Environment-friendly efficient self-cleaning photocatalytic mixed matrix membrane as well as preparation method and application thereof

By using the combination of MIL-125(Ti) with carboxylated nanofibers and PVDF in water treatment technology, an efficient self-cleaning photocatalytic mixed matrix membrane was prepared, which solved the problem of insufficient water treatment performance in the prior art and achieved high The improvement of permeability and self-cleaning function significantly improves the removal efficiency of organic pollutants and the stability of the membrane.

CN118904400APending Publication Date: 2024-11-08JIANGSU UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411056893.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing water treatment technology has shortcomings in removing organic pollutants and sterilization, and the preparation of MOF-enhanced mixed matrix membranes faces the problems of poor compatibility and dispersion of fillers and polymer matrixes, which affects the overall performance.

Method used

The MIL-125(Ti) crystal was synthesized by hydrothermal method using an efficient self-cleaning photocatalytic mixed matrix film composed of MIL-125(Ti), carboxylated nanofibers (CNF-C) and polyvinylidene fluoride (PVDF). Combined with PVDF, CNF-C and PVP, a membrane with a high specific surface area and self-cleaning function is formed.

Benefits of technology

It significantly improves the permeability, mechanical properties and self-cleaning function of the hybrid matrix membrane, enhances the efficiency of removing organic pollutants, reduces maintenance needs and operating costs, and complies with the principle of green chemistry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904400A_ABST
    Figure CN118904400A_ABST
Patent Text Reader

Abstract

The invention provides an environment-friendly efficient self-cleaning photocatalytic mixed matrix membrane and a preparation method and application thereof.The preparation method includes the steps that MIL-125 (Ti) crystals are prepared from carboxylic acid ligands, titanium salt and methyl alcohol through a hydrothermal reaction, and then the high-permeability mixed matrix membrane is successfully prepared from polyvinylidene fluoride (PVDF) and polyvinylpyrrolidone (PVP). Carboxylated nanofibers (CNF-C), MIL-125 (Ti), polyvinylidene fluoride (PVDF) and polyvinylpyrrolidone (PVP) are adopted to prepare a membrane casting solution, and after the membrane casting solution is coated, a non-solvent induced phase separation (NIPS) technology is adopted to prepare the mixed matrix membrane. According to the invention, carboxylated nanofibers (CNF-C) and MIL-125 (Ti) are incorporated into a polyvinylidene fluoride (PVDF) and polyvinylpyrrolidone (PVP) matrix, the prepared matrix membrane has high wettability, rich functional groups, high porosity and high specific surface area, and the mixed matrix membrane shows excellent organic dye permeation and removal capability and remarkable self-cleaning characteristic in wastewater purification.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a green and environmentally friendly high-efficiency self-cleaning photocatalytic mixed matrix membrane and a preparation method and application thereof, belonging to the technical field of membrane water treatment. Background Art

[0002] Although traditional water treatment technologies such as precipitation, filtration, and adsorption can remove pollutants to a certain extent, they have many shortcomings in removing organic pollutants and sterilizing and disinfecting. Therefore, finding an efficient, environmentally friendly, and economical water treatment technology has become a research hotspot. In recent years, photocatalytic technology has become an important research direction in the field of water treatment due to its excellent pollutant degradation performance, reusability, and environmental friendliness.

[0003] In recent years, photocatalytic technology has shown great potential in the application of mixed matrix membranes (MMMs) to remove organic pollutants from water. In particular, functionalized metal organic frameworks (MOFs) have become popular candidates in the field of light harvesting and photocatalysis due to their excellent semiconductor properties. MIL-125 (Ti) is a metal organic framework (MOF) material composed of TiO2 and organic ligands, which has excellent photocatalytic performance. Compared with traditional TiO2, MIL-125 (Ti) has the following advantages in membrane treatment technology: 1) It has a wide light absorption range, which can effectively utilize visible light energy and improve photocatalytic efficiency; 2) It shows high stability under light conditions, is not prone to photocorrosion, and ensures catalytic performance in long-term use; 3) It has excellent self-cleaning ability, which can effectively prevent pollutants from depositing on its surface and maintain photocatalytic activity; 4) It can be loaded on different substrates such as fiber, glass, ceramic, polymer film, etc. through various methods to form a mixed matrix membrane; 5) Unlike some photocatalytic materials doped with heavy metal elements, MIL-125 (Ti) is composed of non-toxic metals and organic ligands, which is environmentally friendly and avoids secondary pollution problems. Studies have shown that after pollutants are adsorbed on the surface of MIL-125 (Ti), their photosensitization will cause a red shift in the absorption spectrum, thereby generating holes and superoxide radicals, effectively promoting the decomposition of organic pollutants.

[0004] PVDF is widely used as a membrane substrate due to its excellent chemical stability, mechanical strength and heat resistance. However, PVDF itself is highly hydrophobic and easily causes membrane fouling problems. However, the preparation of ideal MOF-enhanced mixed matrix membranes still faces many challenges. First, the poor compatibility between the filler and the polymer matrix often leads to non-selective defects. Secondly, the poor dispersibility and easy agglomeration of the filler in the polymer matrix still exist. These problems are closely related to the structural properties of the filler and seriously affect the overall performance and application effect of the mixed matrix membrane. Therefore, the development of new and efficient fillers and the optimization of the compatibility of fillers with polymer matrices are key technical issues that need to be urgently solved in the current research and application of mixed matrix membranes in the field of water purification. Summary of the invention

[0005] The present invention proposes a novel high permeability and self-cleaning mixed matrix membrane and its preparation method and application. The method focuses on cost-effectiveness, energy efficiency and sustainability, and can prepare a structurally stable mixed matrix membrane with a high specific surface area. This mixed matrix membrane not only exhibits excellent permeability and high efficiency in removing organic dyes, but also has a self-cleaning function, making it have a wide range of application potential in the fields of wastewater purification and environmental protection.

[0006] The technical solution adopted by the present invention to solve the above technical problems is as follows:

[0007] A method for preparing a green and environmentally friendly high-efficiency self-cleaning photocatalytic mixed matrix membrane, characterized in that it comprises the following steps:

[0008] (1) Synthesis of MIL-125(Ti): dissolving a carboxylic acid ligand in an organic solvent A to form a uniform mixed solution; then, adding a titanium salt to the mixed solution, and adding methanol, mixing, and performing a hydrothermal reaction in a reactor. After the reaction is completed, centrifugation and vacuum drying are performed to obtain MIL-125(Ti) crystals;

[0009] (2) Preparation of mixed matrix membrane: The MIL-125 (Ti) crystals, carboxylated nanofibers (CNF-C), and polyvinyl pyrrolidone (PVP) synthesized in step (1) are placed in an organic solvent B for ultrasonic dissolution, and then polyvinylidene fluoride (PVDF) is added, and heated and stirred to form a homogeneous casting solution; the casting solution is coated on a coating machine, and the coated membrane is placed in deionized water for 8 to 12 hours for phase separation, and finally vacuum dried to obtain a high-efficiency self-cleaning photocatalytic mixed matrix membrane.

[0010] Furthermore, the carboxylic acid ligand in step (1) is any one or more of terephthalic acid, 2,6-naphthalene dicarboxylic acid, and tetraphenyl dicarboxylic acid, the organic solvent A is one or more of N,N-dimethylformamide, cyclohexane, and trichloroethylene, and the titanium salt is tetrabutyl titanate.

[0011] Furthermore, the amount of titanium salt added is 1-2 mL, the amount of methanol added is 5-10 mL, and the amount of organic solvent added is 30-50 mL.

[0012] Furthermore, the temperature of the hydrothermal reaction in step (1) is 150-180°C, the reaction time is 16-24 hours, the centrifugal speed is 8000-10000 rpm, the centrifugal time is 8-10 minutes / time, for a total of 2-4 times, and the drying condition is vacuum drying at 70-80°C for 10-12 hours.

[0013] Furthermore, in step (2), the organic solvent B is one or more of N-methylpyrrolidone, styrene, and n-hexane, and the mass fraction of the solute is 16-30%, wherein the mass fraction of the carboxylated nanofibers (CNF-C) is 1-5%.

[0014] Furthermore, in the step (2), the weight ratio of MIL-125 (Ti) crystal, carboxylated nanofiber (CNF-C), polyvinyl pyrrolidone (PVP), and polyvinylidene fluoride (PVDF) is 2-8:1-4:0.5:15.

[0015] Furthermore, the coating process parameters in step (2) are: advancing speed of 5 mm / s, sedimentation time in water of 8 to 12 h, drying conditions of 70 to 80° C., and vacuum drying for 2 to 4 h.

[0016] The high-efficiency self-cleaning photocatalytic mixed matrix membrane prepared by the preparation method is characterized in that the mixed matrix membrane is mainly composed of MIL-125 (Ti), carboxylated nanofibers (CNF-C), polyvinyl pyrrolidone (PVP) and polyvinylidene fluoride (PVDF), and the weight fraction of MIL-125 (Ti) crystals, carboxylated nanofibers (CNF-C), polyvinyl pyrrolidone (PVP), and polyvinylidene fluoride (PVDF) is 2 to 8:1 to 4:0.5:15, and the mixed matrix membrane has a finger-like pore structure with a diameter of micrometers in the thickness direction of the membrane.

[0017] Furthermore, the specific surface area of ​​the mixed matrix membrane is not less than 276.24 m 2 / g.

[0018] The highly efficient self-cleaning photocatalytic mixed matrix membrane is used for water treatment.

[0019] The beneficial effects of the present invention are:

[0020] (1) The synergistic effect between the components significantly improves the water flux and hydrophilicity of the mixed matrix membrane: Carboxylated nanofibers (CNF-C) have a high specific surface area and good mechanical properties, which can effectively enhance the structural strength and durability of the membrane. The present invention uses carboxylated nanofibers, and the carboxylation modification of the nanofibers greatly improves their hydrophilicity. When the content of carboxylated nanofibers (CNF-C) increases from 1wt% to 4wt%, the pure water permeability of the mixed matrix membrane increases from 283L m –2 h –1 bar -1 Increased to 340L m –2 h –1 bar -1 The flux recovery rate remained above 91%, and the contact angle decreased to 42°. When the MIL-125(Ti) loading rate was 8 wt%, the pure water permeability of the mixed matrix membrane reached 410 L m –2 h –1 bar -1 , the flux recovery rate was maintained above 94%, and the contact angle was further reduced to 30°, showing excellent anti-pollution and stability.

[0021] The PVP is dispersed in the PVDF matrix, which helps to regulate the pore size of the membrane and increase the hydrophilicity of the membrane. The presence of PVP can form a hydration layer on the PVDF surface, reducing the adhesion of organic matter to the membrane.

[0022] (2) The optimization of MIL-125 (Ti) loading significantly enhanced the mechanical properties of the mixed matrix membrane: when the MIL-125 (Ti) loading rate was increased from 2wt% to 10wt%, the tensile strength of the mixed matrix membrane increased from 12.96MPa to 15.38MPa, and the maximum elongation at break reached 121.6%, which showed high toughness.

[0023] (3) The mixed matrix membrane exhibits excellent self-cleaning function: The MIL-125 (Ti) nanomaterial synthesized in the present invention is a porous framework structure with a specific surface area of ​​up to 276.24 m 2 / g, and can catalytically decompose organic pollutants under ultraviolet or visible light irradiation to achieve self-cleaning function. When the loading amount of MIL-125(Ti) is 8wt%, the degradation rate of methylene blue (MB) can reach 97.83%, and the permeation flux can reach 233.7L m –2 h –1 bar -1 .

[0024] (4) The raw materials used in the present invention, such as PVDF, CNF and MIL-125(Ti), are all low-cost and easily available. The preparation process is simple and effective and can be easily expanded to large-scale production. These characteristics make the PVDF / MIL-125(Ti) / CNF mixed matrix membrane a new type of separation membrane material, which is significantly superior to traditional membrane materials in terms of organic pollutant removal efficiency, showing the potential to replace existing technologies.

[0025] (5) The self-cleaning ability of the PVDF / MIL-125(Ti) / CNF-C mixed matrix membrane is in line with the principles of green chemistry and the country's sustainable development strategy. The self-cleaning function of the membrane reduces the need for cleaning and the associated maintenance costs, while reducing the overall environmental impact.

[0026] Therefore, in the high-efficiency self-cleaning photocatalytic mixed matrix membrane prepared by the present invention, PVP, MIL-125 (Ti) and CNF enhance the hydrophilicity and structural stability of PVDF through physical and chemical effects, and the high specific surface area and porosity of MIL-125 (Ti) itself make it have high catalytic activity, so that the membrane can spontaneously degrade organic pollutants under natural light conditions, and improve the self-cleaning ability of the membrane. At the same time, the finger-like micropores densely distributed in the thickness direction of the matrix membrane prepared by the present invention make the matrix membrane have a higher specific surface area and porosity, significantly improve the membrane's permeability, pollutant removal ability and self-cleaning performance characteristics, can significantly reduce maintenance requirements and operating costs, so that the membrane material has high economic benefits and application potential in industrial and environmental applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 . Flow chart of preparation of PVDF / MIL-125(Ti) / CNF-C mixed matrix membrane.

[0028] Figure 2 This is a scanning electron microscope image of MIL-125(Ti) synthesized by hydrothermal method.

[0029] Figure 3 Transmission electron microscope image of MIL-125(Ti) synthesized by hydrothermal method.

[0030] Figure 4The scanning electron microscope images of the surface and cross section of the mixed matrix membranes with different MIL-125 (Ti) loadings. (a) to (f) are the surface morphologies of the mixed matrix membranes, and (g) to (l) are the cross-sectional morphologies of the mixed matrix membranes. (a) and (g) are the surface and cross-section of PCM-1 with a MIL-125 (Ti) loading of 0 wt% prepared in Example 1; (b) and (h) are the surface and cross-section of TiPCM-1 and PCM-2 with a MIL-125 (Ti) loading of 2 wt% prepared in Example 5; (c) and (i) are the surface and cross-section of TiPCM-2 with a MIL-125 (Ti) loading of 4 wt% prepared in Example 6; (d) and (j) are the surface and cross-section of TiPCM-3 with a MIL-125 (Ti) loading of 6 wt% prepared in Example 7; (e) and (k) are the surface and cross-section of TiPCM-4 with a MIL-125 (Ti) loading of 8 wt% prepared in Example 8; (f) and (l) are the surface and cross-section of TiPCM-5 with a MIL-125 (Ti) loading of 10 wt% prepared in Example 9.

[0031] Figure 5 The tensile stress-strain curves of the PVDF / MIL-125(Ti) / CNF-C mixed matrix membranes prepared in Examples 5 to 9.

[0032] Figure 6 This is the infrared spectrum of the PVDF / MIL-125(Ti) / CNF-C mixed matrix membrane prepared in Example 8.

[0033] Figure 7 Pure water permeability (J) and flux recovery rate (FRR) of different types of mixed matrix membranes; (a) PCM-1 prepared in Example 1; (b) PCM-2 prepared in Example 2; (c) PCM-3 prepared in Example 3; (d) PCM-4 prepared in Example 4; (e) TiPCM-1 prepared in Example 5; (f) TiPCM-2 prepared in Example 6; (g) TiPCM-3 prepared in Example 7; (h) TiPCM-4 prepared in Example 8; (i) TiPCM-5 prepared in Example 9.

[0034] Figure 8 Dynamic water contact angles (WCA) of different types of mixed matrix membranes. (a) WCA of PCMs with different CNF-C loadings; (b) WCA of TiPCMs with different MIL-125(Ti) loadings.

[0035] Fig. 9 The dye rejection rate (a) and permeability (b) of PVDF / MIL-125(Ti) / CNF mixed matrix membrane.

[0036] Fig.10 This is a test of the self-cleaning performance of PVDF / MIL-125(Ti) / CNF mixed matrix membrane.

[0037] Fig.11 This is the self-cleaning color change diagram of PVDF / MIL-125(Ti) / CNF mixed matrix membrane.

[0038] Fig.12 Schematic diagram of the self-cleaning mechanism of PVDF / MIL-125(Ti) / CNF mixed matrix membrane. DETAILED DESCRIPTION

[0039] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited thereto.

[0040] Example 1

[0041] Weigh 0.1g carboxylated nanofibers (CNF-C), 0.05g polyvinyl pyrrolidone and 8.35g N-methyl pyrrolidone, add CNF-C and polyvinyl pyrrolidone to N-methyl pyrrolidone, first ultrasonically disperse for 10min, then add 1.5g polyvinylidene fluoride to the above solution, stir at 70℃ for 8h, and let stand for 12h to obtain a homogeneous casting solution. Pour the casting solution onto the glass plate of the coating machine, coat it with a coating rod (coating speed is 5mm / s), then put the glass plate into deionized water for 30min for phase separation, and then put the membrane after phase separation into deionized water for deposition for 12h to obtain a PVDF / CNF-C mixed matrix membrane, which is called PCM-1.

[0042] Example 2

[0043] Weigh 0.2g CNF-C, 0.05g polyvinyl pyrrolidone and 8.25g N-methyl pyrrolidone, add CNF-C and polyvinyl pyrrolidone to N-methyl pyrrolidone, first ultrasonically disperse for 10min, then add 1.5g polyvinylidene fluoride to the above solution, stir at 70℃ for 8h, and let stand for 12h to obtain a homogeneous casting solution. Pour the casting solution onto the glass plate of the coating machine, and coat it with a coating rod (coating speed is 5mm / s), then put the glass plate into deionized water for 30min for phase separation, and then put the membrane after phase separation into deionized water for deposition for 12h to obtain a PVDF / CNF-C mixed matrix membrane, which is called PCM-2.

[0044] Example 3

[0045] Weigh 0.3g CNF-C, 0.05g polyvinyl pyrrolidone and 8.15g N-methyl pyrrolidone, add CNF-C and polyvinyl pyrrolidone to N-methyl pyrrolidone, first ultrasonically disperse for 10 minutes, then add 1.5g polyvinylidene fluoride to the above solution, stir at 70°C for 8 hours, and stand for 12 hours to obtain a homogeneous casting solution. Pour the casting solution on the glass plate of the coating machine, coat it with a coating rod (coating speed is 5mm / s), then put the glass plate into deionized water for 30 minutes for phase separation, and then put the membrane after phase separation into deionized water for deposition for 12 hours to obtain a PVDF / CNF-C mixed matrix membrane, which is called PCM-3.

[0046] Example 4

[0047] Weigh 0.4g CNF-C, 0.05g polyvinyl pyrrolidone and 8.05g N-methyl pyrrolidone, add CNF-C and polyvinyl pyrrolidone to N-methyl pyrrolidone, first ultrasonically disperse for 10 minutes, then add 1.5g polyvinylidene fluoride to the above solution, stir at 70°C for 8 hours, and stand for 12 hours to obtain a homogeneous casting solution. Pour the casting solution on the glass plate of the coating machine, and coat it with a coating rod at a coating speed of 5mm / s. Then put the glass plate into deionized water for 30 minutes for phase separation, and then put the membrane after phase separation into deionized water for deposition for 12 hours to obtain a PVDF / CNF-C mixed matrix membrane, which is called PCM-4.

[0048] Example 5

[0049] 1.8 g of terephthalic acid was dissolved in 40 mL of DMF and ultrasonically treated for 30 min to form solution A; 1 mL of tetrabutyl titanate and 6 mL of anhydrous methanol were added to solution A and stirred at room temperature for 6 h, and the mixed solution was transferred to a polytetrafluoroethylene reaction container and hydrothermally reacted at 150 ° C for 24 h. Subsequently, the product was collected by centrifugation at a centrifugal speed of 9000 r / min for 8 min and washed with methanol and DMF three times. The milky white precipitate obtained after centrifugation was placed in an oven and dried at 70 ° C for 12 h to obtain MIL-125 (Ti) nanoparticles. Figure 2 , Figure 3 The scanning electron microscope image and transmission electron microscope image of the MIL-125 (Ti) nanoparticles prepared in this embodiment clearly show that MIL-125 (Ti) has a regular and ordered truncated cone structure, with a diameter ranging from 400 to 540 nm and a height ranging from 250 to 350 nm, with a relatively consistent size, a smooth surface and clear edges.

[0050] Weigh 0.4 g CNF-C, 0.2 g MIL-125 (Ti), 0.05 g polyvinyl pyrrolidone and 7.85 g N-methyl pyrrolidone, add CNF-C, MIL-125 (Ti), and polyvinyl pyrrolidone to N-methyl pyrrolidone, first ultrasonically disperse for 10 min, then add 1.5 g polyvinylidene fluoride to the above solution, stir at 70 ° C for 8 h, and let stand for 12 h to obtain a homogeneous casting solution.

[0051] The casting liquid was poured onto the glass plate of the coating machine and coated with a coating rod at a coating speed of 5 mm / s. The glass plate was then placed in deionized water for 30 minutes for phase separation. The membrane after phase separation was placed in deionized water for deposition for 12 hours to obtain a PVDF / MIL-125(Ti) / CNF-C mixed matrix membrane, which was called TiPCM-1.

[0052] Example 6

[0053] 1.8 g of terephthalic acid was dissolved in 40 mL of DMF and ultrasonically treated for 30 min to form solution A; 1 mL of tetrabutyl titanate and 6 mL of anhydrous methanol were added to solution A and stirred at room temperature for 6 h, and the mixed solution was transferred to a polytetrafluoroethylene reaction container and reacted at 150 ° C for 24 h. Subsequently, the product was collected by centrifugation (9000 r / min, 8 min) and washed with methanol and DMF three times. The milky white precipitate obtained after centrifugation was placed in an oven and dried at 70 ° C for 12 h to obtain MIL-125 (Ti) nanoparticles.

[0054] Weigh 0.4 g CNF-C, 0.4 g MIL-125 (Ti), 0.05 g polyvinyl pyrrolidone and 7.65 g N-methyl pyrrolidone, add CNF-C, MIL-125 (Ti) and polyvinyl pyrrolidone to N-methyl pyrrolidone, first ultrasonically disperse for 10 min, then add 1.5 g polyvinylidene fluoride to the above solution, stir at 70 ° C for 8 h, and let stand for 12 h to obtain a homogeneous casting solution.

[0055] The casting liquid was poured onto the glass plate of the coating machine and coated with a coating rod at a coating speed of 5 mm / s. The glass plate was then placed in deionized water for 30 minutes for phase separation. The membrane after phase separation was placed in deionized water for deposition for 12 hours to obtain a PVDF / MIL-125(Ti) / CNF-C mixed matrix membrane, which was called TiPCM-2.

[0056] Example 7

[0057] 1.8 g of terephthalic acid was dissolved in 40 mL of DMF and ultrasonically treated for 30 min to form solution A; 1 mL of tetrabutyl titanate and 6 mL of anhydrous methanol were added to solution A and stirred at room temperature for 6 h, and the mixed solution was transferred to a polytetrafluoroethylene reaction container and reacted at 150 ° C for 24 h. Subsequently, the product was collected by centrifugation (9000 r / min, 8 min) and washed with methanol and DMF three times. The milky white precipitate obtained after centrifugation was placed in an oven and dried at 70 ° C for 12 h to obtain MIL-125 (Ti) nanoparticles.

[0058] Weigh 0.4g CNF-C, 0.6g MIL-125(Ti), 0.05g polyvinyl pyrrolidone and 7.45g N-methyl pyrrolidone, add CNF-C, MIL-125(Ti) and polyvinyl pyrrolidone to N-methyl pyrrolidone, first ultrasonically disperse for 10min, then add 1.5g polyvinylidene fluoride to the above solution, stir at 70℃ for 8h, and stand for 12h to obtain a homogeneous casting solution. Pour the casting solution on the glass plate of the coating machine, and coat it with a coating rod at a coating speed of 5mm / s. Then put the glass plate into deionized water for 30min for phase separation, and then put the membrane after phase separation into deionized water for deposition for 12h to obtain a PVDF / MIL-125(Ti) / CNF-C mixed matrix membrane, which is called TiPCM-3.

[0059] Example 8

[0060] 1.8 g of terephthalic acid was dissolved in 40 mL of DMF and ultrasonically treated for 30 min to form solution A; 1 mL of tetrabutyl titanate and 6 mL of anhydrous methanol were added to solution A and stirred at room temperature for 6 h, and the mixed solution was transferred to a polytetrafluoroethylene reaction container and reacted at 150 ° C for 24 h. Subsequently, the product was collected by centrifugation (9000 r / min, 8 min) and washed with methanol and DMF three times. The milky white precipitate obtained after centrifugation was placed in an oven and dried at 70 ° C for 12 h to obtain MIL-125 (Ti) nanoparticles.

[0061] Weigh 0.4g CNF-C, 0.8g MIL-125(Ti), 0.05g polyvinyl pyrrolidone and 7.25g N-methyl pyrrolidone, add CNF-C, MIL-125(Ti) and polyvinyl pyrrolidone to N-methyl pyrrolidone, first ultrasonically disperse for 10min, then add 1.5g polyvinylidene fluoride to the above solution, stir at 70℃ for 8h, and stand for 12h to obtain a homogeneous casting solution. Pour the casting solution onto the glass plate of the coating machine, and coat it with a coating rod at a coating speed of 5mm / s. Then put the glass plate into deionized water for 30min for phase separation, and then put the membrane after phase separation into deionized water for deposition for 12h to obtain a PVDF / MIL-125(Ti) / CNF-C mixed matrix membrane, which is called TiPCM-4.

[0062] Example 9

[0063] 1.8 g of terephthalic acid was dissolved in 40 mL of DMF and ultrasonically treated for 30 min to form solution A; 1 mL of tetrabutyl titanate and 6 mL of anhydrous methanol were added to solution A and stirred at room temperature for 6 h, and the mixed solution was transferred to a polytetrafluoroethylene reaction container and reacted at 150 ° C for 24 h. Subsequently, the product was collected by centrifugation (9000 r / min, 8 min) and washed with methanol and DMF three times. The milky white precipitate obtained after centrifugation was placed in an oven and dried at 70 ° C for 12 h to obtain MIL-125 (Ti) nanoparticles.

[0064] Weigh 0.4g CNF-C, 1.0g MIL-125(Ti), 0.05g polyvinylpyrrolidone and 7.05g N-methylpyrrolidone, add CNF-C, MIL-125(Ti) and polyvinylpyrrolidone to N-methylpyrrolidone, first ultrasonically disperse for 10min, then add 1.5g polyvinylidene fluoride to the above solution, stir at 70℃ for 8h, and stand for 12h to obtain a homogeneous casting solution. Pour the casting solution onto the glass plate of the coating machine, and coat it with a coating rod at a coating speed of 5mm / s. Then put the glass plate into deionized water for 30min for phase separation, and then put the membrane after phase separation into deionized water for deposition for 12h to obtain a PVDF / MIL-125(Ti) / CNF-C mixed matrix membrane, which is called TiPCM-5.

[0065] From PCM-1 to TiPCM-5, the increase in MIL-125(Ti) loading brought about significant structural changes in the structure of the mixed matrix membrane. Figure 4(a) to (f), as the content of MIL-125 (Ti) increases, the roughness of the mixed matrix membrane surface gradually increases. This is because the introduction of MIL-125 (Ti) nanoparticles leads to the formation of more tiny concave and convex structures on the surface of the mixed matrix membrane, thereby increasing the surface area, that is, increasing the specific surface area of ​​the mixed matrix membrane, thereby improving the membrane's filtration efficiency and pollutant adsorption capacity. Figure 4 (g) to (l), all the mixed matrix membranes prepared in the examples of the present invention have a typical finger-like pore structure, and as the loading amount of MIL-125(Ti) gradually increases, the internal structure of the mixed matrix membrane shows more obvious porosity and layering, the pore size and pore structure of the mixed matrix membrane change significantly, and the pores are more uniform and more densely distributed. Figure 4 In (k) and (l), the membranes containing a higher proportion of MIL-125(Ti) show a more complex and well-defined pore structure. The presence of these pores plays an important role in improving the permeability and selective filtration of the membrane, and can effectively promote the separation of water and harmful substances.

[0066] Figure 5 The tensile stress-strain curves of mixed matrix membranes with different MIL-125 (Ti) loadings are shown. The mechanical strength of the membrane increases significantly with the increase of MIL-125 (Ti) content. As shown in Table 1, the Young's modulus of TiPCM-1 to TiPCM-5 are approximately 12.96 MPa, 13.43 MPa, 14.43 MPa, 15.27 MPa and 15.38 MPa, respectively. It can be seen that MIL-125 (Ti) enhances the mechanical properties of the membrane, making it more resistant under tensile stress. This is mainly attributed to the addition of MIL-125 (Ti) nanoparticles, which increase the rigidity and strength of the membrane. PCMT-4 exhibits the largest elongation at break, which is 121.6%, and has high toughness. Further increasing the loading of MIL-125 (Ti) will cause molecular chain accumulation, making the membrane material brittle.

[0067] Table 1. Tensile strength and elongation at break of PVDF / MIL-125(Ti) / CNF-C mixed matrix membranes

[0068] TiPCM-1 TiPCM-2 TiPCM-3 TiPCM-4 TiPCM-5 Tensile strength(MPa) 12.96 13.43 14.43 15.27 15.38 Elongation at break (%) 119 93.5 97.3 121.6 67.2

[0069] Figure 6 The FTIR spectrum of Example 8 (TiPCM-4) shows multiple characteristic absorption peaks: 2930 cm -1 The peak at 1750 cm is attributed to the stretching vibration of CH; -1 and 1280cm -1 The peak at 1420 cm corresponds to the stretching vibration of C=O and CO;-1 The peak at 1200cm is related to the vibration of the benzene ring skeleton; -1 The peak at 840 cm is attributed to CF stretching vibration; -1 and 880cm -1 The peaks at and are attributed to the vibration of Ti-O-Ti, respectively. MIL-125(Ti) and CNF-C were successfully introduced and uniformly distributed in the PVDF matrix.

[0070] Figure 7 The changes of pure water permeability (J) and flux recovery rate (FRR) of different types of mixed matrix membranes during five cycles are shown. Figure 7 (a) to (d), PCM-1 to PCM-4 membranes showed higher initial permeabilities. –2 h –1 bar -1 Starting from the beginning, gradually increasing to nearly 340L m of PCM-4 –2 h –1 bar -1 The flux recovery rate was roughly maintained above 91%, indicating that the membrane had excellent anti-fouling properties. With the increase of CNF-C loading, the permeability and FRR of the membrane showed a gradual improvement trend from PCM-1 to PCM-4, indicating that increasing the content of CNF-C can effectively improve the performance of the membrane. Figure 7 (e) to (i), the TiPCM series membranes showed higher initial permeabilities from 350 L m-1 for TiPCM-1 to 450 L m-2 for TiPCM-1. –2 h –1 bar -1 Gradually increase to 400 L m of TiPCM-5 –2 h –1 bar -1 , FRR generally maintained above 94%, showing excellent anti-pollution and stability. In particular, the initial permeability of TiPCM-4 reached 410L m –2 h –1 bar -1 , and the permeability and FRR hardly decreased significantly, indicating that the structure and function of the membrane were significantly enhanced under high MIL-125(Ti) loading. Overall, the performance of the membrane was significantly improved with the increase of MIL-125(Ti) content. Especially under high loading conditions (TiPCM-3 to TiPCM-5), the membrane not only showed high water permeability, but also maintained high flux recovery rate after multiple cycle tests, indicating that these membranes have good fouling resistance and stability.

[0071] Figure 8The dynamic water contact angle (WCA) of the mixed matrix membrane with CNF-C and MIL-125(Ti) loading. As the MIL-125(Ti) loading gradually increased, a significant WCA decrease trend was observed. When the MIL-125(Ti) loading increased to 8wt%, the prepared MMMs surface showed the best hydrophilicity. The WCA dropped from 54.1° to 28.6° in just 30 seconds. This is mainly attributed to the fact that the introduction of hydrophilic MIL-125(Ti) nanoparticles significantly increased the surface hydrophilicity of TiPCM, and the introduction of CNF-C improved the wettability of TiPCM, which is conducive to the penetration of water molecules. This phenomenon highlights the important role of porous MOF materials and CNF-C in separation membranes, which can not only adjust the surface properties, but also improve the wetting properties of the membrane and increase its hydrophilicity. By optimizing the hydrophilicity of the membrane surface, it is expected to achieve higher water flux and longer membrane service life, while reducing the contamination of the membrane surface and the clogging of the pores by pollutants.

[0072] Fig. 9 The performance of PVDF / MIL-125(Ti) / CNF-C mixed matrix membranes in terms of dye and metal ion removal performance and water permeability was demonstrated. With the increase of MIL-125(Ti) loading, the organic dye rejection rate and permeation flux of TiPCMs were significantly improved. In particular, the permeation flux of TiPCMs-4 in treating methylene blue (MB) reached 233.7 L·m -2 ·h -1 bar -1 , and the interception rate of MB reached 97.83%.

[0073] Fig.10 The permeation flux and retention rate of the dye on the surface of TiPCMs-4 after three cycles under natural light are shown. The study found that the permeation flux of TiPCM-4 for methylene blue (MB) gradually decreased during use, which was mainly due to the accumulation of MB in the pores on the surface of TiPCM-4, forming a hydration layer, which affected the permeation flux. However, after the membrane was exposed to natural light for 2 hours, its permeation flux and retention rate for MB were measured again, and it was found that the permeation flux of the membrane was almost completely restored to its initial state. This shows that MB on the membrane surface and in the pores has been effectively photocatalytically degraded.

[0074] In addition, through three cycles of rejection and photodegradation experiments, MB was successfully degraded, and the permeation flux and retention rate of TiPCMs-4 were almost restored to the original level. This recovery was mainly due to the addition of CNF-C, which improved the wetting properties of the PVDF membrane, while the photocatalytic activity of MIL-125(Ti) gave the mixed matrix membrane excellent self-cleaning ability. The results showed that the color on the surface of TiPCMs-4 was almost completely removed by photodegradation, such as Fig.11 This not only demonstrates the high efficiency of TiPCM-4 in water treatment applications, but also highlights its ability to maintain high performance in continuous operation.

[0075] Fig.12 The potential mechanism of the self-cleaning of organic pollutants by PVDF / MIL-125(Ti) / CNF-C mixed matrix membrane was revealed. Under the irradiation of natural light, when the energy of the photon exceeds the band gap of MIL-125(Ti), MIL-125(Ti) is excited to produce electrons and holes. These electrons are excited to the lowest unoccupied orbital of the conduction band, while the holes remain in the highest occupied orbital of the valence band, thereby achieving effective separation of electrons and holes. These separated electrons and holes migrate to the surface of MIL-125(Ti), promoting the generation of hydroxyl radicals, which have strong oxidizing properties and can effectively catalyze the photodegradation of organic dyes such as MB, thereby removing organic pollutants attached to the membrane surface. This process not only cleans the membrane material, but also restores its permeability, demonstrating the self-cleaning function and high efficiency of PVDF / MIL-125(Ti) / CNF-C mixed matrix membrane in water treatment.

[0076] The embodiments are preferred implementations of the present invention, but the present invention is not limited to the above-mentioned implementations. Any obvious improvements, substitutions or modifications that can be made by those skilled in the art without departing from the essential content of the present invention belong to the protection scope of the present invention.

Claims

1. A method for preparing a green, environmentally friendly, efficient, self-cleaning photocatalytic mixed matrix membrane, characterized in that: The following steps are involved: (1) Synthesis of MIL-125(Ti): dissolving a carboxylic acid ligand in an organic solvent A to form a uniform mixed solution; then, adding a titanium salt to the mixed solution, and adding methanol, mixing, and performing a hydrothermal reaction in a reactor. After the reaction is completed, centrifugation and vacuum drying are performed to obtain MIL-125(Ti) crystals; (2) Preparation of mixed matrix membrane: The MIL-125 (Ti) crystals, carboxylated nanofibers (CNF-C), and polyvinyl pyrrolidone (PVP) synthesized in step (1) are placed in an organic solvent B for ultrasonic dissolution, and then polyvinylidene fluoride (PVDF) is added, and heated and stirred to form a homogeneous casting solution; the casting solution is coated on a coating machine, and the coated membrane is placed in deionized water for 8 to 12 hours for phase separation, and finally vacuum dried to obtain a high-efficiency self-cleaning photocatalytic mixed matrix membrane.

2. The method for preparing a green, environmentally friendly, efficient, self-cleaning photocatalytic mixed matrix membrane according to claim 1, characterized in that: The carboxylic acid ligand in step (1) is any one or more of terephthalic acid, 2,6-naphthalene dicarboxylic acid, and tetraphenyl dicarboxylic acid, the organic solvent A is one or more of N,N-dimethylformamide, cyclohexane, and trichloroethylene, and the titanium salt is tetrabutyl titanate.

3. The method for preparing a green, environmentally friendly, efficient and self-cleaning photocatalytic mixed matrix membrane according to claim 1, characterized in that: The amount of titanium salt added is 1-2 mL, the amount of methanol added is 5-10 mL, and the amount of organic solvent added is 30-50 mL.

4. The method for preparing a green, environmentally friendly, efficient and self-cleaning photocatalytic mixed matrix membrane according to claim 1, characterized in that: The temperature of the hydrothermal reaction in step (1) is 150-180° C., the reaction time is 16-24 hours, the centrifugal speed is 8000-10000 rpm, the centrifugal time is 8-10 minutes / time, a total of 2-4 times, and the drying condition is vacuum drying at 70-80° C. for 10-12 hours.

5. The method for preparing a green, environmentally friendly, efficient and self-cleaning photocatalytic mixed matrix membrane according to claim 1, characterized in that: In step (2), the organic solvent B is one or more of N-methylpyrrolidone, styrene, and n-hexane, and the mass fraction of the solute is 16-30%, wherein the mass fraction of the carboxylated nanofibers (CNF-C) is 1-5%.

6. The method for preparing a green, environmentally friendly, efficient and self-cleaning photocatalytic mixed matrix membrane according to claim 1, characterized in that: In the step (2), the weight ratio of MIL-125 (Ti) crystal, carboxylated nanofiber (CNF-C), polyvinyl pyrrolidone (PVP), and polyvinylidene fluoride (PVDF) is 2-8:1-4:0.5:

15.

7. The method for preparing a green, environmentally friendly, efficient and self-cleaning photocatalytic mixed matrix membrane according to claim 1, characterized in that: The coating process parameters in step (2) are: advancing speed is 5 mm / s, and sedimentation time in water is 8 to 12 hours.

8. The method for preparing a green, environmentally friendly, efficient and self-cleaning photocatalytic mixed matrix membrane according to claim 1, characterized in that: The vacuum drying condition in step (2) is 70-80° C. and the drying time is 2-4 hours.

9. A highly efficient self-cleaning photocatalytic mixed matrix membrane prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The mixed matrix membrane is mainly composed of MIL-125 (Ti), carboxylated nanofibers (CNF-C), polyvinyl pyrrolidone (PVP) and polyvinylidene fluoride (PVDF). The weight fractions of MIL-125 (Ti) crystals, carboxylated nanofibers (CNF-C), polyvinyl pyrrolidone (PVP) and polyvinylidene fluoride (PVDF) are 2 to 8:1 to 4:0.5:

15. The mixed matrix membrane has a finger-like pore structure with a diameter of micrometers in the thickness direction of the membrane.

10. The high-efficiency self-cleaning photocatalytic mixed matrix membrane according to claim 9, characterized in that: The specific surface area of ​​the mixed matrix membrane is not less than 276.24 m 2 / g.

11. Use of the highly efficient self-cleaning photocatalytic mixed matrix membrane according to claim 9 for water treatment.

Citation Information

Patent Citations

  • Polyvinylidene fluoride-based nano composite ultrafiltration membrane and preparation method thereof

    CN112206661A

  • Nanoparticle modified PVDF (Polyvinylidene Fluoride) ultrafiltration membrane composite material as well as preparation method and application thereof

    CN114950160A

  • PVDF photocatalytic self-cleaning film containing Z-type 2D / 3D heterojunction as well as preparation method and application of PVDF photocatalytic self-cleaning film