Cu-SSZ-13 molecular sieve loaded CeO2 catalyst as well as preparation method and application thereof
Through the preparation of Cu-SSZ-13 molecular sieve-loaded CeO2 catalyst, the problem of simultaneously eliminating soot particles and nitrogen oxides in diesel vehicle exhaust was solved, and efficient and low-cost pollutant degradation effect was achieved.
Patent Information
- Application Number
- CN202410430654.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-11
- Publication Date
- 2024-11-08
AI Technical Summary
The existing diesel vehicle exhaust after-treatment system has problems of low efficiency and high cost in eliminating soot particles and nitrogen oxides. It is difficult for traditional catalysts to effectively degrade these two pollutants at the same time.
The Cu-SSZ-13 molecular sieve supported CeO2 catalyst was used to synthesize it by one-step hydrothermal method and combined with an equal volume impregnation method to prepare a catalyst with excellent redox properties for the elimination of soot particles and nitrogen oxides.
It realizes efficient elimination of soot particles and nitrogen oxides in the same temperature window, reduces the peak temperature of the catalyst, and the NOx conversion rate is greater than 80%, while reducing production costs and device complexity.
Smart Images

Figure CN118904388A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalyst material preparation, and in particular to a Cu-SSZ-13 molecular sieve loaded with CeO 2 Catalyst, preparation method and application thereof. Background Art
[0002] As the importance and necessity of environmental protection and sustainable development in my country become increasingly prominent, the purification and elimination of motor vehicle exhaust pollutants has become a hot topic in the field of environmental protection research. Among them, diesel engine exhaust contains carbon monoxide (CO), nitrogen oxides (NO x ), hydrocarbons (C x H y ) and soot particles and other pollutants. Studies have shown that soot particles and nitrogen oxides in diesel exhaust are the main components of exhaust pollutants, and are also one of the main sources of urban air pollution and acid rain, and also cause serious harm to human health. Therefore, it is an important topic in the field of environmental protection to reduce the emission of diesel exhaust pollutants, especially the elimination of soot particles and nitrogen oxides. At present, a variety of technologies including clean oil technology, engine fuel optimization combustion and exhaust after-treatment technology have been widely studied and used to eliminate soot particles and nitrogen oxides. Among them, catalytic purification of diesel exhaust pollutants before they are discharged into the atmosphere is one of the most effective means to solve the two major environmental pollution problems of diesel exhaust soot particles and nitrogen oxides. However, in the traditional diesel vehicle exhaust after-treatment system, although the combination of soot particle filter (DPF) and selective catalytic reduction (SCR) is considered to be an effective after-treatment technology for eliminating soot particles and nitrogen oxides, the system also has some defects, such as the size of the device and the space required for installation, as well as quality and cost issues. In order to simplify and optimize the aftertreatment system and improve efficiency, researchers have proposed a new catalytic purification technology called SCRPF (Selective Catalytic Reduction and Particulate Filter). This new technology combines the functions of DPF and SCR into one unit, which can effectively reduce or remove PM and NO at the same time. x The key to the development of this catalytic purification technology is the research and development of high-performance catalysts.
[0003] In the simultaneous elimination reaction, the oxidation reaction of soot particles and the reduction reaction of nitrogen oxides proceed simultaneously. Therefore, in order to achieve the effect of simultaneous elimination of soot particles and nitrogen oxides, it is necessary to select a catalyst with moderate redox ability. In the application of selective catalytic reduction technology, the Cu-SSZ-13 molecular sieve catalyst is low in price, large in specific surface area, adjustable in denitration temperature window, and has porosity and abundant acid sites, which are conducive to the high dispersion of active species and the adsorption and activation of reactants. These advantages make it gradually become a hot spot for denitration catalysts. However, the activity of molecular sieves in catalyzing the combustion of soot particles is low. In the catalytic combustion of soot particles, researchers have studied many types of catalysts with different components. Among them, cerium-based oxide catalysts in rare earth metals are considered to have broad application prospects in the study of soot catalytic combustion reactions due to their excellent redox properties, oxygen storage / release capacity and low cost.
[0004] In summary, it is very meaningful to use Cu-SSZ-13 molecular sieve and cerium-based oxide to prepare a catalyst that can be used in the catalytic combustion reaction of soot. Summary of the invention
[0005] The present invention discloses a Cu-SSZ-13 molecular sieve loaded with CeO 2 A catalyst, a preparation method and an application thereof are provided to prepare a catalyst capable of simultaneously eliminating soot particles and nitrogen oxides.
[0006] The present invention provides a Cu-SSZ-13 molecular sieve loaded with CeO 2 Catalyst, wherein CeO 2 Evenly distributed on the Cu-SSZ-13 molecular sieve carrier, the composition formula of the catalyst is: X% CeO 2 / Cu-SSZ-13, where X% represents CeO 2 The mass percentage of the load,
[0007] Preferably, the X%CeO 2 / Cu-SSZ-13, the value of X is 10, 20, 30, 40, 50, 60.
[0008] The present invention also provides a Cu-SSZ-13 molecular sieve loaded with CeO 2 The preparation method of the catalyst comprises: synthesizing a Cu-SSZ-13 molecular sieve carrier by a one-step hydrothermal method, adding different amounts of hexa-Ce 4+ The salt was loaded onto the support by an equal volume impregnation method and finally calcined to obtain X% CeO 2 / Cu-SSZ-13 catalyst.
[0009] Preferably, the Cu-SSZ-13 molecular sieve carrier is synthesized by a one-step hydrothermal method, comprising:
[0010] 1) Dissolve copper sulfate pentahydrate, tetraethylene pentamine and deionized water in a stoichiometric ratio and stir thoroughly for 1.5 hours to form solution A;
[0011] 2) dissolving sodium hydroxide, sodium aluminate and deionized water in a stoichiometric ratio and stirring until clear to form solution B;
[0012] 3) Pour the solution B into the solution A, add 40% silica sol according to the stoichiometric ratio, mix well, and stir for 3 hours to form solution C;
[0013] 4) Solution C was transferred to a reactor, and the reactor was dried in an oven at 140° C. for 96 h, cooled to room temperature, filtered, and the obtained solid was placed in a constant temperature drying oven at 80° C. to form solid D;
[0014] 5) calcining solid D at 550° C. for 6 h in a muffle furnace to obtain Cu-SSZ-13 molecular sieve;
[0015] 6) The Cu-SSZ-13 molecular sieve carrier was placed in a 0.01 mol / L dilute nitric acid solution, reacted in a water bath at 80°C for 12 h, and then filtered, dried at a constant temperature of 80°C, and calcined at 550°C for 4 h to obtain the molecular sieve carrier Cu-SSZ-13.
[0016] Preferably, in step 5), the calcination heating rate is 5°C / min and the temperature is increased to 550°C.
[0017] Preferably, the Ce 4+ The salt is cerium nitrate hexahydrate.
[0018] In addition, the present invention also provides a Cu-SSZ-13 molecular sieve loaded with CeO 2 The application of catalysts is used in the simultaneous elimination of soot particles and nitrogen oxides.
[0019] The Cu-SSZ-13 molecular sieve provided by the present invention is loaded with CeO 2 The preparation method of the catalyst adopts a preparation method combining a hydrothermal method with an equal volume impregnation method, which has the advantages of simple process, rapid reaction, easy operation, low cost, no pollution to the environment, and compliance with green chemistry requirements; the prepared Cu-SSZ-13 molecular sieve loaded with CeO 2 The catalytic material overcomes the problem that traditional catalytic materials can only catalytically degrade soot particles and nitrogen oxides separately, and achieves the simultaneous catalytic degradation and elimination of these two pollutants, which is highly practical and efficient. According to measurements, the peak temperature of PM combustion is 376°C, and NO xThe temperature range for a conversion rate greater than 80% is 147-440°C, achieving efficient elimination of soot particles and nitrogen oxides within the same temperature window.
[0020] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0023] Figure 1 XRD pattern of X%CeO2 / Cu-SSZ-13 catalyst prepared in Example 1-6;
[0024] Where: a:Cu-SSZ-13, b:10% CeO 2 / Cu-SSZ-13, c:20% CeO 2 / Cu-SSZ-13, d:30%CeO 2 / Cu-SSZ-13, e:40% CeO 2 / Cu-SSZ-13, f:50% CeO 2 / Cu-SSZ-13, g: 60% CeO 2 / Cu-SSZ-13;
[0025] Figure 2 X% CeO prepared in Example 1-6 2 / SEM photograph of Cu-SSZ-13 catalyst. DETAILED DESCRIPTION
[0026] The present invention is further explained below in conjunction with specific implementation schemes, but it is not intended to limit the protection scope of the present invention.
[0027] In order to effectively reduce or remove PM and NO emissions from diesel engines xThis embodiment provides a novel binary component molecular sieve catalyst material, which has the catalytic oxidation ability of soot particles by introducing cerium-based oxides in rare earth metals, and combined with the excellent denitrification performance of molecular sieves, a catalytic material with complementary advantages for simultaneously eliminating soot particles and nitrogen oxides is prepared.
[0028] Specifically, the catalyst provided in this embodiment is Cu-SSZ-13 molecular sieve loaded with CeO 2 Catalyst, the expression is: X%CeO 2 / Cu-SSZ-13, where X is CeO 2 Load, the values are 10, 20, 30, 40, 50, 60;
[0029] The catalyst has obvious Cu-SSZ-13 molecular sieve support CHA structural characteristic diffraction peaks and CeO 2 Crystal characteristic diffraction peaks, the carrier presents a spherical structure, CeO 2 The nanoparticles are attached to the surface of the carrier.
[0030] This embodiment provides a Cu-SSZ-13 molecular sieve loaded with CeO in the above embodiment. 2 The preparation method of the catalyst is a synthesis method combining a hydrothermal method with an equal volume impregnation method. The preparation process is simple, and the specific process is as follows:
[0031] 1) Dissolve copper sulfate pentahydrate, tetraethylene pentamine and deionized water in a stoichiometric ratio and stir thoroughly for 1.5 hours to form solution A;
[0032] 2) dissolving sodium hydroxide, sodium aluminate and deionized water in a stoichiometric ratio and stirring until clear to form solution B;
[0033] 3) Pour the solution B into the solution A, add 40% silica sol according to the stoichiometric ratio, mix well, and stir for 3 hours to form solution C;
[0034] 4) Solution C was transferred to a reactor, and the reactor was dried in an oven at 140° C. for 96 h, cooled to room temperature, filtered, and the obtained solid was placed in a constant temperature drying oven at 80° C. to form solid D;
[0035] 5) calcining solid D at 550° C. in a muffle furnace for 6 h to form solid E;
[0036] 6) Solid E was placed in a 0.01 mol / L dilute nitric acid solution, reacted in a water bath at 80°C for 12 hours, then filtered, dried at 80°C, and calcined at 550°C for 4 hours to obtain a molecular sieve carrier Cu-SSZ-13. ;
[0037] 7) Different amounts of cerium salt were loaded onto the support by equal volume impregnation method, followed by calcination to obtain X% CeO 2 / Cu-SSZ-13 catalyst.
[0038] In order to ensure the quality of the molecular sieve carrier Cu-SSZ-13, the calcination heating rate is 5°C / min and the temperature is raised to 550°C; the above-mentioned cerium salt can be selected from cerium nitrate hexahydrate, with an amount of 0.04-0.22g.
[0039] The above Cu-SSZ-13 molecular sieve is loaded with CeO 2 The catalyst can be used in the catalytic reaction of simultaneously eliminating soot particles and nitrogen oxides.
[0040] The present invention is further explained below in conjunction with specific embodiments, but is not intended to limit the protection scope of the present invention.
[0041] Example 1
[0042] 10%CeO 2 Preparation of Cu-SSZ-13 catalyst
[0043] According to the stoichiometric ratio, 3.91g of copper sulfate pentahydrate and 5.96mL of deionized water were weighed, and the above materials were placed in beaker A, and then placed on a magnetic stirrer and stirred until fully dissolved, and then 3.64g of tetraethylene pentamine was added and stirred for 1 hour; in beaker B, 2.32g of sodium aluminate and 6.55g of deionized water were weighed, and then placed on a magnetic stirrer and stirred until the solution was clear, and then 1.72g of sodium hydroxide was added and stirred. The mixture in beaker B was added to beaker A, and then 20.60g of silica sol (30%) was added. After fully stirring for 3 hours, it was added to a polytetrafluoroethylene-lined reactor, placed in an oven for hydrothermal heating for 96h, and the oven temperature was 140°C. After cooling to room temperature, the solution was removed by suction filtration, and the obtained solid was placed in a constant temperature drying oven at 80°C for drying. The dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain Cu-SSZ-13 molecular sieve. The obtained Cu-SSZ-13 molecular sieve was treated in a 0.01mol / L dilute nitric acid solution at a water bath temperature of 80°C for 12 hours. The mass ratio of the Cu-SSZ-13 molecular sieve to the dilute nitric acid solution was 1:100. After the treatment, the solution was cooled to room temperature, and then the solution was removed by suction. The obtained solid was placed in a constant temperature drying oven at 80°C for drying, and the dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain the Cu-SSZ-13 molecular sieve carrier. Weigh 0.1g of the Cu-SSZ-13 molecular sieve carrier and place it in a 50mL beaker. Then, 0.036g of hexahydrated cerium nitrate was dissolved in 1mL of deionized water, and then the cerium nitrate solution was impregnated on the Cu-SSZ-13 molecular sieve carrier. The impregnated solid was placed in a constant temperature drying oven at 80°C for drying. The dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain 10% CeO 2 / Cu-SSZ-13 catalyst.
[0044] The XRD pattern of Cu-SSZ-13 molecular sieve carrier is shown in Figure 1 As shown in the figure, it can be seen that the characteristic diffraction peak of the CHA structure of the catalyst carrier is weakened and CeO 2 Crystal characteristic diffraction peak. Its SEM photo is as follows Figure 2 As shown, CeO appears on the surface of the catalyst support. 2 The activity of the catalyst support in the simultaneous elimination of soot particles and nitrogen oxides is shown in Table 1.
[0045] Example 2
[0046] 20% CeO 2 Preparation of Cu-SSZ-13 catalyst
[0047] At room temperature, 3.91g of copper sulfate pentahydrate was weighed according to a certain stoichiometric ratio, and 5.96mL of deionized water was measured. The above materials were placed in beaker A, and then placed on a magnetic stirrer and stirred until fully dissolved, followed by adding 3.64g of tetraethylene pentamine and stirring for 1 hour; in beaker B, 2.32g of sodium aluminate and 6.55g of deionized water were weighed, and then placed on a magnetic stirrer and stirred until the solution was clear, followed by adding 1.72g of sodium hydroxide and stirring. The mixture in beaker B was added to beaker A, and then 20.60g of silica sol (30%) was added. After stirring for 3 hours, it was added to a polytetrafluoroethylene-lined reactor, placed in an oven for hydrothermal heating for 96h, and the oven temperature was 140°C. After cooling to room temperature, the solution was removed by suction filtration, and the obtained solid was placed in a constant temperature drying oven at 80°C for drying. The dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain Cu-SSZ-13 molecular sieve. The obtained Cu-SSZ-13 molecular sieve was treated in a 0.01mol / L dilute nitric acid solution at a water bath temperature of 80°C for 12 hours. The mass ratio of the Cu-SSZ-13 molecular sieve to the dilute nitric acid solution was 1:100. After the treatment, the solution was cooled to room temperature, and then the solution was removed by suction. The obtained solid was placed in a constant temperature drying oven at 80°C for drying, and the dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain the Cu-SSZ-13 molecular sieve carrier. Weigh 0.1g of the Cu-SSZ-13 molecular sieve carrier and place it in a 50mL beaker. Then, 0.073g of hexahydrated cerium nitrate was dissolved in 1mL of deionized water, and then the cerium nitrate solution was impregnated on the Cu-SSZ-13 molecular sieve carrier. The impregnated solid was placed in a constant temperature drying oven at 80°C for drying. The dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain 20% CeO 2 / Cu-SSZ-13 catalyst.
[0048] The XRD pattern of Cu-SSZ-13 molecular sieve carrier is shown in Figure 1 As shown in the figure, it can be seen that the characteristic diffraction peak of the CHA structure of the catalyst carrier is weakened, and CeO 2 The characteristic diffraction peak of the crystal gradually increases. Its SEM photo is as follows Figure 2 As shown, CeO appears on the surface of the catalyst support. 2 The activity of the catalyst support in the simultaneous elimination of soot particles and nitrogen oxides is shown in Table 1.
[0049] Example 3
[0050] 30% CeO 2 Preparation of Cu-SSZ-13 catalyst
[0051] At room temperature, 3.91g of copper sulfate pentahydrate was weighed according to a certain stoichiometric ratio, and 5.96mL of deionized water was measured. The above materials were placed in beaker A, and then placed on a magnetic stirrer and stirred until fully dissolved, followed by adding 3.64g of tetraethylene pentamine and stirring for 1 hour; in beaker B, 2.32g of sodium aluminate and 6.55g of deionized water were weighed, and then placed on a magnetic stirrer and stirred until the solution was clear, followed by adding 1.72g of sodium hydroxide and stirring. The mixture in beaker B was added to beaker A, and then 20.60g of silica sol (30%) was added. After stirring for 3 hours, it was added to a polytetrafluoroethylene-lined reactor, placed in an oven for hydrothermal heating for 96h, and the oven temperature was 140°C. After cooling to room temperature, the solution was removed by suction filtration, and the obtained solid was placed in a constant temperature drying oven at 80°C for drying. The dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain Cu-SSZ-13 molecular sieve. The obtained Cu-SSZ-13 molecular sieve was treated in a 0.01mol / L dilute nitric acid solution at a water bath temperature of 80°C for 12 hours. The mass ratio of the Cu-SSZ-13 molecular sieve to the dilute nitric acid solution was 1:100. After the treatment, the solution was cooled to room temperature, and then the solution was removed by suction. The obtained solid was placed in a constant temperature drying oven at 80°C for drying, and the dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain the Cu-SSZ-13 molecular sieve carrier. Weigh 0.1g of the Cu-SSZ-13 molecular sieve carrier and place it in a 50mL beaker. Then, 0.109g of hexahydrated cerium nitrate was dissolved in 1mL of deionized water, and then the cerium nitrate solution was impregnated on the Cu-SSZ-13 molecular sieve carrier. The impregnated solid was placed in a constant temperature drying oven at 80°C for drying. The dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain 30% CeO 2 / Cu-SSZ-13 catalyst.
[0052] The XRD pattern of Cu-SSZ-13 molecular sieve carrier is shown in Figure 1 As shown in the figure, it can be seen that the characteristic diffraction peak of the CHA structure of the catalyst carrier is weakened, and CeO 2 The characteristic diffraction peak of the crystal gradually increases. Its SEM photo is as follows Figure 2 As shown in Figure 2, a large amount of CeO appeared on the surface of the catalyst support. 2 The activity of the catalyst support in the simultaneous elimination of soot particles and nitrogen oxides is shown in Table 1.
[0053] Example 4
[0054] 40% CeO 2 Preparation of Cu-SSZ-13 catalyst
[0055] At room temperature, 3.91g of copper sulfate pentahydrate was weighed according to a certain stoichiometric ratio, and 5.96mL of deionized water was measured. The above materials were placed in beaker A, and then placed on a magnetic stirrer and stirred until fully dissolved, followed by adding 3.64g of tetraethylene pentamine and stirring for 1 hour; in beaker B, 2.32g of sodium aluminate and 6.55g of deionized water were weighed, and then placed on a magnetic stirrer and stirred until the solution was clear, followed by adding 1.72g of sodium hydroxide and stirring. The mixture in beaker B was added to beaker A, and then 20.60g of silica sol (30%) was added. After stirring for 3 hours, it was added to a polytetrafluoroethylene-lined reactor, placed in an oven for hydrothermal heating for 96h, and the oven temperature was 140°C. After cooling to room temperature, the solution was removed by suction filtration, and the obtained solid was placed in a constant temperature drying oven at 80°C for drying. The dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain Cu-SSZ-13 molecular sieve. The obtained Cu-SSZ-13 molecular sieve was treated in a 0.01mol / L dilute nitric acid solution at a water bath temperature of 80°C for 12 hours. The mass ratio of the Cu-SSZ-13 molecular sieve to the dilute nitric acid solution was 1:100. After the treatment, the solution was cooled to room temperature, and then the solution was removed by suction. The obtained solid was placed in a constant temperature drying oven at 80°C for drying, and the dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain the Cu-SSZ-13 molecular sieve carrier. Weigh 0.1g of the Cu-SSZ-13 molecular sieve carrier and place it in a 50mL beaker. Then, 0.145g of hexahydrated cerium nitrate was dissolved in 1mL of deionized water, and then the cerium nitrate solution was impregnated on the Cu-SSZ-13 molecular sieve carrier. The impregnated solid was placed in a constant temperature drying oven at 80°C for drying. The dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain 40% CeO 2 / Cu-SSZ-13 catalyst.
[0056] The XRD pattern of Cu-SSZ-13 molecular sieve carrier is shown in Figure 1 As shown in the figure, it can be seen that the characteristic diffraction peak of the CHA structure of the catalyst carrier is weakened, and CeO 2 The characteristic diffraction peak of the crystal gradually increases. Its SEM photo is as follows Figure 2 As shown in Figure 2, a large amount of CeO appeared on the surface of the catalyst support. 2 The activity of the catalyst support in the simultaneous elimination of soot particles and nitrogen oxides is shown in Table 1.
[0057] Example 5
[0058] 50%CeO 2 Preparation of Cu-SSZ-13 catalyst
[0059] At room temperature, 3.91g of copper sulfate pentahydrate was weighed according to a certain stoichiometric ratio, and 5.96mL of deionized water was measured. The above materials were placed in beaker A, and then placed on a magnetic stirrer and stirred until fully dissolved, followed by adding 3.64g of tetraethylene pentamine and stirring for 1 hour; in beaker B, 2.32g of sodium aluminate and 6.55g of deionized water were weighed, and then placed on a magnetic stirrer and stirred until the solution was clear, followed by adding 1.72g of sodium hydroxide and stirring. The mixture in beaker B was added to beaker A, and then 20.60g of silica sol (30%) was added. After stirring for 3 hours, it was added to a polytetrafluoroethylene-lined reactor, placed in an oven for hydrothermal heating for 96h, and the oven temperature was 140°C. After cooling to room temperature, the solution was removed by suction filtration, and the obtained solid was placed in a constant temperature drying oven at 80°C for drying. The dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain Cu-SSZ-13 molecular sieve. The obtained Cu-SSZ-13 molecular sieve was treated in a 0.01mol / L dilute nitric acid solution at a water bath temperature of 80°C for 12 hours. The mass ratio of the Cu-SSZ-13 molecular sieve to the dilute nitric acid solution was 1:100. After the treatment, the solution was cooled to room temperature, and then the solution was removed by suction. The obtained solid was placed in a constant temperature drying oven at 80°C for drying, and the dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain the Cu-SSZ-13 molecular sieve carrier. Weigh 0.1g of the Cu-SSZ-13 molecular sieve carrier and place it in a 50mL beaker. Then, 0.181g of cerium nitrate hexahydrate was dissolved in 1mL of deionized water, and then the cerium nitrate solution was impregnated on the Cu-SSZ-13 molecular sieve carrier. The impregnated solid was placed in a constant temperature drying oven at 80°C for drying. The dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain 50% CeO 2 / Cu-SSZ-13 catalyst.
[0060] The XRD pattern of Cu-SSZ-13 molecular sieve carrier is shown in Figure 1 As shown in the figure, it can be seen that the characteristic diffraction peak of the CHA structure of the catalyst carrier is further weakened and CeO 2 The characteristic diffraction peak of the crystal is strengthened. Its SEM photo is as follows Figure 2 As shown in Figure 2, a large amount of CeO appeared on the surface of the catalyst support. 2 The activity of the catalyst support in the simultaneous elimination of soot particles and nitrogen oxides is shown in Table 1.
[0061] Example 6
[0062] 60% CeO 2 Preparation of Cu-SSZ-13 catalyst
[0063] At room temperature, 3.91g of copper sulfate pentahydrate was weighed according to a certain stoichiometric ratio, and 5.96mL of deionized water was measured. The above materials were placed in beaker A, and then placed on a magnetic stirrer and stirred until fully dissolved, followed by adding 3.64g of tetraethylene pentamine and stirring for 1 hour; in beaker B, 2.32g of sodium aluminate and 6.55g of deionized water were weighed, and then placed on a magnetic stirrer and stirred until the solution was clear, followed by adding 1.72g of sodium hydroxide and stirring. The mixture in beaker B was added to beaker A, and then 20.60g of silica sol (30%) was added. After stirring for 3 hours, it was added to a polytetrafluoroethylene-lined reactor, placed in an oven for hydrothermal heating for 96h, and the oven temperature was 140°C. After cooling to room temperature, the solution was removed by suction filtration, and the obtained solid was placed in a constant temperature drying oven at 80°C for drying. The dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain Cu-SSZ-13 molecular sieve. The obtained Cu-SSZ-13 molecular sieve was treated in a 0.01mol / L dilute nitric acid solution at a water bath temperature of 80°C for 12 hours. The mass ratio of the Cu-SSZ-13 molecular sieve to the dilute nitric acid solution was 1:100. After the treatment, the solution was cooled to room temperature, and then the solution was removed by suction. The obtained solid was placed in a constant temperature drying oven at 80°C for drying, and the dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain the Cu-SSZ-13 molecular sieve carrier. Weigh 0.1g of the Cu-SSZ-13 molecular sieve carrier and place it in a 50mL beaker. Then, 0.218g of hexahydrated cerium nitrate was dissolved in 1mL of deionized water, and then the cerium nitrate solution was impregnated on the Cu-SSZ-13 molecular sieve carrier. The impregnated solid was placed in a constant temperature drying oven at 80°C for drying. The dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain 60% CeO 2 / Cu-SSZ-13 catalyst.
[0064] The XRD pattern of Cu-SSZ-13 molecular sieve carrier is shown in Figure 1 As shown in the figure, it can be seen that the characteristic diffraction peak of the CHA structure of the catalyst carrier is further weakened and CeO 2 The characteristic diffraction peak of the crystal is strengthened. Its SEM photo is as follows Figure 2 As shown in Figure 2, a large amount of CeO appeared on the surface of the catalyst support. 2 The activity of the catalyst support in the simultaneous elimination of soot particles and nitrogen oxides is shown in Table 1.
[0065] Table 1X%CeO 2 Catalytic activity of Cu-SSZ-13 catalyst in simultaneous removal of soot particles and nitrogen oxides
[0066]
[0067] a: Peak temperature of soot combustion
[0068] b: Temperature window where NO conversion is greater than 80%
[0069] c: Maximum NO conversion rate
[0070] Comparative Example 1
[0071] Preparation of Cu-SSZ-13 molecular sieve carrier
[0072] According to the stoichiometric ratio, 3.91g of copper sulfate pentahydrate and 5.96mL of deionized water were weighed, and the above materials were placed in beaker A, and then placed on a magnetic stirrer and stirred until fully dissolved, and then 3.64g of tetraethylene pentamine was added and stirred for 1 hour; in beaker B, 2.32g of sodium aluminate and 6.55g of deionized water were weighed, and then placed on a magnetic stirrer and stirred until the solution was clear, and then 1.72g of sodium hydroxide was added and stirred. The mixture in beaker B was added to beaker A, and then 20.60g of silica sol (30%) was added. After fully stirring for 3 hours, it was added to a polytetrafluoroethylene-lined reactor, placed in an oven for hydrothermal heating for 96h, and the oven temperature was 140°C. After cooling to room temperature, the solution was removed by suction filtration, and the obtained solid was placed in a constant temperature drying oven at 80°C for drying. The dried sample was placed in a muffle furnace and calcined at 550°C for 4h to obtain Cu-SSZ-13 molecular sieve. The obtained Cu-SSZ-13 molecular sieve was treated in a 0.01 mol / L dilute nitric acid solution at a water bath temperature of 80°C for 12 hours. The mass ratio of Cu-SSZ-13 molecular sieve to dilute nitric acid solution was 1:100. After the treatment, the solution was cooled to room temperature and then filtered to remove the solution. The obtained solid was placed in a constant temperature drying oven at 80°C for drying. The dried sample was placed in a muffle furnace and calcined at 550°C for 4 hours to obtain a Cu-SSZ-13 molecular sieve carrier.
[0073] The XRD pattern of Cu-SSZ-13 molecular sieve carrier is shown in Figure 1 As shown in the figure, it can be seen that the catalyst carrier has obvious characteristic diffraction peaks of CHA structure. Figure 2 As shown in Table 1, the catalyst support presents a spherical structure in the shape of a litchi. The activity of the catalyst support in the simultaneous elimination of soot particles and nitrogen oxides is shown in Table 1.
[0074] It can be seen from Table 1 that with the increase of CeO 2 With the increase of loading, the peak temperature of soot combustion is greatly reduced. m =525℃) compared to 50% CeO 2 / Cu-SSZ-13 catalyst (T m=376℃) was reduced by 149℃. The excellent soot combustion activity of the catalyst is attributed to the CeO 2 The redox performance of Cu-SSZ-13 molecular sieve catalyst was improved. 2 As the loading increases, the denitration temperature window of the catalyst becomes narrower, especially reducing the high-temperature denitration performance of the catalyst. The reason may be that the CeO 2 It occupies part of the microporous structure of the Cu-SSZ-13 molecular sieve, reducing the activation of the molecular sieve catalyst for small gas molecules, thereby reducing the denitration performance of the catalyst. On the other hand, due to CeO 2 The loading of the catalyst enhances the redox capacity of the catalyst, resulting in the simultaneous elimination of soot and NO x The NH 3 Oxidation in NH 3 - In the SCR reaction, the reducing agent NH 3 The lack of will inevitably lead to a decrease in the denitrification performance of the catalyst. x In the simultaneous elimination reaction, the elimination of soot occurs through oxidation reaction, NO x Therefore, CeO 2 There is an optimal value for the loading amount of CeO. 2 The loading of CeO will lead to a decrease in the denitration performance of the catalyst. 2 Insufficient loading is not conducive to reducing the combustion temperature of soot. x Reduction factors: 50% CeO 2 / Cu-SSZ-13 catalyst has excellent soot and NO x At the same time, the activity is eliminated, and its T m =376℃, the temperature window where NO conversion rate is greater than 80% is 147℃-440℃. This achieves the same catalyst in the same temperature window for soot and NO x At the same time, the purpose of efficient elimination.
[0075] Based on in situ FTIR characterization, 50% CeO 2 / Cu-SSZ-13 catalyst simultaneously removes soot and NO x The reaction mechanism diagram is as follows: Figure 2 In the denitrification reaction, NH 3 Adsorbed on the acidic sites of the catalyst to form adsorbed NH 3 Species (-NH 3 ), -NH 3 The NO in the gas is measured by the "standard NH 3 -SCR" generates N 2 and H2 O (path 1); in addition, 50% CeO 2 / Cu-SSZ-13 catalyst also has strong NO oxidation ability. NO is oxidized to NO under the action of the catalyst. 2 , the generated NO 2 With -NH 3 By "Quick NH 3 -SCR" reaction generates N 2 and H 2 O (pathway 3). In the denitrification reaction, both pathways 1 and 3 are carried out by the ER mechanism. In the soot oxidation reaction, it is mainly carried out by the active mechanism and NO 2 The auxiliary soot oxidation mechanism is carried out simultaneously. In the active mechanism, O 2 Reacts with the catalyst to generate active oxygen (O * ), the generated O * Directly reacts with soot to generate CO 2 (Pathway 4); in NO 2 In the auxiliary mechanism, NO generated by pathway 2 2 On the one hand, we participated in the “Rapid NH 3 -SCR" reaction, on the other hand, NO 2 With stronger oxidation ability and higher mobility, the generated NO 2 Migrate to the surface of soot and oxidize the soot into CO 2 (Pathway 5), which is itself reduced to NO and enters the next redox cycle.
[0076] Those skilled in the art will readily appreciate other embodiments of the present invention after considering the specification and practicing the invention disclosed herein. This application is intended to cover any variations, uses or adaptations of the present invention that follow the general principles of the present invention and include common knowledge or customary techniques in the art that are not disclosed by the present invention. The specification and examples are to be considered exemplary only, and the true scope and spirit of the present invention are indicated by the following claims.
[0077] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.
Claims
1. A Cu-SSZ-13 molecular sieve loaded CeO2 catalyst, characterized in that: In the catalyst, CeO2 is uniformly distributed on the Cu-SSZ-13 molecular sieve carrier, and the composition formula of the catalyst is: X% CeO2 / Cu-SSZ-13, wherein X% represents the mass percentage of CeO2 loading.
2. The Cu-SSZ-13 molecular sieve supported CeO2 catalyst according to claim 1, characterized in that: In the X% CeO2 / Cu-SSZ-13, the value of X is 10, 20, 30, 40, 50, or 60.
3. The method for preparing the Cu-SSZ-13 molecular sieve supported CeO2 catalyst according to any one of claims 1-2, characterized in that: include: The Cu-SSZ-13 molecular sieve carrier was synthesized by a one-step hydrothermal method. 4+ The salt was loaded onto the support by an equal volume impregnation method, and finally calcined to obtain an X% CeO2 / Cu-SSZ-13 catalyst.
4. The preparation method according to claim 3, characterized in that: The Cu-SSZ-13 molecular sieve support is synthesized by a one-step hydrothermal method, comprising: 1) Dissolve copper sulfate pentahydrate, tetraethylene pentamine and deionized water in a stoichiometric ratio and stir thoroughly for 1.5 hours to form solution A; 2) dissolving sodium hydroxide, sodium aluminate and deionized water in a stoichiometric ratio and stirring until clear to form solution B; 3) Pour the solution B into the solution A, add 40% silica sol according to the stoichiometric ratio, mix well, and stir for 3 hours to form solution C; 4) Solution C was transferred to a reactor, and the reactor was dried in an oven at 140° C. for 96 h, cooled to room temperature, filtered, and the obtained solid was placed in a constant temperature drying oven at 80° C. to form solid D; 5) calcining solid D at 550° C. for 6 h in a muffle furnace to obtain Cu-SSZ-13 molecular sieve; 6) The Cu-SSZ-13 molecular sieve carrier was placed in a 0.01 mol / L dilute nitric acid solution, reacted in a water bath at 80°C for 12 h, and then filtered, dried at a constant temperature of 80°C, and calcined at 550°C for 4 h to obtain the molecular sieve carrier Cu-SSZ-13.
5. The method for preparing the Cu-SSZ-13 molecular sieve loaded CeO2 catalyst according to claim 2, characterized in that: In step 5), the calcination heating rate is 5°C / min and the temperature is increased to 550°C.
6. The method for preparing the Cu-SSZ-13 molecular sieve loaded CeO2 catalyst according to claim 3, characterized in that: The Ce 4+ The salt is cerium nitrate hexahydrate.
7. An application of the Cu-SSZ-13 molecular sieve loaded CeO2 catalyst according to claim 1, characterized in that: Used in the simultaneous elimination of soot particles and nitrogen oxides.
Citation Information
Patent Citations
Preparation method for synthesizing Cu-SSZ-39 molecular sieve based catalyst by using one-step method and application
CN106799255A
SCR catalyst capable of resisting water sulfur poisoning and hydrothermal aging and preparation method thereof
CN112675900A
MnOx-loaded Cu-SSZ-13 molecular sieve composite catalyst as well as preparation method and application thereof
CN115672390A
Preparation method and application of supported CeO2 / Cu-SSZ-13 composite catalyst
CN116532151A
Method for preparing Cu-SSZ-13 molecular sieve catalyst through mechanical pressurization water heat exchange loaded copper and application of Cu-SSZ-13 molecular sieve catalyst
CN117258834A
Cited By
Preparation method and application of high-efficiency low-N2O-selectivity monolithic CeOx-Cu / SSZ-13 catalyst
CN121402136A