the Co concentration in the mixed solution may be 0.1~1 mol / L, for example, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, etc.

[0017] In some embodiments, in the method for preparing the neodymium-doped cobalt-based catalyst described in the second aspect, the solvent in the mixed liquid may be water.

[0018] In some embodiments, in the preparation method of the neodymium-doped cobalt-based catalyst described in the second aspect, the molar ratio of cobalt nitrate, neodymium nitrate, urea and citric acid can be 1:(0.02~0.14):4~6:(2~6), preferably 1:(0.02~0.14):4~6:(2~4). The inventors have found that if the amount of urea is insufficient, the oxidation combustion process during the roasting process will be insufficient, and the roasting product will not be a fine powder. For example, when the molar ratio of cobalt nitrate, neodymium nitrate, urea and citric acid is 1:(0.02~0.14):0~2:(2~6), the roasting product is in a block shape, indicating that the oxidation combustion during the roasting process is insufficient and is not the target product required by the present invention.

[0019] In the method for preparing the neodymium-doped cobalt-based catalyst described in the second aspect, the heating is sufficient to evaporate the solution into a gel state.

[0020] In some embodiments, in the method for preparing the neodymium-doped cobalt-based catalyst described in the second aspect, the heating may be water bath heating.

[0021] In some embodiments, in the method for preparing the neodymium-doped cobalt-based catalyst described in the second aspect, the heating temperature may be 70-90° C., for example, 80° C.

[0022] In some embodiments, in the method for preparing the neodymium-doped cobalt-based catalyst described in the second aspect, the drying temperature may be 100-130° C. (eg, 110° C., etc.), and the drying time may be 10-24 h (eg, 12 h, etc.).

[0023] In some embodiments, in the method for preparing the neodymium-doped cobalt-based catalyst described in the second aspect, the heating rate of the calcination may be 1 to 10° C. / min, preferably 1 to 5° C. / min.

[0024] In some embodiments, in the method for preparing the neodymium-doped cobalt-based catalyst described in the second aspect, the calcination insulation temperature may be 400-600°C, preferably 400-500°C.

[0025] In some embodiments, in the method for preparing the neodymium-doped cobalt-based catalyst described in the second aspect, the calcination holding time can be 3 to 7 hours, preferably 5 to 7 hours.

[0026] In some embodiments, in the method for preparing the neodymium-doped cobalt-based catalyst described in the second aspect, the calcination atmosphere can be an air atmosphere or a nitrogen atmosphere, preferably an air atmosphere.

[0027] In a third aspect, the present invention provides use of the neodymium-doped cobalt-based catalyst described in the first aspect in catalytic decomposition of nitrous oxide.

[0028] In some preferred embodiments, the neodymium-doped cobalt-based catalyst is pretreated in an inert atmosphere at 450-500° C. for 0.2-1.5 (or further 0.5-1) hours before being used to catalyze the decomposition of nitrous oxide. The inert atmosphere refers to a gas atmosphere that does not participate in the reaction, such as a nitrogen atmosphere and / or a rare gas atmosphere (such as argon, etc.).

[0029] The neodymium-doped cobalt-based catalyst can be used to treat polluted gas containing nitrous oxide. Further, the treatment temperature can be 100-750°C, such as 350°C, 500°C, etc. Using the catalyst of the present invention, the minimum temperature for complete catalytic decomposition of N2O can reach 350°C.

[0030] In some embodiments, the polluted gas may further contain zero, one or more of oxygen, water vapor and nitric oxide.

[0031] In some embodiments, the polluted gas may contain 0-5 vol% oxygen, 0-5 vol% water vapor, and 0-100 ppm nitrogen monoxide.

[0032] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention adopts highly active cobalt tetroxide as the basic active component and dopes the lattice with neodymium. While ensuring the original high activity of the cobalt-based catalyst, the catalyst's water resistance and resistance to interference from impurity gases are increased. Compared with other catalysts, it has great advantages in actual industrial production.

[0033] 2. Compared with other metal oxide catalysts, the catalyst prepared by the sol-gel method of the present invention has a larger specific surface area, a smaller grain size and better stability. Therefore, the catalyst has the advantages of high conversion rate, strong thermal stability and high catalytic efficiency in the medium and low temperature stages.

[0034] 3. The catalyst prepared by the present invention uses cobalt as the basic active element, which has abundant underground reserves, is cheap and easy to obtain. At the same time, the preparation method adopted by the present invention is simple in technology, has a low threshold, and has a low overall cost. It is suitable for large-scale industrial production and has good application potential. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 The present invention is a schematic flow chart of a method for preparing a neodymium-doped cobalt-based catalyst that can directly catalyze the decomposition of nitrous oxide and resist interference from water vapor and impurity gases.

[0036] Figure 2 The performance comparison chart of the catalysts prepared in Examples 1 to 9 and Comparative Example 1 is shown.

[0037] Figure 31 and 2 are X-ray diffraction (XRD) diagrams of the catalysts prepared in Examples 1 to 6 and Comparative Example 1, wherein A is an overall diagram and B is a local magnified diagram of the peak position corresponding to the (311) crystal plane.

[0038] Figure 4 Graphs showing the nitrogen adsorption and desorption test results of the catalysts prepared in Examples 1 to 6 and Comparative Example 1; wherein: A is an isothermal adsorption curve graph of the catalysts prepared in Examples 1-6, and B is a pore size distribution graph of the catalysts prepared in Examples 1-6.

[0039] Figure 5 This is a transmission electron microscope (TEM) particle size statistics diagram of the catalyst prepared in Comparative Example 1.

[0040] Figure 6 This is the TEM particle size statistics of the catalyst prepared in Example 1.

[0041] Figure 7 The graph is a test result of catalyst activity in Example 1 and Examples 10-13.

[0042] Figure 8 This is a performance comparison chart of the catalysts prepared in Example 1 and Examples 14-15.

[0043] Fig. 9 This is a performance comparison chart of the catalysts prepared in Example 1 and Examples 16-17.

[0044] Fig.10 This is a performance comparison chart of the catalysts prepared in Example 1 and Examples 18-19.

[0045] Fig.11 This is a performance comparison chart of the catalysts prepared in Example 1 and Example 20.

[0046] Fig.12 This is a performance comparison chart of the catalysts prepared in Example 1 and Examples 21-22.

[0047] Fig.13 This is a graph showing the catalyst performance test results in Example 23 and Comparative Example 2. DETAILED DESCRIPTION

[0048] The present invention will be further described below in conjunction with the accompanying drawings and specific examples. It should be understood that these examples are only intended to illustrate the present invention and are not intended to limit the scope of the present invention. The operating methods for the unrecorded specific conditions in the following examples are usually carried out under normal conditions or under the conditions recommended by the manufacturer. Unless otherwise specified, the roasting atmosphere refers to air atmosphere.

[0049] Combination Figure 1The present invention discloses a method for preparing a neodymium-doped cobalt-based catalyst that can directly catalyze and decompose nitrous oxide and resist the interference of water vapor and impurity gases, comprising: using cobalt nitrate and neodymium nitrate as precursors, using citric acid and urea as chelating agents, preparing a mixed solution containing cobalt nitrate, neodymium nitrate, urea and citric acid, heating and evaporating in a water bath with stirring at 70-90°C to form a sol-gel state, then drying and calcining at 400-600°C for 3-7 hours to obtain a powdered neodymium-doped cobalt-based catalyst, pressing and sieving to obtain a catalyst with a desired mesh size. Example 1

[0050] A catalyst S(1)-Nd for catalytic decomposition of nitrous oxide with water resistance and resistance to interference from impurity gases 0.08 Co: Weigh 14.55g Co(NO3)2·6H2O and 1.75g ​​Nd(NO3)3·6H2O, mix them evenly, and then weigh 12.01g urea and 38.42g citric acid. Then add 90mL pure water to form a solution. After continuous stirring for 3 hours, place the solution in a water bath for water bath heating. The water bath temperature is set to 80℃, and the solution is heated and evaporated to a gel state. Then the gel catalyst is placed in a blast heater for drying. The drying temperature is 110℃ and the drying time is 12 hours. The dried catalyst is placed in a muffle furnace for calcination. The calcination temperature is 500℃, the calcination time is 5 hours, and the heating rate is 5℃ / min. After calcination, the catalyst is ground, pressed and sieved, and the catalyst particles with a particle size of 40~60 mesh after sieving are sampled.

[0051] Catalytic decomposition of N2O performance test: The residual N2O after the catalytic decomposition of the catalyst was detected and quantitatively analyzed by gas chromatography equipped with a thermal conductivity detector (TCD detector). The test carrier gas was hydrogen; the injection port temperature was 130°C, the column box temperature was 60°C; the TCD detector temperature was 120°C, and the current was 100 mA. The catalyst with a particle size of 40-60 mesh was loaded in a fixed bed quartz tube with a loading amount of 0.3 mL. The conversion efficiency test required pretreatment. The quartz tube was heated to 500°C and maintained for 0.5 h, and 50 mL / min of argon was introduced into the quartz tube. During the test, the total gas flow rate of the raw gas was 100 mL / min, of which the N2O volume concentration was 2000 ppm, and the remaining gas was argon.

[0052] Under the above reaction test conditions, if Figure 2 As shown, the activity of the catalyst in Example 1 is the temperature (T 90 ) = 336℃, and the complete decomposition temperature is 350℃. Example 2

[0053] A catalyst S(2)-Nd for catalytic decomposition of nitrous oxide with water resistance and resistance to interference from impurity gases 0.02 Co, refer to Example 1, change the amount of Nd(NO3)3·6H2O, make the molar ratio of Nd to Co be 0.02:1, and the rest is the same as Example 1. Under the test conditions of Example 1, Figure 2 As shown, the activity of the catalyst in Example 2 is T 90 =360℃, and the complete decomposition temperature is 375℃. Example 3

[0054] A catalyst S(3)-Nd for catalytic decomposition of nitrous oxide with water resistance and resistance to interference from impurity gases 0.04 Co, refer to Example 1, change the amount of Nd(NO3)3·6H2O, make the molar ratio of Nd to Co be 0.04:1, and the rest is the same as Example 1. Under the test conditions of Example 1, Figure 2 As shown, the activity of the catalyst in Example 3 is T 90 =357℃, and the complete decomposition temperature is 375℃. Example 4

[0055] A catalyst S(4)-Nd for catalytic decomposition of nitrous oxide with water resistance and resistance to interference from impurity gases 0.06 Co, refer to Example 1, change the amount of Nd(NO3)3·6H2O, make the molar ratio of Nd to Co be 0.06:1, and the rest is the same as Example 1. Under the test conditions of Example 1, Figure 2 As shown, the activity of the catalyst in Example 4 is T 90 =365℃, and the complete decomposition temperature is 375℃. Example 5

[0056] A catalyst S(5)-Nd for catalytic decomposition of nitrous oxide with water resistance and resistance to interference from impurity gases 0.1 Co, refer to Example 1, change the amount of Nd(NO3)3·6H2O, make the molar ratio of Nd to Co be 0.1:1, and the rest is the same as Example 1. Under the test conditions of Example 1, Figure 2 As shown, the activity of the catalyst in Example 5 is T 90 =342℃, and the complete decomposition temperature is 350℃. Example 6

[0057] A catalyst S(6)-Nd for catalytic decomposition of nitrous oxide with water resistance and resistance to interference from impurity gases 0.12Co, refer to Example 1, change the amount of Nd(NO3)3·6H2O, make the molar ratio of Nd to Co be 0.12:1, and the rest is the same as Example 1. Under the test conditions of Example 1, Figure 2 As shown, the activity of the catalyst in Example 6 is T 90 =351℃, and the complete decomposition temperature is 375℃. Example 7

[0058] A catalyst S(7)-Nd for catalytic decomposition of nitrous oxide with water resistance and resistance to interference from impurity gases 0.14 Co, refer to Example 1, change the amount of Nd(NO3)3·6H2O, make the molar ratio of Nd to Co be 0.14:1, and the rest is the same as Example 1. Under the test conditions of Example 1, Figure 2 As shown, the activity of the catalyst in Example 7 is T 90 =342℃, and the complete decomposition temperature is 350℃. Example 8

[0059] A catalyst S(8)-Nd for catalytic decomposition of nitrous oxide with water resistance and resistance to interference from impurity gases 0.2 Co, refer to Example 1, change the amount of Nd(NO3)3·6H2O, make the molar ratio of Nd to Co be 0.2:1, and the rest is the same as Example 1. Under the test conditions of Example 1, Figure 2 As shown, the activity of the catalyst in Example 8 is T 90 =372℃, and the complete decomposition temperature is 400℃. Example 9

[0060] A catalyst S(9)-Nd for catalytic decomposition of nitrous oxide with water resistance and resistance to interference from impurity gases 0.5 Co, refer to Example 1, change the amount of Nd(NO3)3·6H2O, make the molar ratio of Nd to Co be 0.5:1, and the rest is the same as Example 1. Under the test conditions of Example 1, Figure 2 As shown, the activity of the catalyst in Example 9 is T 90 =384℃, and the complete decomposition temperature is 400℃. Comparative Example 1

[0061] Catalyst A(1)-Co3O4, referring to Example 1, does not add Nd(NO3)3·6H2O, that is, the molar ratio of Nd to Co is 0:1, and the rest is the same as Example 1. Under the test conditions of Example 1, Figure 2 As shown, the activity of the catalyst in Comparative Example 1 is T 90 =375℃, and the complete decomposition temperature is 400℃.

[0062] from Figure 2 It can be seen that a certain amount of Nd lattice doping can significantly improve the performance of Co3O4 in catalytic decomposition of N2O, among which the doping amount of Nd:Co=0.08:1 molar ratio performs best.

[0063] Figure 3 The XRD test results of the catalysts prepared in Examples 1 to 6 and Comparative Example 1 are shown. Figure 3 It can be seen from Figure A that the diffraction peaks of the pure Co3O4 catalyst in Comparative Example 1 appear at diffraction angles 2θ=31.27°, 36.85°, 44.81°, 59.36° and 65.24°, and the positions of the above diffraction peaks are consistent with the XRD standard card (JCPDS card No. 042-1467). The XRD spectra of the catalysts in Examples 1 to 6 are similar to that of the pure Co3O4 catalyst in Comparative Example 1, and no diffraction peaks representing Nd2O3 are found, which indicates that Nd is doped into the lattice of Co3O4, rather than existing in the form of Nd2O3. In addition, by Figure 3 As can be seen in B, the lattice doping of Nd leads to a weakening of the protrusion of the diffraction peak of Co3O4. It can be seen that the lattice doping of Nd obviously inhibits the growth of Co3O4 crystals in the catalyst, proving that the lattice doping of Nd can refine the catalyst grains and reduce the degree of crystallization of Co3O4.

[0064] We conducted nitrogen adsorption and desorption tests on the catalysts prepared in Examples 1 to 6 and Comparative Example 1. The results are shown in Figure 4 .from Figure 4 It can be seen from A that the isothermal adsorption-desorption curves of the catalysts of Examples 1 to 6 all show the characteristics of the H2-type hysteresis loop of the type IV isotherm, indicating that the catalysts of Examples 1 to 6 have a mesoporous structure and are uniformly distributed. Figure 4 Figure B shows the pore size distribution of the catalysts of Examples 1 to 6. It can be seen that the pore size distribution of the catalysts of Examples 1 to 6 is smaller than the pore size distribution of the pure Co3O4 catalyst of Comparative Example 1, indicating that the lattice doping of Nd leads to a reduction in the size of the Co3O4 crystallites in the catalyst, which is also mutually confirmed by the aforementioned XRD analysis results.

[0065] from Figure 5 and Figure 6 It can be clearly seen from the comparison that the Nd lattice doping significantly reduces the average crystallite size (d) of the catalyst. The average particle size (d) of the pure Co3O4 catalyst in Comparative Example 1 is 18.69 nm. 0.08 The average particle size (d) of the Co catalyst is 8.37 nm, which is consistent with the XRD results above.

[0066] In addition, Nd in Example 1 0.08In the transmission electron microscope test, only the lattice fringes of Co3O4 (JCPDS card No. 042-1467) were observed for the Co catalyst and the pure Co3O4 catalyst of Example 1, indicating that Nd lattice doping did not change the original spinel structure of Co3O4. 0.08 The presence of any Nd2O3 lattice fringes in the Co catalyst further indicates that Nd is lattice doped rather than existing in the form of Nd2O3.

[0067] Table 1 shows the particle sizes and BET (Brunner-Emmet-Teller) specific surface area results of the catalysts prepared in Examples 1 to 6 and Comparative Example 1.

[0068] Table 1

[0069] Example 10 The catalyst of Example 1 was used, and the test conditions were changed. The catalyst was tested for catalytic decomposition of N2O in the presence of water vapor. The test environment and test equipment were the same as those of Example 1. The concentration or content of the catalyst raw gas was as follows: N2O volume concentration 2000 ppm; H2O (vapor state) 2 vol%; the remaining gas was argon, and the total gas flow rate was 100 mL / min. For the catalyst activity, see Figure 7 . Embodiment 11

[0070] The only difference from Example 10 is that the H2O (vapor state) content in the catalyst feed gas is 4 vol%. The rest is the same. For the catalyst activity, see Figure 7 . Example 12

[0071] The only difference from Example 10 is that the H2O (vapor state) content in the catalyst feed gas is 5 vol%. The rest is the same. For the catalyst activity, see Figure 7 . Example 13

[0072] The only difference from Example 10 is that the H2O (vapor state) content in the catalyst feed gas is 7 vol%. The rest is the same. For the catalyst activity, see Figure 7 .

[0073] from Figure 7 It can be seen that water vapor has a negative effect on the catalytic decomposition of N2O. When 4 vol%, 5 vol% and 7 vol% water vapor exist in the gas path, the catalytic efficiency of the catalyst is consistent. It can be seen that Nd lattice doping can significantly improve the water resistance of the catalyst. When the water vapor content increases, the activity of the catalyst decreases slightly. Embodiment 14

[0074] The only difference from Example 1 is that the heating rate is changed to 1°C / min, and the rest are the same. The obtained catalyst is tested according to the conditions of Example 1, and the results are shown in Figure 8 . Embodiment 15

[0075] The only difference from Example 1 is that the heating rate is changed to 10°C / min, and the rest are the same. The obtained catalyst is tested according to the conditions of Example 1, and the results are shown in Figure 8 . Example 16

[0076] The only difference from Example 1 is that the calcination time is changed to 3 h, and the rest are the same. The obtained catalyst is tested according to the conditions of Example 1, and the results are shown in Fig. 9 . Embodiment 17

[0077] The only difference from Example 1 is that the calcination time is changed to 7 h, and the rest are the same. The obtained catalyst is tested according to the conditions of Example 1, and the results are shown in Fig. 9 . Embodiment 18

[0078] The only difference from Example 1 is that the calcination temperature is changed to 400°C, and the rest is the same. The obtained catalyst is tested according to the conditions of Example 1, and the results are shown in Fig.10 . Embodiment 19

[0079] The only difference from Example 1 is that the calcination temperature is changed to 600°C, and the rest are the same. The obtained catalyst is tested according to the conditions of Example 1, and the results are shown in Fig.10 . Embodiment 20

[0080] The only difference from Example 1 is that the calcination atmosphere is changed to nitrogen, and the rest is the same. The obtained catalyst is tested according to the conditions of Example 1, and the results are shown in Fig.11 . Embodiment 21

[0081] The only difference from Example 1 is that the amount of citric acid is changed so that the molar ratio of Co(NO3)2·6H2O to citric acid is 1:2. The rest is the same. The obtained catalyst is tested according to the conditions of Example 1. The results are shown in Fig.12 . Embodiment 22

[0082] The only difference from Example 1 is that the amount of citric acid is changed so that the molar ratio of Co(NO3)2·6H2O to citric acid is 1:6. The rest is the same. The obtained catalyst is tested according to the conditions of Example 1. The results are shown in Fig.12 . Embodiment 23

[0083] The catalyst of Example 1 was used, and the test conditions were changed. The performance and stability of the catalyst in catalytic decomposition of N2O in the presence of impurity gas were tested. The test environment and test equipment were the same as those of Example 1. The concentration or content of the catalyst raw gas was as follows: N2O volume concentration of 2000 ppm; NO volume concentration of 100 ppm; 5 vol% H2O (vapor state); 5 vol% O2; the remaining gas was argon, and the total gas flow rate was 100 mL / min. The test temperature was 350°C. The test results are shown in Fig.13 . Comparative Example 2

[0084] Using the catalyst of Comparative Example 1, refer to the test conditions of Example 23, and the test results are shown in Fig.13 .

[0085] Fig.13 It is shown that Nd lattice doping can significantly improve the anti-interference ability of the catalyst; at the same time, it can be seen that when the catalyst cuts off the entry of impurity gases, Nd lattice doping can gradually restore its activity, which will be a great advantage in subsequent practical applications.

[0086] In addition, it should be understood that after reading the above description of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. A neodymium-doped cobalt-based catalyst that can directly catalyze the decomposition of nitrous oxide and resist the interference of water vapor and impurity gases, characterized in that: The neodymium-doped cobalt-based catalyst is a cobalt tetroxide catalyst doped with a neodymium lattice having a mesoporous structure, wherein the molar ratio of neodymium to cobalt is 0.02-0.14:

1.

2. The neodymium-doped cobalt-based catalyst according to claim 1, characterized in that: The average particle size of the neodymium-doped cobalt-based catalyst is less than 15 nm, and the specific surface area is greater than 20 m 2 / g.

3. The neodymium-doped cobalt-based catalyst according to claim 1, characterized in that: The molar ratio of neodymium to cobalt in the neodymium-doped cobalt-based catalyst is 0.08-0.1:1; The average particle size of the neodymium-doped cobalt-based catalyst is less than 10 nm, and the specific surface area is greater than 60 m 2 / g.

4. The method for preparing a neodymium-doped cobalt-based catalyst according to any one of claims 1 to 3, characterized in that: include: A mixed solution containing cobalt nitrate, neodymium nitrate, urea and citric acid is prepared, stirred and heated to form a gel, and then dried and calcined to obtain the neodymium-doped cobalt-based catalyst; The molar ratio of cobalt nitrate, neodymium nitrate, urea and citric acid is 1:(0.02-0.14):4-6:(2-6); The heating rate of the calcination is 1-10°C / min; The calcination temperature is 400-600°C. The holding time of the calcination is 3 to 7 hours; The calcination atmosphere is air atmosphere or nitrogen atmosphere.

5. The preparation method according to claim 4, characterized in that: The molar ratio of cobalt nitrate, neodymium nitrate, urea and citric acid is 1:(0.02~0.14):4~6:(2~4).

6. The preparation method according to claim 4, characterized in that: The heating temperature is 70-90°C.

7. The preparation method according to claim 4, characterized in that: The heating rate of the calcination is 1-5°C / min; The calcination temperature is 400-500°C. The holding time of the calcination is 5 to 7 hours; The calcination atmosphere is air atmosphere.

8. Use of the neodymium-doped cobalt-based catalyst according to any one of claims 1 to 3 in catalytic decomposition of nitrous oxide.

9. The use according to claim 8, characterized in that: Before the neodymium-doped cobalt-based catalyst is used to catalytically decompose nitrous oxide, the neodymium-doped cobalt-based catalyst is pretreated in an inert atmosphere at 450-500° C. for 0.2-1.5 hours.

10. The use according to claim 8, characterized in that: The neodymium-doped cobalt-based catalyst is used to treat polluted gas containing nitrous oxide at a treatment temperature of 100-750°C; The polluted gas also contains zero, one or more of oxygen, water vapor and nitric oxide; The polluted gas has an oxygen content of 0-5 vol%, a water vapor content of 0-5 vol%, and a nitrogen monoxide volume content of 0-100 ppm.

Citation Information

Patent Citations

  • Formed catalyst for directly catalyzing N2O to decompose and manufacturing method thereof

    CN103506128A

  • Catalyst for decomposing nitrous oxide, preparation method of catalyst and nitrous oxide decomposition method

    CN113600202A

  • Modified cobalt-based catalyst for efficiently decomposing nitrous oxide at low temperature as well as preparation method and application of modified cobalt-based catalyst

    CN116371413A

  • Rare earth doped cobalt-based catalyst for catalytic decomposition of N2O and preparation method and application thereof

    CN117282434A

  • Nitrous oxide-decomposing catalyst and method for production thereof