Heterostructure BWxCy composite nanomaterial as well as preparation method and application thereof
The heterostructure BWxCy composite nanomaterial composited with BiOCl is improved by improving the carrier separation efficiency of Bi2WO6, solving the problem of low carrier separation efficiency of Bi2WO6 photocatalyst, and achieving efficient organic pollutant degradation effect.
Patent Information
- Application Number
- CN202410971010.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
The carrier separation efficiency of a single Bi2WO6 photocatalyst during the photocatalysis process is low, resulting in low pollutant degradation efficiency.
By compounding with BiOCl, a heterostructured BWxCy composite nanomaterial was synthesized by a one-step hydrothermal method to improve the Bi2WO6 carrier separation efficiency.
The charge separation efficiency and photocatalytic performance of the photocatalyst are significantly improved, and it can degrade 92.5% of the organic dye RhB and 80.4% of the antibiotic TC in 120 minutes, and has a wide light absorption range, low charge transfer resistance and high stability.
Smart Images

Figure CN118904366A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of photocatalysis technology and particularly provides a BW with a heterogeneous structure. x C y Composite nanomaterials and their preparation methods and applications. Background Art
[0002] With the acceleration of industrialization, the accumulation of organic pollutants in natural water bodies has posed a great threat to the global environment and human health. Traditional organic pollutant degradation technologies, such as physical adsorption, chemical oxidation and biodegradation, are usually not ideal due to their low efficiency and high energy consumption. Semiconductor-based photocatalytic technology is green and environmentally friendly, and has attracted people's attention in recent years. It directly uses solar energy to decompose pollution in the environment and has great development potential. Bi2WO6 is a simple n-type semiconductor material with a special chemical structure and excellent visible light response performance, which has attracted a lot of research attention. Single Bi2WO6 responds very well to visible light, but the photocatalyst has a high recombination rate of photogenerated electron-hole pairs, which shortens the residence time of active species and has a low photocarrier separation, which greatly limits its photocatalytic degradation of pollutants.
[0003] Therefore, how to improve the carrier separation efficiency of Bi2WO6 is an urgent problem to be solved. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a BW x C y Composite nanomaterials, preparation methods and applications thereof are used to couple Bi2WO6 with other bismuth-based photocatalysts to improve the carrier separation efficiency of Bi2WO6.
[0005] The present invention provides a heterogeneous structure BW x C y The preparation method of the composite nano material comprises: using Bi(NO3)3·5H2O as a bismuth source and Na2WO4·2H2O as a tungsten source, and synthesizing a Bi2WO6 / BiOCl composite material by a one-step hydrothermal method.
[0006] Preferably, step 1: using 30 mL of deionized water as a solvent, weighing 2 mmol of Bi(NO3)3·5H2O and dissolving it therein, stirring evenly to obtain a Bi(NO3)3·5H2O solution;
[0007] Step 2: Add x mmol Na2WO4·2H2O to the Bi(NO3)3·5H2O solution in sequence, and continue to stir the mixture to obtain an ivory white suspension; at the same time, dissolve y mmol NaCl in the ivory white suspension, and stir until the white suspension turns light yellow after being mixed evenly;
[0008] Step 3: The light yellow suspension obtained after uniform mixing was transferred to a sealed autoclave lined with polytetrafluoroethylene, and a hydrothermal reaction was carried out at 160° C. for 12 h;
[0009] Step 4: After the reactor is cooled to room temperature, it is washed three times with deionized water and ethanol respectively, and then centrifuged and dried to obtain the Bi2WO6 / BiOCl composite material, which is recorded as BW x C y composites, x and y represent the molar amounts of Na2WO4·2H2O and NaCl used in the reaction system, respectively.
[0010] The BW x C y Composite material is BW 0.5 C 0.5 .
[0011] The present invention also provides a heterogeneous structure BW prepared according to the above preparation method. x C y Composite nanomaterials.
[0012] Finally, the present invention provides the BW of the above heterostructure x C y Application of composite nanomaterials, wherein the composite materials are used to degrade organic pollutants in the atmosphere or water.
[0013] The present invention provides a heterogeneous structure BW x C y Composite nanomaterials, preparation methods and applications thereof, by coupling Bi2WO6 with other bismuth-based photocatalysts to improve the carrier separation efficiency of Bi2WO6. Bi2WO6 has a similar crystal structure to BiOCl, which is composed of [WO4] 2- or Cl - [Bi2O2] between ions 2+ The present invention uses Bi(NO3)3·5H2O as bismuth source and Na2WO4·2H2O as tungsten source to synthesize BW by one-step hydrothermal method. x C y The synthesized samples were subjected to a series of characterizations, confirming the formation of heterojunctions. The BW performance of the organic dye RhB and antibiotic TC was evaluated under 250W high-pressure mercury lamp irradiation. x C yPhotocatalytic performance of the composite material. The results show that the composite material exhibits significant photocatalytic performance in the process of degrading RhB compared with Bi2WO6 and BiOCl. The photocatalytic material was used to degrade the pollutants rhodamine B (RhB) and tetracycline (TC). The results showed that the photocatalytic material could degrade about 92.5% of RhB and 80.4% of TC within 120 minutes, and had a wide light absorption range, high charge separation efficiency, low charge transfer resistance, large specific surface area, and high stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments:
[0015] Figure 1 Pure Bi2WO6, pure BiOCl and BW x C y XRD pattern of heterojunction;
[0016] Figure 2 For BW 0.5 C 0.5 SEM images of the composite materials;
[0017] Figure 3 For Bi2WO6 and BW x C y N2 adsorption-desorption isotherms of the composites;
[0018] Figure 4 For Bi2WO6, BiOCl and BW x C y PL spectra of the composite materials;
[0019] Figure 5 For Bi2WO6, BiOCl and BW x C y Degradation curves of composite materials (a: RhB b: TC);
[0020] Figure 6 For Bi2WO6, BiOCl and BW x C y Kinetic fitting curves of composite materials (a: RhB b: TC);
[0021] Figure 7 For BW 0.5 C 0.5 Cyclic test diagram of composite material for Rhodamine B;
[0022] Figure 8 For BW 0.5 C 0.5 Diagram of the possible photocatalytic mechanism of degradation of Rhodamine B dye by the composite material. DETAILED DESCRIPTION
[0023] The present invention will be further explained below in conjunction with specific implementation schemes, but the present invention is not limited thereto.
[0024] This embodiment provides a heterostructure BW x C y The preparation method of the composite nanomaterial is as follows: 30 mL of deionized water is used as a solvent, 2 mmol of Bi(NO3)3·5H2O is weighed and dissolved therein, and stirred for 30 minutes. Then x mmol Na2WO4·2H2O is added to the Bi(NO3)3·5H2O solution in sequence, and the mixture is stirred continuously to obtain an ivory white suspension. At the same time, y mmol NaCl is dissolved in the above mixed solution and stirred for 3 hours until the mixed white suspension turns light yellow. The suspension obtained after mixing evenly is transferred to a 50 mL polytetrafluoroethylene-lined autoclave, sealed, and placed in an oven at 160°C for a hydrothermal reaction for 12 hours. After the reactor is cooled to room temperature, it is washed three times with deionized water and ethanol respectively, collected by centrifugation, and dried at 60°C for 12 hours to obtain a Bi2WO6 / BiOCl composite material. A series of materials prepared by the above method are marked as BW x C y (BW 0.8 C 0.2 , BW 0.5 C 0.5 and BW 0.2 C 0.8 ). x and y represent the molar amounts of Na2WO4·2H2O and NaCl used in the reaction system, respectively.
[0025] Example 1
[0026] 1. BW 0.5 C 0.5 A method for preparing a composite material, comprising:
[0027] 1) Take 30 mL of deionized water as solvent, weigh 2 mmol Bi(NO3)3·5H2O and dissolve it in it, stir for 30 min to fully dissolve it; the concentration is 6.67×10 -8 mol / L Bi(NO3)3 solution;
[0028] 2) 0.5 mmol Na2WO4·2H2O was added to the solution obtained in step 1) to obtain an ivory white suspension, and 0.5 mmol NaCl was added at the same time, and the mixture was stirred for 3 h to mix the solution thoroughly until the solution turned light yellow.
[0029] 3) The suspension obtained in step 2) is subjected to a hydrothermal reaction. First, the suspension is transferred to a 50 mL polytetrafluoroethylene-lined autoclave and sealed, and then transferred to a 160° C. oven for 12 h.
[0030] 4) After the hydrothermal reaction was completed, the reactor was taken out and cooled to room temperature, washed three times with deionized water and ethanol respectively, and then collected by centrifugation (i.e., deionized water-ethanol-deionized water). The collected final sample was placed in an oven at 60°C and dried for 12 hours to obtain BW 0.5 C 0.5 Composite materials.
[0031] BW 0.8 C 0.2 and BW 0.2 C 0.8 The preparation method is the same as above. In addition, for the convenience of comparison, pure Bi2WO6 and BiOCl were also prepared under the same experimental conditions without Na2WO4·2H2O and NaCl.
[0032] 2. BW x C y The composite materials were characterized as follows:
[0033] like Figure 1 Shown are simple compounds Bi2WO6, BiOCl and different [WO4] 2- With Cl - Molar ratio BW x C y XRD pattern of the composite material. BW x C y The diffraction peaks of the composite material are sharp and strong, indicating that the catalyst has good crystallinity; no other new phases and impurities are found in the figure, confirming the BW x C y Bi2WO6 and BiOCl phases coexist in the heterojunction.
[0034] like Figure 2 BW shown 0.5 C 0.5 SEM image of the composite material. It can be seen that the Bi2WO6 microspheres have abundant pores, which can not only promote the physical adsorption of organic dyes, but also provide space for the deposition of BiOCl, which is embedded in the pores of the Bi2WO6 microspheres to produce a hydrangea-like microstructure; in addition, BiOCl nanosheets are also deposited on the surface of the microspheres, which also proves that the product prepared by the method of the present invention is a nanoscale photocatalytic material.
[0035] like Figure 3 For Bi2WO6, BiOCl and BW x C yN2 adsorption-desorption isotherm of the composite material. BW was measured using ST-2000 adsorption analyzer. 0.5 C 0.5 The effective specific surface area is the largest, which can effectively improve the adsorption capacity of the photocatalyst and thus improve the photocatalytic activity.
[0036] To quantify BW x C y The transfer efficiency of photogenerated charge carriers was analyzed by photoluminescence (PL) spectroscopy. Figure 4 It shows that pure Bi2WO6, BiOCl, BW 0.8 C 0.2 , BW 0.5 C 0.5 and BW 0.2 C 0.8 PL spectra of the samples. In terms of emission intensity, it is found that after combining with BiOCl, BW x C y The emission intensity of Bi2WO6 is reduced, which means that by forming a heterojunction between Bi2WO6 and BiOCl, BiOCl can act as an acceptor for the electrons transferred by Bi2WO6, effectively suppressing the recombination rate of electron-hole pairs. In summary, the results obtained from the PL spectra and N2 adsorption-desorption isotherms confirm that compared with pure BiOCl, Bi2WO6 and other samples, BW 0.5 C 0.5 The charge carrier recombination rate of photocatalysts is slow, so their photocatalytic efficiency is also high.
[0037] 3. BW x C y Composite material properties
[0038] Using a 250W high-pressure mercury lamp as the light source, the change in the absorption peak intensity at a wavelength of 554nm was used to determine the photodegradation of organic pollutants RhB and antibiotics TC. x C y The performance of the samples was analyzed. First, the concentration curves of dye RhB and antibiotic TC with irradiation time were as follows: Figure 5 As shown in the figure, without the participation of photocatalyst, after the light source irradiated RhB and TC solutions for 120 minutes, it was found that their degradation was particularly slow and the photolysis process was almost undetectable. x C y The adsorption capacity and photocatalytic performance of the samples are higher than those of pure Bi2WO6 and BiOCl. Among them, BW shows the highest photocatalytic activity. 0.5 C 0.5 After 120 min, the degradation rate of RhB was 92.5%, while that of pure Bi2WO6 and BW 0.8 C 0.2, BW 0.2 C 0.8 The degradation rates of RhB in pure Bi2WO6, BW 0.8 C 0.2 , BW 0.5 C 0.5 , BW 0.2 C 0.8 The TC degradation rates of the BiOCl and BiOCl composites under light irradiation were 43.56%, 50.49%, 80.48%, 69.5% and 54.3%, respectively.
[0039] Figure 6 The photocatalytic performance of RhB and TC was well fitted with the pseudo-first-order reaction kinetic model. The slope can be obtained from the relationship between ln(C0 / C) and t, which is the rate constant. 0.8 C 0.2 , BW 0.5 C 0.5 , BW 0.2 C 0.8 The rate constants of α-BiOCl and α-BiOCl are 0.00657, 0.00914, 0.02100, 0.01152 and 0.01233 min, respectively. -1 Obviously, the largest rate constant is BW 0.5 C 0.5 , which are 3.17 times and 1.70 times of Bi2WO6 and BiOCl respectively.
[0040] like Figure 7 BW shown 0.5 C 0.5 Repeatability in actual use. The photodegradation of RhB was tested for four cycles. After the first cycle, the samples were collected, centrifuged, washed and dried, and then used for the next cycle, and so on. There was no obvious inactivation of RhB after four runs, and the degradation rates of RhB were 92.5%, 91.2%, 90.4% and 87.5% respectively. This shows that BW 0.5 C 0.5 Photocatalysts have good stability in decomposing organic pollutants.
[0041] 4. The present invention also proposed BW through capture experiments 0.5 C 0.5 A possible photocatalytic mechanism of the composite material is as follows Figure 8 As shown, under the irradiation of 250W ultraviolet high-pressure mercury lamp, BiOCl and Bi2WO6 discharge simultaneously, VB M The electrons in the CB M VBM The same number of holes h remains in + Due to the CB of BiOCl M Potential (0.22eV) is lower than that of Bi2WO6 M The potential (0.44 eV) is smaller, so the photoinduced electrons on the BiOCl interface can migrate to the CB of Bi2WO6 through the heterojunction interface in the composite system. M Similarly, the photogenerated holes on the Bi2WO6 surface can also migrate to the VB of BiOCl. M The electrons in Bi2WO6 can be captured by the adsorbed oxygen to generate hydroxyl radicals, while the photogenerated holes are concentrated on the BiOCl surface, thus achieving the effective separation of photoinduced electrons and holes on the heterojunction. In addition, the existence of the internal electric field can further promote the effective transfer of photogenerated carriers and improve the photocatalytic activity. BW x C y The possible mechanism of photodegradation of RhB dye in the system is as follows:
[0042] BW 0.5 C 0.5 hν→Bi2WO6(e - ,h + ) / BiOCl(e - ,h + )
[0043] Bi2WO6(e - ,h + ) / BiOCl(e - ,h + )→Bi2WO6 e - +BiOCl h +
[0044] Bi2WO6e - +O2→Bi2WO6+·O2 -
[0045] O2 - +RhB→products
[0046] BiOCl(h + )+RhB→products
[0047] O2 - +H2O→H2O2+O2+2OH -
[0048] H2O2+e - → OH+OH -
[0049] OH+RhB→products
[0050] BW 0.5 C 0.5 The active species superoxide anion radicals and photogenerated holes in the photocatalytic reaction play a major role in the degradation of RhB molecules.
[0051] The embodiments of the present invention are described in detail above with reference to the accompanying drawings, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A heterostructured BW x C y The method for preparing a composite nanomaterial is characterized in that: include: Bi2WO6 / BiOCl composites were synthesized by a one-step hydrothermal method using Bi(NO3)3·5H2O as bismuth source and Na2WO4·2H2O as tungsten source.
2. The BW of a heterostructure according to claim 1 x C y The method for preparing a composite nanomaterial is characterized in that: include: Step 1: Take 30 mL of deionized water as solvent, weigh 2 mmol Bi(NO3)3·5H2O and dissolve it in it, and stir it evenly to obtain a Bi(NO3)3·5H2O solution; Step 2: Add x mmol Na2WO4·2H2O to the Bi(NO3)3·5H2O solution in sequence, and continue to stir the mixture to obtain an ivory white suspension; at the same time, dissolve y mmol NaCl in the ivory white suspension, and stir until the white suspension turns light yellow after being mixed evenly; Step 3: The light yellow suspension obtained after uniform mixing was transferred to a sealed autoclave lined with polytetrafluoroethylene, and a hydrothermal reaction was carried out at 160° C. for 12 h; Step 4: After the reactor is cooled to room temperature, it is washed three times with deionized water and ethanol respectively, and then centrifuged and dried to obtain the Bi2WO6 / BiOCl composite material, which is recorded as BW x C y composites, x and y represent the molar amounts of Na2WO4·2H2O and NaCl used in the reaction system, respectively.
3. The BW of a heterostructure according to claim 1 x C y The method for preparing a composite nanomaterial is characterized in that: The BW x C y Composite material is BW 0.5 C 0.5 .
4. The heterostructure BW prepared by any one of the preparation methods described in claim 1-3 x C y Composite nanomaterials.
5. The heterostructure BW prepared by any one of the preparation methods described in claims 1 to 3 x C y The application of composite nanomaterials is characterized by: The composite material is used for degrading organic pollutants in the atmosphere or water.
Citation Information
Patent Citations
Method for one-step hydrothermal synthesis of different-morphology bismuth tungstate two-dimensional photocatalytic materials
CN107376899A
Preparation method of BiOCl-Bi2WO6 functional cotton fabric
CN113774652A
Bismuth oxychloride / bismuth tungstate nano-catalyst as well as preparation method and application thereof
CN114345380A
Compound bismuth type bismuth oxychloride / bismuth tungstate heterojunction photocatalytic material, preparation method thereof and application of photocatalytic material in removal of tetracycline in water body
CN117181248A