Sulfur-tolerant high-dispersion Pd-coated HZSM5 molecular sieve catalyst as well as preparation method and application thereof

By encapsulating Pd noble metal in situ within the pores of HZSM5 molecular sieve, the problem of noble metal catalysts being easily poisoned by sulfur was solved, resulting in a highly efficient sulfur-resistant catalyst that improves the activity and stability of deep hydrogenation treatment of coal tar.

CN118904386AActive Publication Date: 2024-11-08CHINA UNIV OF MINING & TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410958095.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

Precious metal catalysts are easily poisoned by sulfur-containing compounds, resulting in a significant reduction in activity and stability. Existing supported catalysts have limited sulfur resistance, which increases the energy consumption and production cost of deep hydrogenation of coal tar.

Method used

Highly dispersed Pd@HZSM5 molecular sieve catalysts were prepared by in-situ encapsulation. By uniformly encapsulating Pd noble metal in the pores of HZSM5 molecular sieve, the hydrogen overflow effect of acidic sites on the support surface is utilized to protect the metal from sulfur poisoning and to achieve the hydrogenation reaction of naphthalene.

Benefits of technology

It improves the catalyst's sulfur resistance and hydrogenation activity, enhances product selectivity and yield, and exhibits excellent catalytic performance, especially in sulfur-containing naphthalene hydrogenation systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904386A_ABST
    Figure CN118904386A_ABST
Patent Text Reader

Abstract

The invention discloses a sulfur-tolerant high-dispersion Pd-coated HZSM5 molecular sieve catalyst as well as a preparation method and application thereof. The method comprises the following steps: uniformly mixing a Pd precursor, a silicon source, an aluminum source, a template agent and water, fully stirring, and synthesizing the HZSM5 molecular sieve encapsulated Pd-based catalyst by using an in-situ encapsulation method. Pd metal is fixed in micropores or cages of the molecular sieve, and molecules with the diameter larger than the pore size are difficult to diffuse into the molecular sieve to be in contact with the Pd metal due to the influence of the size effect. The particle size of the active metal ranges from 2.28 nm to 3.75 nm, and the content of the active metal ranges from 0.1 wt% to 0.5 wt%. The Pd-coated HZSM5 molecular sieve catalyst prepared by the invention is applied to a polycyclic aromatic hydrocarbon naphthalene hydrogenation system containing macromolecular organic sulfur, shows excellent catalytic hydrogenation activity and hydrogenation sulfur-resistant effect, and has a good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a palladium-based molecular sieve catalyst, in particular to a sulfur-resistant highly dispersed Pd@HZSM5 molecular sieve catalyst and a preparation method and application thereof, belonging to the technical field of catalyst preparation technology and condensed ring aromatic hydrocarbon catalytic hydrogenation. Background Art

[0002] As the main energy source in my country, coal tar produced by coal gasification, dry distillation and pyrolysis has a huge output. It fully retains the unique macromolecular aromatic ring structure in coal, has high energy density and good thermal oxidation stability. Therefore, using coal tar as the starting material, enriching polycyclic aromatic hydrocarbons and catalytic hydrogenation to synthesize high-density fuels to alleviate the oil crisis has become an inevitable trend in the development of aerospace jet fuel in the future, and has great strategic significance for national defense. Precious metal catalysts are considered to be ideal catalysts for deep hydrogenation of coal tar under mild conditions (<250℃) due to their excellent low-temperature hydrogen dissociation and aromatic activation abilities. However, precious metal catalysts are easily poisoned by sulfur-containing compounds (ppm level), resulting in significantly reduced activity and stability. In industrial production, coal tar usually needs to be deeply desulfurized before it can be hydrogenated, which undoubtedly greatly increases energy consumption and production costs. Therefore, strengthening the sulfur resistance of precious metal catalysts is the key to ensuring both high activity and high stability of catalysts for deep hydrogenation, which is also the primary problem that must be solved in the production of high-density fuels from coal tar.

[0003] At present, precious metal catalysts are mostly used in a supported form, so adjusting the acidity of the support also has a great influence on the sulfur resistance of the catalyst. The interaction between the acid sites and the adjacent noble metals can promote the migration of metal charges to the acid centers, and improve the sulfur resistance of the catalyst by increasing the electronic defects of the noble metal clusters. However, the sulfur resistance of the catalyst synthesized by simple impregnation is limited. It is particularly important to develop an encapsulated catalyst that uses a physical coating method to prevent large molecular sulfur-containing organic matter from directly contacting the noble metal active sites. The present invention is proposed to solve the above problem. Summary of the invention

[0004] One of the purposes of the present invention is to provide a method for preparing a sulfur-resistant highly dispersed Pd@HZSM5 molecular sieve catalyst, which has simple synthesis steps and can achieve uniform and stable encapsulation of highly dispersed Pd precious metal into the pores of the HZSM5 molecular sieve.

[0005] The second object of the present invention is to provide a sulfur-resistant highly dispersed Pd@HZSM5 molecular sieve catalyst prepared by the above preparation method.

[0006] The third object of the present invention is to provide the application of the above-mentioned sulfur-resistant highly dispersed Pd@HZSM5 molecular sieve catalyst, which is used in a sulfur-containing naphthalene hydrogenation system to exhibit excellent catalytic hydrogenation activity and hydrogenation sulfur resistance effect.

[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0008] The first aspect of the present invention provides a method for preparing a sulfur-resistant highly dispersed Pd@HZSM5 molecular sieve catalyst, comprising the following steps:

[0009] (1) Weigh tetraethyl orthosilicate (TEOS) and tetrapropylammonium hydroxide (TPAOH), stir and mix at 80-120°C for 18-24h to form a gel, and then add aluminum nitrate nonahydrate (Al(NO 3 ) 3 9H 2 O) and sodium hydroxide (NaOH) mixed solution, and continued stirring at room temperature for 3-5h to obtain a first mixture;

[0010] (2) adding the ethylenediamine mixed solution containing the palladium precursor to the first mixture obtained in step (1), and continuing stirring for 1-2 hours to obtain a second mixture;

[0011] (3) transferring the second mixture obtained in step (2) to a hydrothermal reactor, crystallizing at 150-200° C. for 36-48 hours, cooling to room temperature, centrifuging, and drying. The dried solid was ground into powder and then calcined in a muffle furnace for 6 hours to obtain a first solid;

[0012] (4) subjecting the first solid obtained in step (3) to three consecutive ion exchanges, and then drying the first solid, grinding the dried solid into powder, and calcining the powder in a muffle furnace for 6 hours to obtain a second solid;

[0013] (5) placing the second solid obtained in step (4) in a tube furnace, heating it to 300-400° C. under an argon atmosphere, then switching to a hydrogen atmosphere, reducing it for 2 h, and then switching back to argon and cooling it to room temperature to obtain a HZSM5 molecular sieve encapsulated palladium catalyst, recorded as Pd@HZSM5 catalyst.

[0014] Preferably, the palladium precursor in step (2) is palladium chloride. Palladium chloride is slightly soluble in water at room temperature, and ethylenediamine is added to fully dissolve it. Ethylenediamine can react with Pd 2+ Chelation to form a stable metal complex precursor (Pd(en) 2 ), which is easily soluble in water. The molar ratio of n(Pd) / n(en) is controlled to be 1 / 10 to ensure the full complexation of the precious metal.

[0015] Preferably, the calcination in step (3) and step (4) is for the purpose of removing impurities and templates, the calcination temperature is 450-650° C., and the heating rate is 1.5° C. / min.

[0016] Preferably, the specific operation of ion exchange in step (4) is to mix the sample powder with 0.8M NH 4 The Cl solution was stirred at 80-100 °C for 1-3 h.

[0017] Preferably, in step (5), the heating rate is 10-15°C / min, and the Ar and H 2 The flow rate is 70-100mL / min.

[0018] Preferably, in step (5), the n(SiO 2 / Al 2 O 3 ) is 50.

[0019] Preferably, the palladium loading in the Pd@HZSM5 catalyst in step (5) is 0.1 wt.%-0.5 wt.%.

[0020] The second aspect of the present invention provides a sulfur-resistant highly dispersed Pd@HZSM5 molecular sieve catalyst prepared by the above preparation method. The Pd metal in the Pd@HZSM5 molecular sieve catalyst is evenly distributed inside the carrier HZSM5 molecular sieve, with an average particle size of 2.28-3.75nm, and remains highly dispersed after high-temperature calcination.

[0021] The third aspect of the present invention provides the application of the above-mentioned sulfur-resistant highly dispersed Pd@HZSM5 molecular sieve catalyst, which is used as a catalyst for the hydrogenation reaction of sulfur-containing naphthalene. Compared with the impregnated catalyst, its reaction activity, product selectivity and product yield can be improved.

[0022] The specific application steps include: placing substrate naphthalene (or containing dibenzothiophene), Pd@HZSM5 catalyst and n-hexane solvent in a reactor, wherein the hydrogenation reaction temperature is 200-260°C and the initial pressure of the hydrogenation reaction is 2.0-2.5MPa.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The present invention selects A highly dispersed Pd@HZSM5 molecular sieve catalyst was prepared by in-situ synthesis using an HZSM5 carrier with acid sites. The catalyst has a typical ZSM5 diffraction peak. It can be seen from the examples and comparative examples that the highest naphthalene conversion rate of the catalyst prepared with the extremely weakly acidic pure silicon S-1 molecular sieve as the carrier is only 3.61%, while the naphthalene conversion rate of the catalyst prepared with the acidic carrier HZSM5 can be increased to more than 60%. The results show that there is a synergistic hydrogen overflow effect between the precious metal Pd nanoparticles and the acidic sites of the carrier, which increases the accessibility of the metal sites to the reactant molecules, and ultimately achieves the improvement of the catalyst activity and the regulation of product selectivity.

[0025] 2. The present invention adopts an in-situ encapsulation method to synthesize an encapsulated precious metal catalyst, and the metal Pd is confined to the internal pores of the HZSM5 molecular sieve. Due to the pore size restriction, the macromolecular organic sulfur molecules cannot directly contact the naphthalene hydrocarbons, so that the encapsulated metal Pd is protected from sulfur poisoning. At the same time, the hydrogen overflow effect of the acidic sites on the surface of the HZSM5 molecular sieve carrier is utilized to transfer the active hydrogen to the carrier surface, thereby realizing the hydrogenation reaction of naphthalene. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 1 is the XRD diagram of the catalysts obtained in Example 1 and Example 2.

[0027] Figure 2 This is a TEM image of the catalyst obtained in Example 1.

[0028] Figure 3 This is a particle size distribution diagram of the Pd metal particles in the catalyst obtained in Example 1.

[0029] Figure 4 This is a TEM image of the catalyst obtained in Example 2.

[0030] Figure 5 This is a particle size distribution diagram of the Pd metal particles in the catalyst obtained in Example 2.

[0031] Figure 6 This is the XPS chart of the catalyst obtained in Example 1.

[0032] Figure 7 This is the XPS chart of the catalyst obtained in Example 2.

[0033] Figure 8 It is the conversion rate of dibenzothiophene in the hydrogenation reaction of naphthalene (including dibenzothiophene) catalyzed by the catalysts obtained in Examples 1 and 2. DETAILED DESCRIPTION

[0034] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0035] Example 1-2 modulates the bonding position of Pd metal and HZSM5 molecular sieve carrier.

[0036] Example 1: Synthesis of 0.5wt.% Pd@HZSM5-50 catalyst by in-situ encapsulation method.

[0037] The 0.5 wt.% Pd@HZSM5-50 catalyst was synthesized by in-situ encapsulation method. 22.2169 g of tetraethyl orthosilicate (TEOS) and 21.6882 g of tetrapropylammonium hydroxide (TPAOH) were weighed and mixed in a beaker, stirred at 80 °C for 24 h to form a transparent gel, and then 1.6002 g of aluminum nitrate nonahydrate (Al(NO 3 ) 3 9H 2 O) and 0.7401g sodium hydroxide (NaOH) mixed solution, continue stirring at room temperature for 4.5h. Then add metal ligand solution, specifically 0.0529g PdCl 2 Dissolve in 6 ml of water with 2 mL of ethylenediamine. Stir for another 1 h after adding the metal ligand solution, then add the mixture to the solution that has been stirred for 4.5 h and continue stirring for 1 h. Then stop stirring, transfer the final mixture into a 100 mL polytetrafluoroethylene hydrothermal autoclave, crystallize in a 170 ° C oven for 48 h, wait to cool to room temperature, wash the mixture with deionized water until neutral, and dry the resulting solid in a 100 ° C oven for 12 h; grind the dried solid into powder and place it in a muffle furnace, heat it to 550 ° C at a heating rate of 1.5 ° C / min, keep it for 6 h, and collect the solid powder after cooling. The powder is mixed with 0.8M NH 4 The Cl solution was stirred for 3 hours for ion exchange, and the exchange was continued three times, and then the solid was dried in an oven at 100°C for 12 hours. The solid was then ground into powder, and then calcined in a muffle furnace for 6 hours, cooled to room temperature, and placed in a tube furnace, heated to 400°C under an argon atmosphere, switched to a hydrogen atmosphere, and reduced for 2 hours under this atmosphere. After reduction, it was switched to argon and cooled to room temperature, and the solid powder was collected to obtain the target catalyst 0.5wt.%Pd@HZSM5-50.

[0038] The XRD pattern of the catalyst prepared in Example 1 is as follows: Figure 1 As shown in the TEM image Figure 2 As shown in the figure, the particle size distribution of Pd metal particles is as follows Figure 3 As shown, XPS Figure 6 As shown. Figure 1 It can be seen that the catalyst of Example 1 prepared by the in-situ encapsulation method exhibits typical ZSM5 molecular sieve crystal diffraction peaks, and has no diffraction peaks of metal Pd or metal oxide PdO, indicating that the metal particles are small and dispersed more evenly. Figure 2It can be seen that the in-situ synthesized HZSM5 molecular sieve has a regular morphology. Figure 3 It can be seen that the average particle size of Pd metal is small, only 2.28nm, indicating that the metal is evenly dispersed on the carrier surface. Figure 6 No obvious Pd metal diffraction peak was observed in the results. Since XPS, a surface technique, is difficult to detect metals encapsulated inside the molecular sieve, this indicates that Pd metal was successfully encapsulated into the HZSM5 molecular sieve.

[0039] Example 2: Synthesis of 0.5wt.% Pd / HZSM5-50 catalyst by impregnation method.

[0040] The HZSM5-50 carrier was synthesized by a method similar to that in Example 1, but without adding any metal palladium-related substances. Then, a 0.5 wt.% Pd / HZSM5-50 catalyst was prepared by a conventional impregnation method, and the specific steps were as follows:

[0041] 0.0105 g of palladium acetate and 20 mL of dichloromethane were added to a beaker to obtain a uniform mixed solution; 0.995 g of calcined HZSM5-50 molecular sieve was weighed and added to the solution, stirred at room temperature for 3 h, and then allowed to stand for 24 h; the beaker was placed in a blast oven and dried at 120 ° C for 12 h; the dried solid was ground into powder and placed in a muffle furnace, heated to 550 ° C at a heating rate of 2.5 ° C / min, and maintained for 4 h to obtain a solid powder; then it was placed in an atmosphere furnace, heated to 400 ° C at a heating rate of 15 ° C / min in an Ar atmosphere, and replaced with H with the same flow rate. 2 The mixture was reduced under an Ar atmosphere for 2 h. Finally, the mixture was replaced with an Ar atmosphere and cooled to room temperature to obtain the target catalyst 0.5 wt. % Pd / HZSM5-50.

[0042] The XRD pattern of the catalyst prepared in Example 2 is as follows: Figure 1 As shown in the TEM image Figure 4 As shown in the figure, the particle size distribution of Pd metal particles is as follows Figure 5 As shown, XPS Figure 7 As shown. Figure 1 It can be seen that the crystal structure of the catalyst molecular sieve of Example 2 prepared by the hydrothermal method combined with the impregnation method is very similar to that of Example 1, and both show obvious ZSM5 crystal diffraction peaks. Figure 5 It can be seen that the average size of the Pd metal particles loaded by the impregnation method is slightly larger than that of Example 1, which is 3.75 nm, and the metal dispersion is slightly poor. Figure 7 It can be seen that, significantly different from Example 1, the intensity of the Pd metal diffraction peak is significantly enhanced. Among them, the Pd 3d energy spectrum presents two sets of double peaks, corresponding to the Pd 3d5 / 2 and Pd 3d3 / 2 orbitals respectively. 2+ The presence of unreduced PdO and Pd0 Oxidation with air causes it to become oxidized.

[0043] Comparative Example 1 changes the carrier type based on Example 1.

[0044] Comparative Example 1: Synthesis of 0.5 wt.% Pd@S-1 catalyst by in-situ encapsulation method.

[0045] 6.5 g TPAOH solution was added to deionized water under stirring, and then 4.16 g TEOS was added dropwise and stirred for 6 h until it became clear and TEOS was completely hydrolyzed. 2 Dissolve 0.0395g ethylenediamine in 3ml water, stir for half an hour, transfer the solution to the PTFE lining of a stainless steel crystallization kettle (100mL), and place it in an oven at 170℃ for 96h. After cooling, wash with deionized water and ethanol and centrifuge to wash away excess template. Then put it in a 100℃ oven to dry for 12h. The dried sample is placed in a muffle furnace and calcined at 550℃ for 6h, and then heated to 400℃ at a heating rate of 15℃ / min in an Ar atmosphere, and replaced with the same flow rate of H 2 The mixture was reduced under an Ar atmosphere for 2 h. Finally, the mixture was replaced with an Ar atmosphere and cooled to room temperature. The powder was collected to obtain the target catalyst 0.5 wt. % Pd@S-1.

[0046] Comparative Examples 2-4 vary the acidity of the HZSM5 carrier based on Example 2.

[0047] Comparative Example 2: Synthesis of 0.5wt.% Pd / HZSM5-20 catalyst by impregnation method.

[0048] The specific implementation conditions are similar to those in Example 2, except that Al(NO 3 ) 3 9H 2 O was 4.0005 g, and the target catalyst 0.5wt.% Pd / HZSM5-20 was obtained.

[0049] Comparative Example 3: A 0.5 wt. % Pd / HZSM5-100 catalyst was synthesized by a hydrothermal method and an impregnation method.

[0050] The specific implementation conditions are similar to those in Example 2, except that Al(NO 3 ) 3 9H 2 O was 0.8001 g, and the target catalyst 0.5wt.% Pd / HZSM5-100 was obtained.

[0051] Comparative Example 4: Synthesis of 0.5 wt.% Pd / S-1 catalyst by impregnation method.

[0052] The S-1 carrier was synthesized by a method similar to that in Example 3, but no metal palladium-related substances were added. After the S-1 carrier was prepared, a 0.5 wt. % Pd / S-1 catalyst was prepared by a conventional impregnation method similar to that in Example 2, but the carrier was changed to S-1, to obtain the target catalyst 0.5 wt. % Pd / S-1.

[0053] Example 3-8: The above catalyst is applied to the catalytic hydrogenation reaction of naphthalene (or dibenzothiophene).

[0054] Example 3: The catalysts obtained in Example 2 and Comparative Examples 2 and 3 were applied to the naphthalene hydrogenation reaction.

[0055] In a typical experiment, 100 mg of naphthalene, 50 mg of catalyst, and 20 mL of n-hexane solvent were placed in a reactor. After sealing, H 2 Remove the remaining air and check the tightness of the reactor. 2 The reactor was pressurized to 2 MPa, the temperature was raised to 220°C, and the reaction was carried out under vigorous stirring at a speed of 800 rpm / min for 60 min. The hydrogenation product was qualitatively and quantitatively analyzed by GC-MS and GC-FID.

[0056] The reaction results of naphthalene hydrogenation using catalysts with different acidic HZSM5 carriers are shown in Table 1. By comparing the naphthalene hydrogenation performance of different acidic HZSM5 carriers, it is found that the catalyst prepared by using HZSM5-50 molecular sieve as a carrier is significantly more active in naphthalene hydrogenation than that prepared by using HZSM5-20 and HZSM5-100 as carriers. For 0.5wt% Pd / HZSM5-20 and 0.5wt% Pd / HZSM5-10, the conversion of naphthalene is only 33.81% and 70.41%, respectively. However, the 0.5wt% Pd / HZSM5-50 catalyst increases the naphthalene conversion rate to 75.18%, and the yields of tetralin and decalin are also improved. The results show that the acidity of the carrier has a significant effect on the catalytic performance of the catalyst. The HZSM5-50 carrier provides a more suitable acid site, which can further promote the naphthalene hydrogenation conversion.

[0057] Table 1 Naphthalene hydrogenation reaction results of catalysts with different acidic HZSM5 supports

[0058]

[0059] Example 4: The catalysts obtained in Example 1, Example 2 and Comparative Example 1 and Comparative Example 4 were applied to the naphthalene hydrogenation reaction. The specific implementation conditions were the same as those in Example 3.

[0060] The reaction results of naphthalene hydrogenation using catalysts prepared by different methods are shown in Table 2. Under the same reaction conditions, 0.5wt% Pd@S-1 is almost inactive, indicating that naphthalene molecules cannot enter the interior of the molecular sieve; the conversion rate of naphthalene hydrogenation catalyzed by 0.5wt% Pd / S-1 is only 3.61%, indicating that the single metal site hydrogenation activity is low; the conversion rates of naphthalene hydrogenation catalyzed by 0.5wt% Pd@HZSM5-50 and 0.5wt% Pd / HZSM5-50 are significantly improved, which are 60.38% and 75.18%, respectively, and the latter is slightly higher than the former. This is because the Pd catalyst encapsulated by the silicon-aluminum molecular sieve (Pd@HZSM-5) synthesized in situ by ethylenediamine complex metal only has hydrogenation at the acidic site assisted by hydrogen overflow. However, the Pd catalyst supported by the silicon-aluminum molecular sieve (Pd / HZSM-5) synthesized by the impregnation method has both metal site and acid site hydrogenation effects, so the hydrogenation activity is slightly improved.

[0061] Table 2 Naphthalene hydrogenation reaction results of different prepared and synthesized catalysts

[0062]

[0063]

[0064] Example 5: The catalysts obtained in Example 1 and Example 2 were applied to the naphthalene hydrogenation reaction. The specific implementation conditions were similar to those in Example 3. However, in a typical experiment, the specific reaction temperature involved was 220-260°C.

[0065] The catalysts obtained in Example 1 and Example 2 were used for the reaction results of naphthalene hydrogenation at different temperatures as shown in Table 3. The results show that the reaction temperature is an important factor affecting the naphthalene hydrogenation reaction. The more suitable reaction temperature of the 0.5wt% Pd@HZSM5-50 catalyst is 220°C, which is slightly different from the other two higher reaction temperatures; on the 0.5wt% Pd / HZSM5-50 catalyst, with the increase of the reaction temperature, the hydrogenation activity of the catalyst increases significantly. Under the condition of a reaction temperature of 260°C, naphthalene can be completely converted, and the yield of decalin is 62.70%, wherein the selectivity of trans-decalin is as high as 71.30%.

[0066] Table 3 Naphthalene hydrogenation reaction results of catalysts at different reaction temperatures

[0067]

[0068] Example 6: The catalysts obtained in Example 1 and Example 2 were applied to the naphthalene hydrogenation reaction. The specific implementation conditions were similar to those in Example 3. However, in a typical experiment, the specific reaction temperature was 200-240° C., and the initial pressure was increased to 2.5 MPa.

[0069] The catalysts obtained in Example 1 and Example 2 are used for the reaction results of catalytic naphthalene hydrogenation at the same pressure and different reaction temperatures as shown in Table 4. When the initial pressure is 2.5MPa, it is found that when the pressure increases from 2MPa (Table 1) to 2.5MPa (Table 4), the catalytic performance of the catalyst is slightly enhanced. At 240°C, the 0.5wt%Pd@HZSM5-50 catalyst increases the conversion rate of naphthalene by about 6%; at 220°C, the 0.5wt%Pd / HZSM5-50 catalyst increases the conversion rate of naphthalene by 11.52%. The naphthalene hydrogenation reaction is a reversible exothermic process, and increasing the pressure is conducive to the forward occurrence of the reaction. However, when hydrogen is excessive during the reaction, the reaction is less affected, which is also the main reason why the catalyst activity is only slightly improved by increasing the pressure.

[0070] Table 4 Naphthalene hydrogenation reaction results of catalysts at different reaction temperatures under the same pressure

[0071]

[0072] Example 7: The catalysts obtained in Examples 1 and 2 were applied to the hydrogenation reaction of naphthalene (containing dibenzothiophene). The specific implementation conditions were similar to those in Example 3, but in a typical experiment, 50 ppm of dibenzothiophene was added to the reactor.

[0073] The reaction results of naphthalene (containing 50ppm dibenzothiophene) hydrogenation under sulfur-containing system catalyzed by the catalyst prepared by in-situ encapsulation and impregnation method are shown in Table 5. The results show that after adding 50ppm dibenzothiophene in the naphthalene hydrogenation catalytic reaction system, the Pd noble metal on the surface of the 0.5wt%Pd / HZSM5-50 catalyst in Example 2 directly contacts with the macromolecular organic sulfur dibenzothiophene, resulting in a significant reduction in catalyst activity, from 75.18% to 13.73%. However, the activity of the 0.5wt%Pd@HZSM5-50 catalyst in Example 1 also decreases, and the naphthalene hydrogenation conversion rate decreases from 60.38% to 24.36%, but the yield of tetralin still maintains at 20.70%, which shows that the catalyst has a good function of resisting the poisoning of macromolecular sulfur-containing organic matter. Figure 8 is the conversion rate of dibenzothiophene in the hydrogenation reaction of naphthalene (including dibenzothiophene) catalyzed by the catalysts obtained in Examples 1 and 2. Due to the good hydrogen overflow ability of Pd metal in the pores, dibenzothiophene molecules are hydrodesulfurized to generate small molecules H 2 S, part H 2 S enters the pores of the molecular sieve in the closed reactor and poisons the Pd metal, thereby reducing the catalytic activity.

[0074] Table 5 Hydrogenation reaction results of naphthalene (containing 50ppm dibenzothiophene) with encapsulated and impregnated catalysts

[0075]

[0076] Example 8: The catalysts prepared in Examples 1 and 2 were applied to the hydrogenation reaction of naphthalene (containing dibenzothiophene). The specific implementation conditions were similar to those in Example 3, but in a typical experiment, 100 ppm of dibenzothiophene was added to the reactor for co-reaction.

[0077] The reaction results of the hydrogenation of naphthalene (containing 100 ppm dibenzothiophene) in a sulfur-containing system catalyzed by the catalyst prepared by the in-situ encapsulation and impregnation method are shown in Table 6. With the increase of macromolecular organic sulfur-containing substances, the catalytic activity of the catalysts prepared in Examples 1 and 2 further decreased, but the activity of the 0.5wt% Pd@HZSM5-50 catalyst was still significantly higher than that of the 0.5wt% Pd / HZSM5-50 catalyst, indicating that the 0.5wt% Pd@HZSM5-50 catalyst also has a certain sulfur-resistant activity in a high sulfur-containing system.

[0078] Table 6 Hydrogenation reaction results of naphthalene (containing 100 ppm dibenzothiophene) with encapsulated and impregnated catalysts

[0079]

[0080] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a sulfur-resistant highly dispersed Pd@HZSM5 molecular sieve catalyst, characterized in that: The following steps are involved: (1) Weighing tetraethyl orthosilicate and tetrapropylammonium hydroxide, stirring and mixing at 80-120° C. for 18-24 hours to form a gel, then adding a mixed solution of aluminum nitrate nonahydrate and sodium hydroxide, and continuing to stir at room temperature for 3-5 hours to obtain a first mixture; (2) adding the ethylenediamine mixed solution containing the palladium precursor to the first mixture obtained in step (1), and continuing stirring for 1-2 hours to obtain a second mixture; (3) transferring the second mixture obtained in step (2) to a hydrothermal reactor, crystallizing at 150-200° C. for 36-48 hours, cooling to room temperature, centrifuging, and drying. The dried solid was ground into powder and then calcined in a muffle furnace for 6 hours to obtain a first solid; (4) subjecting the first solid obtained in step (3) to three consecutive ion exchanges, and then drying the first solid, grinding the dried solid into powder, and calcining the powder in a muffle furnace for 6 hours to obtain a second solid; (5) placing the second solid obtained in step (4) in a tube furnace, heating it to 300-400° C. under an argon atmosphere, then switching to a hydrogen atmosphere, reducing it for 2 h, and then switching back to argon and cooling it to room temperature to obtain a HZSM5 molecular sieve encapsulated palladium catalyst, recorded as Pd@HZSM5 catalyst.

2. The method for preparing a sulfur-resistant highly dispersed Pd@HZSM5 molecular sieve catalyst according to claim 1, characterized in that: The palladium precursor in step (2) is palladium chloride, and the molar ratio of n(Pd) / n(ethylenediamine) is controlled to be 1 / 10.

3. The method for preparing a sulfur-resistant highly dispersed Pd@HZSM5 molecular sieve catalyst according to claim 1, characterized in that: In step (3) and step (4), the calcination temperature is 450-650°C, and the heating rate is 1.5°C / min.

4. The method for preparing a sulfur-resistant highly dispersed Pd@HZSM5 molecular sieve catalyst according to claim 1, characterized in that: The specific operation of ion exchange in step (4) is to stir the first solid with 0.8M NH4Cl solution at 80-100°C for 1-3h.

5. The method for preparing a sulfur-resistant highly dispersed Pd@HZSM5 molecular sieve catalyst according to claim 1, characterized in that: In step (5), the heating rate is 10-15°C / min, and the flow rates of Ar and H2 are both 70-100 mL / min.

6. The method for preparing a sulfur-resistant highly dispersed Pd@HZSM5 molecular sieve catalyst according to claim 1, characterized in that: The n(SiO2 / Al2O3) of the HZSM5 carrier in the Pd@HZSM5 catalyst in step (5) is 50.

7. The method for preparing a highly dispersed Pd@HZSM5 molecular sieve catalyst with anti-sulfurization function according to claim 1, characterized in that: The palladium loading in the Pd@HZSM5 catalyst in step (5) is 0.1wt.%-0.5wt.%.

8. The preparation method according to any one of claims 1 to 7 is used to prepare a sulfur-resistant, highly dispersed Pd@HZSM5 molecular sieve catalyst.

9. Use of the sulfur-resistant highly dispersed Pd@HZSM5 molecular sieve catalyst according to claim 8 in hydrogenation reactions in naphthalene and sulfur-containing systems.

10. The use according to claim 9, characterized in that: The specific application steps include: placing substrate naphthalene or naphthalene containing dibenzothiophene, Pd@HZSM5 catalyst and n-hexane solvent in a reactor, the hydrogenation reaction temperature is 200-260°C, and the hydrogenation reaction pressure is 2.0-2.5MPa.

Citation Information

Patent Citations

  • Molecular sieve catalyst with noble metal Pd encapsulated in situ and production method and application thereof

    CN110270367A

  • Hierarchical pore ZSM-5 molecular sieve packaged Pt-Ni bimetallic catalyst as well as preparation method and application thereof

    CN114558612A

  • Preparation method and application of in-situ packaged Pt-coated H-ZSM-5 catalyst

    CN115722254A

  • Molecular sieve confined monatomic catalyst as well as preparation method and application thereof

    CN116832855A

  • Preparation method and application of zeolite encapsulated metal bifunctional catalyst