Aromatic hydrocarbon ammoxidation catalyst and preparation method and application thereof

CN118904371AActive Publication Date: 2024-11-08WANHUA CHEM GRP CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410932534.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-08
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

[0005]CN102527419A公开了一种用于间二甲苯氨氧化制备间苯二甲腈的V-Sb系催化剂,该催化剂在反应温度425℃,反应压力0.01MPa条件下,在流化床中考评时二甲苯的转化率达99.2%,间苯二甲腈收率达80.8%,但其反应温度偏高,氨比和氧比偏高,也未反馈催化剂长周期稳定性能

Benefits of technology

[0043] (1) By hydrothermally treating a part of the carrier silica sol under the synergistic effect of Additive B and Additive C, the resulting catalyst has excellent activity, and the catalyst maintains stable performance during long-term use;

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004940172130000061
    Figure BDA0004940172130000061
  • Figure HDA0004940172140000011
    Figure HDA0004940172140000011
  • Figure HDA0004940172140000012
    Figure HDA0004940172140000012
Patent Text Reader

Abstract

The invention provides an aromatic hydrocarbon ammoxidation catalyst as well as a preparation method and application thereof. The method comprises the following steps: mixing vanadium, chromium and an auxiliary A component, adding organic acid, stirring to obtain a solution, and adding carrier silica sol to form slurry 1; dissolving an auxiliary agent B and an auxiliary agent C in water, stirring to obtain a solution, adding the carrier silica sol, and carrying out hydrothermal treatment to form slurry 2; mixing the slurry 1 and the slurry 2, heating and evaporating to form concentrated slurry; and carrying out spray drying and high-temperature roasting to prepare the target catalyst. The method solves the problems of low catalyst strength, low reaction activity and poor product yield when the catalyst produced in the prior art is used for ammoxidation reaction, and can be used for industrial production of the isophthalonitrile catalyst prepared by ammoxidation of m-xylene.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalysts, and in particular to an aromatic hydrocarbon ammoxidation catalyst and a preparation method and application thereof. Background Art

[0002] Aromatic nitrile is an important intermediate, mainly used in the synthesis of various dyes and fragrances. Due to its unique chemical structure and reaction properties, aromatic nitrile is also widely used in organic synthesis, polymer materials, and medicine. Typical products of aromatic nitrile include isophthalonitrile, and its tetrachloroisophthalonitrile (chlorothalonil) synthesized by chlorination is a highly effective, low-toxic antifungal fungicide; meta-phenylenediamine (MXDA) obtained by hydrogenation is an epoxy resin curing agent with superior performance, and is also a raw material for polyurethane and nylon resins.

[0003] The simplest and most economical method for producing aromatic nitrile is to obtain it by gas phase ammoxidation of aromatic hydrocarbons in the presence of a catalyst. The core technology is the catalyst, of which the most widely used catalyst in industrial applications is the V-Cr fluidized bed catalyst. In recent years, with the expansion of the market for chlorothalonil and MXDA, the production scale of isophthalonitrile in my country has also shown a rapid growth trend, and the research on the corresponding catalyst and its production technology has also received more attention.

[0004] CN106268890A discloses a mixed catalyst V for the oxidation of aromatic hydrocarbons 1.0 Cr a A b B c C d M e O x , wherein A is selected from at least one of P, B, Bi, Sb, and As; B is selected from at least one of Mn, Ni, Co, Ti, Sn, Mo, or rare earth elements; C is selected from at least one of alkali metals or alkaline earth metals; and M is selected from at least one of Zr and W. The wear resistance of the catalyst described in the patent has been optimized, and its minimum wear index is 1.15%, but it still needs to be improved.

[0005] CN102527419A discloses a V-Sb catalyst for preparing isophthalonitrile by ammoxidation of meta-xylene. Under the conditions of reaction temperature of 425°C and reaction pressure of 0.01 MPa, the conversion rate of xylene reaches 99.2% and the yield of isophthalonitrile reaches 80.8% when evaluated in a fluidized bed. However, the reaction temperature is high, the ammonia ratio and oxygen ratio are high, and the long-term stability performance of the catalyst is not fed back.

[0006] CN116237044A discloses a V-Rh catalyst, wherein the molar ratio of the catalyst to m-xylene: ammonia: oxygen is 1:2.1:10.1, the reaction temperature of the ammoxidation reactor is 360°C, the reaction pressure (gauge pressure) is 29 kPa, and the catalyst weight load in the reactor is 0.037 h -1 The m-xylene conversion rate reached 99.9% and the isophthalonitrile selectivity reached 99.8%, but it used the extremely expensive precious metal Rh and the reaction space velocity was low.

[0007] Although many attempts have been made in the literature to improve the strength, activity and stability of aromatic ammoxidation catalysts, it is clear that the existing technologies still need to be greatly improved due to their respective limitations. Summary of the invention

[0008] In view of the problems existing in the above-mentioned prior art, one of the purposes of the present invention is to provide a new preparation method for producing an aromatic nitrile catalyst. The method has the advantages of simple preparation method, good catalyst strength, high activity, good yield and good stability when used in ammoxidation reaction.

[0009] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:

[0010] A method for preparing an aromatic hydrocarbon ammoxidation catalyst, the method comprising the following steps:

[0011] S1: Mix vanadium, chromium and additive A, add organic acid, stir to obtain a solution, add carrier silica sol to form slurry 1;

[0012] S2: dissolving the additive B and additive C components in water, stirring to obtain a solution, adding the carrier silica sol, and subjecting to hydrothermal treatment to form slurry 2;

[0013] S3: mixing slurry 1 and slurry 2, heating and evaporating to form a concentrated slurry;

[0014] S4: The concentrated slurry is spray dried and calcined at high temperature to prepare the target catalyst.

[0015] In one embodiment of the present invention, the acid in S1 is an organic acid, preferably one or more of oxalic acid, tartaric acid, and citric acid. In the process of preparing the catalyst, dissolving the raw materials by various acids is a conventional process in the art.

[0016] In one embodiment of the present invention, the additive A in S1 provides element A, and A is at least one of molybdenum, bismuth, iron, cobalt, nickel, and tungsten.

[0017] In one embodiment of the present invention, the mass ratio of the silica sols S1 and S2 is 20:1 to 1:20, preferably 15:1 to 1:15.

[0018] In one embodiment of the present invention, the hydrothermal treatment temperature in S2 is 100-250°C, preferably 110-200°C.

[0019] In one embodiment of the present invention, the additive B in S2 provides element B, and B is at least one of lithium, sodium, potassium, rubidium, and cesium.

[0020] In one embodiment of the present invention, the additive C in S2 provides the B element, and C is at least two of boron, phosphorus, arsenic, tellurium, and antimony.

[0021] In one embodiment of the present invention, the evaporation concentration temperature of S3 is 60-100°C, preferably 70-95°C.

[0022] In one embodiment of the present invention, heating and evaporation are performed in S3 to form a concentrated slurry with a solid content of 30-60 wt%.

[0023] In one embodiment of the present invention, S4 controls the spray slurry temperature to be 5 to 60° C. lower than the concentrated slurry temperature of S3; preferably, the spray slurry temperature in S4 is 30 to 100° C., preferably 35 to 95° C. It is further preferred that the slurry temperature of S4 is 5 to 20° C. lower than the evaporation concentration temperature of S3.

[0024] In one embodiment of the present invention, the viscosity of the slurry in S4 is 150 to 1000 mPa·s, preferably 150 to 850 mPa·s.

[0025] In one embodiment of the present invention, the spray inlet temperature in S4 is 180-300°C, and the outlet temperature is 90-130°C.

[0026] In one embodiment of the present invention, the calcination temperature in S4 is 500-700° C., and the calcination time is 1-15 hours.

[0027] Another object of the present invention is to provide an aromatic hydrocarbon ammoxidation catalyst.

[0028] An aromatic hydrocarbon ammoxidation catalyst, the catalyst is obtained by the above-mentioned preparation method, and the chemical formula of the catalyst is as follows in terms of atomic ratio:

[0029] V 1.0 Cr a A b B c C d O x / (SiO2) n

[0030] Wherein A is at least one selected from molybdenum, bismuth, iron, cobalt, nickel and tungsten;

[0031] B is at least one selected from lithium, sodium, potassium, rubidium, and cesium;

[0032] C is at least two selected from boron, phosphorus, arsenic, tellurium, and antimony;

[0033] Among them, the value range of a is 0.5~2.0,

[0034] The value range of b is 0.01~0.5.

[0035] The value range of c is 0.001~0.2,

[0036] The value range of d is 0.01~2.0;

[0037] x is the sum of the number of oxygen atoms required to satisfy the valence of other elements;

[0038] The value of n is selected so that the content of carrier silicon dioxide in the catalyst is 25 to 70% by weight.

[0039] In one embodiment of the present invention, the attrition index of the catalyst is <1.5%, preferably <1.1%.

[0040] Another object of the present invention is to provide a use of an aromatic hydrocarbon ammoxidation catalyst.

[0041] A use of an aromatic hydrocarbon ammoxidation catalyst, wherein the catalyst is obtained by the above-mentioned preparation method, or is the above-mentioned catalyst, and the catalyst is used for preparing aromatic nitriles by ammoxidation of aromatic hydrocarbons, preferably for preparing isophthalonitrile by meta-xylene.

[0042] Compared with the prior art, the beneficial effects of the present invention are mainly reflected in:

[0043] (1) By subjecting a portion of the carrier silica sol to hydrothermal treatment under the synergistic effect of the additives B and C, the obtained catalyst has excellent activity, and the catalyst maintains stable performance during long-term use;

[0044] (2) By controlling the viscosity of the spray drying slurry and the calcination process during the catalyst preparation process, a high-performance industrial catalyst can be stably produced. When used in the production of aromatic nitriles by ammoxidation of aromatic hydrocarbons, the catalyst also exhibits excellent mechanical strength, catalytic activity and stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 This is the SEM result of Example 1;

[0046] Figure 2 It is the SEM result of comparative example 2;

[0047] Figure 3 is the XRD result of Example 1;

[0048] Figure 4 This is the XRD result of Comparative Example 1. DETAILED DESCRIPTION

[0049] The method provided by the present invention is described in further detail below, but the present invention is not limited thereby.

[0050] Test Method

[0051] Testing and characterization of various parameters of catalysts:

[0052] 1. Determination method of catalyst wear index (straight tube method):

[0053] The wear index was determined according to the method in the standard “Straight tube method for determination of wear index of catalytic cracking catalyst” Q / TSH3490909 2006.

[0054] 2. Determination of catalyst particle size distribution:

[0055] The particle size was measured using Dandong Bettersize 2000 laser particle size analyzer, and the dispersant was water.

[0056] 3. Method for determining catalyst slurry viscosity

[0057] The Shanghai Changji NDJ-1B rotational viscometer was used for the measurement. No. 3 rotor was selected and the rotation speed was 60 rpm.

[0058] 4. Determination of catalyst specific surface area and pore structure information

[0059] The BET specific surface area, BJH desorption pore volume and pore size of the catalyst were measured by N2 physical adsorption method using Micrometics ASAP 2460 as the testing instrument.

[0060] 5. The catalyst was tested by scanning electron microscopy (SEM) using Hitachi SU3800 scanning electron microscope.

[0061] 6. The X-ray powder diffraction test (XRD) of the catalyst was carried out using Philips' Panalytical X'PertPro rotating target X-ray powder diffractometer.

[0062] 7. Catalyst raw materials

[0063] The metal salt raw materials used in the embodiments or comparative examples of the present invention were purchased from Xilong Chemical Co., Ltd., ammonium heptamolybdate was purchased from Jinduicheng Molybdenum Co., Ltd., and other raw materials were commercially available unless otherwise specified.

[0064] Example

[0065] The calculation formula for the conversion rate of meta-xylene and the selectivity of the target product isophthalonitrile is as follows:

[0066]

[0067] Example 1

[0068] 1) Preparation of catalyst

[0069] 310 g of vanadium pentoxide, 334 g of chromium trioxide, 0.32 g of ammonium heptamolybdate and 0.49 g of ferric nitrate were dispersed in 360 g of water, heated to 70°C, and a solution prepared by dissolving 1950 g of oxalic acid in 1200 g of water was slowly added under stirring, and 1500 g of 40 wt% silica sol was added, and the mixture was stirred for 1 h to obtain slurry 1.

[0070] 0.25 g of sodium nitrate, 116 g of boric acid, and 0.76 g of 85 wt% phosphoric acid were dispersed in 300 g of water, heated to 70° C., 200 g of 40 wt% silica sol was added under stirring, and treated in a hydrothermal autoclave at 150° C. for 12 h to obtain slurry 2.

[0071] Slurry 1 and slurry 2 were mixed and concentrated by evaporation at 95° C. until a concentrated slurry with a solid content of 45 wt % was formed. The concentrated slurry was cooled to 85° C. to obtain a spray-dried slurry with a slurry viscosity of 230 mPa·s.

[0072] The catalyst precursor was obtained by spray drying under the conditions of an inlet temperature of 250°C and an outlet temperature of 110°C. The obtained catalyst precursor was placed in a muffle furnace, heated to 600°C at a heating rate of 2°C / min, kept warm for 4 hours, and finally cooled to room temperature to obtain an ammonia oxidation catalyst. The SEM results of the obtained catalyst are shown in the attached Figure 1 , XRD results are attached Figure 3 .

[0073] The ratio of active components in the above catalyst is V 1.0 Cr 0.98 Mo 0.05 B 0.55 P 0.06 Fe 0.02 Na 0.01 O x , x is the sum of the number of oxygen atoms required to satisfy the valence of other elements, and the catalyst wear index was determined to be 1.05%.

[0074] 2) Ammoxidation of m-xylene

[0075] 300 g of the ammonia oxidation catalyst obtained above was loaded into a fluidized bed reactor for reaction performance evaluation. The molar ratio of the reaction raw materials was m-xylene: ammonia: air was 1:4.7:37, the reaction temperature was 390 ° C, the reaction pressure was 36 kPaG, and the catalyst weight load in the reactor was 0.06 h -1 The conversion rate of m-xylene and the selectivity of m-dibenzonitrile were 98.2% and 81.2% respectively after 20h reaction. The conversion rate of m-xylene and the selectivity of m-dibenzonitrile were 98.9% and 80.9% respectively after 1000h continuous reaction.

[0076] Comparative Example 1

[0077] Compared with Example 1, the difference is that part of the silica sol is not selectively mixed with additives B and C before hydrothermal treatment, but all the silica sol is simply mixed with additives A, additives B and additives C without any hydrothermal treatment step.

[0078] 1) Preparation of catalyst

[0079] Disperse 310g of vanadium pentoxide, 334g of chromium trioxide, 0.32g of ammonium heptamolybdate, 0.49g of ferric nitrate, 0.25g of sodium nitrate, 116g of boric acid, and 0.76g of 85% phosphoric acid in 660g of water, heat to 70°C, slowly add a solution obtained by dissolving 1950g of oxalic acid in 1200g of water under stirring, add 1700g of 40wt% silica sol, and stir for 1h to obtain a slurry. Evaporate and concentrate at 95°C until a concentrated slurry with a solid content of 45% is formed. Cool the concentrated slurry to 85°C to obtain a spray-dried slurry with a slurry viscosity of 270mPa·s.

[0080] The catalyst precursor was obtained by spray drying under the conditions of an inlet temperature of 250°C and an outlet temperature of 110°C. The obtained catalyst precursor was placed in a muffle furnace, heated to 600°C at a heating rate of 2°C / min, kept warm for 4 hours, and finally cooled to room temperature to obtain an ammonia oxidation catalyst. The XRD results of the obtained catalyst are shown in the attached Figure 4 .

[0081] The ratio of active components in the above catalyst is V 1.0 Cr 0.98 Mo 0.05 B 0.55 P 0.06 Fe 0.02 Na 0.01 O x , x is the sum of the number of oxygen atoms required to satisfy the valence of other elements, and the catalyst wear index was determined to be 1.06%.

[0082] 2) Ammoxidation of m-xylene

[0083] 300 g of the ammonia oxidation catalyst obtained above was loaded into a fluidized bed reactor for reaction performance evaluation. The molar ratio of the reaction raw materials was m-xylene: ammonia: air was 1:4.7:37, the reaction temperature was 390 ° C, the reaction pressure was 36 kPaG, and the catalyst weight load in the reactor was 0.06 h -1 The conversion rate of m-xylene and the selectivity of m-dibenzonitrile were 98.4% and 77.2% respectively after 20h reaction. The conversion rate of m-xylene and the selectivity of m-dibenzonitrile were 99.1% and 74.6% respectively after 1000h continuous reaction.

[0084] From the comparison between Example 1 and Comparative Example 1, it can be seen that the diffraction peak intensity at 2θ=28° of the catalyst of Comparative Example 1 which has not undergone hydrothermal treatment is significantly higher, while the diffraction peak intensity of the catalyst of Example 1 which has undergone hydrothermal treatment is weaker. The catalyst prepared by the method of the present invention has higher conversion rate, selectivity and long-term stability.

[0085] Example 2

[0086] 1) Preparation of catalyst

[0087] 310 g of vanadium pentoxide, 348 g of chromium trioxide and 1.882 g of ammonium heptamolybdate were dispersed in 360 g of water, heated to 70° C., and a solution prepared by dissolving 1950 g of oxalic acid in 1200 g of water was slowly added under stirring, and 1300 g of 40 wt % silica sol was added, and stirred for 1 h to obtain slurry 1.

[0088] 1.25 g of sodium nitrate, 1.50 g of potassium nitrate, 97 g of boric acid, 5.32 g of antimony acetate, and 290 g of 80% arsenic acid were dispersed in 300 g of water, heated to 70° C., 400 g of 40% silica sol was added under stirring, and treated in a hydrothermal autoclave at 120° C. for 24 h to obtain slurry 2.

[0089] Slurry 1 and slurry 2 were mixed and concentrated by evaporation at 86° C. until a concentrated slurry with a solid content of 45% was formed. The concentrated slurry was cooled to 35° C. to obtain a spray-dried slurry with a slurry viscosity of 450 mPa·s.

[0090] The catalyst precursor was obtained by spray drying under the conditions of an inlet temperature of 270°C and an outlet temperature of 105°C. The obtained catalyst precursor was placed in a muffle furnace, heated to 600°C at a heating rate of 2°C / min, kept warm for 4 hours, and finally cooled to room temperature to obtain an ammonia oxidation catalyst.

[0091] The ratio of active components in the above catalyst is V 1.0 Cr 1.02 Mo 0.21 B 0.46 Sb 0.06As 0.48 Na 0.05 K 0.05 O x , x is the sum of the number of oxygen atoms required to satisfy the valence of other elements, and the catalyst wear index was determined to be 0.95%.

[0092] 2) Ammoxidation of m-xylene

[0093] 300 g of the ammonia oxidation catalyst obtained above was loaded into a fluidized bed reactor for reaction performance evaluation. The molar ratio of the reaction raw materials was m-xylene: ammonia: air was 1:4.7:37, the reaction temperature was 390 ° C, the reaction pressure was 36 kPaG, and the catalyst weight load in the reactor was 0.06 h -1 The conversion rate of m-xylene and the selectivity of m-dibenzonitrile were 99.1% and 82.5% respectively after 20h reaction. The conversion rate of m-xylene and the selectivity of m-dibenzonitrile were 99.4% and 82.8% respectively after 1000h continuous reaction.

[0094] Comparative Example 2

[0095] Compared with Example 1, the difference is that after the slurry is concentrated, spray drying is started without cooling treatment, and the slurry viscosity is not within the scope of the present invention.

[0096] 1) Preparation of catalyst

[0097] 310 g of vanadium pentoxide, 334 g of chromium trioxide, 0.32 g of ammonium heptamolybdate and 0.49 g of ferric nitrate were dispersed in 360 g of water, heated to 70°C, and a solution prepared by dissolving 1950 g of oxalic acid in 1200 g of water was slowly added under stirring, and 1500 g of 40 wt% silica sol was added, and the mixture was stirred for 1 h to obtain slurry 1.

[0098] 0.25 g of sodium nitrate, 116 g of boric acid, and 0.76 g of 85 wt% phosphoric acid were dispersed in 300 g of water, heated to 70° C., 200 g of 40 wt% silica sol was added under stirring, and treated in a hydrothermal autoclave at 150° C. for 12 h to obtain slurry 2.

[0099] Slurry 1 and slurry 2 were mixed and concentrated by evaporation at 95° C. until a concentrated slurry with a solid content of 45% and a slurry viscosity of 127 mP·s was formed.

[0100] The concentrated slurry at 95°C was spray dried under the conditions of an inlet temperature of 250°C and an outlet temperature of 110°C to obtain a catalyst precursor; the obtained catalyst precursor was placed in a muffle furnace, heated to 600°C at a heating rate of 2°C / min, kept warm for 4 hours, and finally cooled to room temperature to obtain an ammonia oxidation catalyst. The SEM results of the obtained catalyst are shown in the attached Figure 2 .

[0101] The ratio of active components in the above catalyst is V 1.0 Cr 0.98 Mo 0.05 B 0.55 P 0.06 Fe 0.02 Na 0.01 O x , x is the sum of the number of oxygen atoms required to satisfy the valence of other elements, and the catalyst wear index was determined to be 2.49%.

[0102] 2) Ammoxidation of m-xylene

[0103] 300 g of the ammonia oxidation catalyst obtained above was loaded into a fluidized bed reactor for reaction performance evaluation. The molar ratio of the reaction raw materials was m-xylene: ammonia: air was 1:4.7:37, the reaction temperature was 390 ° C, the reaction pressure was 36 kPaG, and the catalyst weight load in the reactor was 0.06 h -1 The conversion rate of m-xylene and the selectivity of m-dibenzonitrile were 98.3% and 80.6% respectively after 20h reaction. The conversion rate of m-xylene and the selectivity of m-dibenzonitrile were 97.6% and 81.1% respectively after 1000h continuous reaction.

[0104] From the comparison between Example 1 and Comparative Example 2, it can be seen that the temperature of the catalyst spray drying slurry is not lower than that of the concentrated slurry, and the slurry viscosity is slightly lower, which causes a large number of cracks on the catalyst surface, a decrease in strength, and damage during long-term operation, and a decrease in activity. Therefore, the catalyst prepared by the method of the present invention has better comprehensive performance.

[0105] Example 3

[0106] 1) Preparation of catalyst

[0107] 310 g of vanadium pentoxide, 533 g of chromium trioxide and 0.179 g of ammonium heptamolybdate were dispersed in 520 g of water, heated to 70° C., and a solution prepared by dissolving 2662 g of oxalic acid in 1200 g of water was slowly added under stirring, and 850 g of 40 wt % silica sol was added, and stirred for 1 h to obtain slurry 1.

[0108] 0.90 g potassium nitrate, 30 g boric acid and 5.32 g antimony acetate were dispersed in 200 g water, heated to 70° C., 850 g 40% silica sol was added under stirring, and treated in a hydrothermal autoclave at 190° C. for 8 h to obtain slurry 2.

[0109] Slurry 1 and slurry 2 were mixed and concentrated by evaporation at 75° C. until a concentrated slurry with a solid content of 55% was formed. The concentrated slurry was cooled to 60° C. to obtain a spray-dried slurry with a slurry viscosity of 810 mPa·s.

[0110] The catalyst precursor was obtained by spray drying under the conditions of an inlet temperature of 290°C and an outlet temperature of 120°C. The obtained catalyst precursor was placed in a muffle furnace, heated to 650°C at a heating rate of 2°C / min, kept warm for 2h, and calcined, and finally cooled to room temperature to obtain an ammonia oxidation catalyst.

[0111] The ratio of active components in the above catalyst is V 1.0 Cr 1.5 Mo 0.02 B 0.14 Sb 0.06 K 0.03 Ox, x is the sum of the number of oxygen atoms required to satisfy the valence of other elements, and the catalyst wear index was determined to be 0.76%.

[0112] 2) Ammoxidation of m-xylene

[0113] 300 g of the ammonia oxidation catalyst obtained above was loaded into a fluidized bed reactor for reaction performance evaluation. The molar ratio of the reaction raw materials was m-xylene: ammonia: air was 1:4.7:37, the reaction temperature was 390 ° C, the reaction pressure was 36 kPaG, and the catalyst weight load in the reactor was 0.06 h -1 The conversion rate of m-xylene and the selectivity of m-dibenzonitrile were 98.3% and 83.9% respectively after 20h reaction. The conversion rate of m-xylene and the selectivity of m-dibenzonitrile were 98.5% and 83.6% respectively after 1000h continuous reaction.

[0114] Example 4

[0115] 1) Preparation of catalyst

[0116] 310 g of vanadium pentoxide, 334 g of chromium trioxide, 0.32 g of ammonium heptamolybdate and 0.49 g of ferric nitrate were dispersed in 360 g of water, heated to 70°C, and a solution prepared by dissolving 1950 g of tartaric acid in 1200 g of water was slowly added under stirring, and 500 g of 40 wt% silica sol was added, and the mixture was stirred for 1 h to obtain slurry 1.

[0117] 0.25 g of sodium nitrate, 116 g of boric acid, and 0.76 g of 85 wt% phosphoric acid were dispersed in 300 g of water, heated to 70° C., 1200 g of 40 wt% silica sol was added under stirring, and treated in a hydrothermal autoclave at 150° C. for 24 h to obtain slurry 2.

[0118] Slurry 1 and slurry 2 were mixed and concentrated by evaporation at 95° C. until a concentrated slurry with a solid content of 40% was formed. The concentrated slurry was cooled to 85° C. to obtain a spray-dried slurry with a slurry viscosity of 190 mPa·s.

[0119] The catalyst precursor was obtained by spray drying under the conditions of an inlet temperature of 200°C and an outlet temperature of 95°C. The obtained catalyst precursor was placed in a muffle furnace, heated to 550°C at a heating rate of 2°C / min, kept warm for 12 hours, and finally cooled to room temperature to obtain an ammonia oxidation catalyst.

[0120] The ratio of active components in the above catalyst is V 1.0 Cr 1.02 Mo 0.05 B 0.46 Sb 0.06 Fe 0.02 K 0.01 O x , x is the sum of the number of oxygen atoms required to satisfy the valence of other elements, and the catalyst wear index was determined to be 1.11%.

[0121] 2) Ammoxidation of m-xylene

[0122] 300 g of the ammonia oxidation catalyst obtained above was loaded into a fluidized bed reactor for reaction performance evaluation. The molar ratio of the reaction raw materials was m-xylene: ammonia: air was 1:4.7:37, the reaction temperature was 390 ° C, the reaction pressure was 36 kPaG, and the catalyst weight load in the reactor was 0.06 h -1 The conversion rate of m-xylene and the selectivity of m-dibenzonitrile were 97.9% and 84.2% respectively after 20h reaction. The conversion rate of m-xylene and the selectivity of m-dibenzonitrile were 98.1% and 83.9% respectively after 1000h continuous reaction.

[0123] Although the present invention has been described in detail for the purpose of illustration in the foregoing text, it should be understood that these detailed descriptions are only for illustration and can be modified by those skilled in the art without departing from the spirit and scope of the present invention. The present invention is limited only by the claims.

Claims

1. A method for preparing an aromatic hydrocarbon ammoxidation catalyst, It is characterized in that The method comprises the following steps: S1: Mix vanadium, chromium and additive A, add organic acid, stir to obtain a solution, add carrier silica sol to form slurry 1; S2: dissolving the additive B and additive C components in water, stirring to obtain a solution, adding the carrier silica sol, and subjecting to hydrothermal treatment to form slurry 2; S3: mixing slurry 1 and slurry 2, heating and evaporating to form a concentrated slurry; S4: spray drying and high temperature calcination to produce the target catalyst.

2. The preparation method according to claim 1, It is characterized in that The acid in S1 is an organic acid, preferably one or more of oxalic acid, tartaric acid, and citric acid; And / or, the additive A in S1 provides element A, and A is at least one of molybdenum, bismuth, iron, cobalt, nickel, and tungsten.

3. The preparation method according to claim 1 or 2, It is characterized in that The mass ratio of silica sol S1 to S2 is 20:1 to 1:20, preferably 15:1 to 1:15; and / or, the hydrothermal treatment temperature in S2 is 100 to 250° C., preferably 110 to 200° C.; and / or, the auxiliary agent B in S2 provides element B, and B is at least one of lithium, sodium, potassium, rubidium, and cesium; And / or, the additive C in S2 provides element B, and C is at least two of boron, phosphorus, arsenic, tellurium, and antimony.

4. The preparation method according to claim 1, It is characterized in that The evaporation concentration temperature of S3 is 60 to 100°C, preferably 70 to 95°C; And / or, heating and evaporation in S3 to form a concentrated slurry with a solid content of 30-60 wt%.

5. The preparation method according to claim 1, It is characterized in that S4 controls the spray slurry temperature to be 5 to 60° C. lower than the concentrated slurry temperature described in S3; Preferably, the spray slurry temperature in S4 is 30 to 100° C., preferably 35 to 95° C.; and / or, the slurry viscosity in S4 is 150 to 1000 mPa·s, preferably 150 to 850 mPa·s; and / or, the spray inlet temperature in S4 is 180-300°C and the outlet temperature is 90-130°C; And / or, the calcination temperature in S4 is 500-700° C., and the calcination time is 1-15 hours.

6. An aromatic hydrocarbon ammoxidation catalyst, the catalyst being obtained by the preparation method according to any one of claims 1 to 5, It is characterized in that The chemical formula of the catalyst is as follows in terms of atomic ratio: V 1.0 Cr a A b B c C d O x / (SiO 2 ) n Wherein A is at least one selected from molybdenum, bismuth, iron, cobalt, nickel and tungsten; B is at least one selected from lithium, sodium, potassium, rubidium, and cesium; C is at least two selected from boron, phosphorus, arsenic, tellurium, and antimony; Among them, the value range of a is 0.5~2.0, The value range of b is 0.01~0.

5. The value range of c is 0.001~0.2, The value range of d is 0.01~2.0; x is the sum of the number of oxygen atoms required to satisfy the valence of other elements; The value of n is selected so that the content of carrier silicon dioxide in the catalyst is 25 to 70% by weight.

7. The catalyst according to claim 6, It is characterized in that The attrition index of the catalyst is <1.5%, preferably <1.1%.

8. Use of an aromatic hydrocarbon ammoxidation catalyst, wherein the catalyst is obtained by the preparation method described in any one of claims 1 to 5, or is the catalyst described in claim 6 or 7, and the catalyst is used for the ammoxidation of aromatic hydrocarbons to prepare aromatic nitriles, preferably for the preparation of isophthalonitrile from meta-xylene.

Citation Information

Patent Citations

  • Method for preparing m-phthalodinitrile catalyst through ammoxidation

    CN102527419A

  • Aromatic ammoxidation fluidized bed catalyst, preparation method and application

    CN106268890A

  • Ammonia oxidation catalyst as well as preparation method and application thereof

    CN116237044A

  • Mixed-phase catalyst for reaction for preparing acrylonitrile acid through one-step ammoxidation of propane

    CN110833828A

  • Selective ammoxidation catalyst, preparation method and application thereof, and preparation method of methylbenzonitrile