Calendering process for producing gold bonding belt
By optimizing the rolling process for bonded alloy strip production, the problems of low equipment efficiency and poor heat dissipation were solved, achieving high-precision, high-efficiency large-scale production and improved heat dissipation performance.
Patent Information
- Application Number
- CN202411131304.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-17
- Publication Date
- 2024-11-08
AI Technical Summary
Existing bonded alloy strip production equipment is inefficient, time-consuming to adjust dimensions, has a low yield, and its smooth surface has poor heat dissipation, making it difficult to scale up production.
The production rolling process of the bonded alloy strip is optimized, including surface cleaning, annealing, mechanical property testing, and five consecutive rolling passes. By adjusting the rolling reduction rate and take-up speed, patterns are finally pressed onto the surface of the gold wire to improve heat dissipation.
It improves the dimensional accuracy and yield of the bonding alloy strip, reduces production costs, enables efficient large-scale production, and enhances heat dissipation performance.
Smart Images

Figure BDA0004997927030000031
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of bonding materials, and in particular to a calendering process for producing bonding gold strips. Background Art
[0002] Currently, gold bonding ribbon is an important electronic material, mainly used for interconnection in semiconductor packaging. It has excellent electrical conductivity, thermal conductivity, corrosion resistance and stability. It is often used in high-frequency microwave / RF and high-power applications. Especially when it is incompatible with materials such as aluminum or copper, gold ribbon becomes the preferred bonding material. Its fusing current is higher than that of standard gold bonding wire, providing higher reliability.
[0003] At present, there are few special rolling equipment for bonding gold strips. The market mostly uses round busbars to be rolled into bonding gold strips. During the rolling and debugging process, a lot of time is consumed to debug the equipment rolling thickness and width. The machine needs to stop to detect the strip size specifications when rolling a 100m long finished strip, and the round busbar size requirements are extremely high. In the production of bonding gold strips, production efficiency and yield rate will be reduced, making it difficult to mass produce on a large scale. The traditionally produced bonding gold strips are mirror gold strips with a smooth surface and no patterns. However, after packaging, the existing RF components require another rolling process because the heat dissipation effect of the smooth surface of the gold strip is not as good as that of the surface with patterns. Summary of the invention
[0004] The purpose of the present invention is to provide a calendering process for producing a bonded gold strip in view of the deficiencies in the prior art.
[0005] The purpose of the present invention is achieved by following steps:
[0006] a. Clean the surface of the gold wire rolling busbar with a diameter error of ±0.0005mm and a surface finish of Ra0.002um;
[0007] b. Annealing the gold wire rolled busbar;
[0008] c. Test the mechanical properties of the gold wire rolled busbar and select qualified gold wire rolled busbar;
[0009] d. The selected gold wire rolling mother bar is rolled five times continuously, the first rolling reduction rate is in the range of 30% to 60%, the second, third and fourth rolling reduction rates are in the range of 10% to 40%, the fifth rolling reduction rate is 10% to 20%, and the wire taking-up speed is 1 to 3 m / s.
[0010] In a preferred embodiment, the annealing temperature in step b is 240-600° C., the annealing speed is 0.5-2.5 m / s, the qualified inspection standard in step c is a tensile speed of 10 mm / min and a wire elongation of 5%-15%, and a pattern is embossed on the surface of the gold wire during the fifth rolling in step d.
[0011] Compared with the prior art, the present invention has the following obvious advantages: the present invention optimizes the rolling method of the bonding gold strip, improves the product dimensional accuracy, the width tolerance is ±0.5%, and the thickness tolerance is ±0.0001㎜, which greatly reduces the production cost. The five pairs of rollers cooperate with each other in the amount of reduction so that the bonding gold strip is no longer limited by the high precision of the busbar, and the overall product output has higher dimensional accuracy. The last roller has a positive pattern, and the wire surface has a heat dissipation effect, which does not affect the mechanical properties of the bonding gold strip and meets the bonding requirements. DETAILED DESCRIPTION
[0012] Example 1
[0013] A target size of a bonding gold ribbon is: 1.5000㎜(width)×0.0250㎜(thickness).
[0014] (1) Use gold wire with a diameter of 0.3211 mm as the rolled master wire, the wire diameter tolerance is ±0.0005 mm, and the surface finish is Ra0.002 um; the product surface should be clean, free of fingerprints, attachments and other contaminants; there should be no obvious defects exceeding the allowable deviation of its width, such as scratches and streaks; use a four-wire horizontal infrared baking annealing furnace to anneal the gold wire, and use linear annealing to eliminate stress; the annealing temperature is 600 ° C, and the annealing speed is 0.5 m / s.
[0015] (2) The annealed wire is subjected to an elongation test of the mechanical properties of the wire using a universal material tensile testing instrument; the elongation of the wire is 15%, and the tensile speed during the test is 10 mm / min.
[0016] (3) The wire is rolled five times continuously to be processed into a gold strip of target size, with a width tolerance of ±0.5% and a thickness tolerance of ±0.0001 mm; the specific operation is to place the gold wire on the pay-off end of the precision rolling mill, automatically pay off the wire, and manually guide the gold wire through the first, second, third, fourth, and fifth rollers and the tension wheel and the guide wheel. After the manual wire guiding is completed, the wire is fixed on the take-up wheel of the take-up part; the rolling program is written on the rolling mill, the gap between the first pair of rollers is 0.1284 mm, the pressing rate is 60%, the gap between the second pair of rollers is 0.0771 mm, the pressing rate is 40%, the gap between the third pair of rollers is 0.0462 mm, the pressing rate is 40%, the gap between the fourth pair of rollers is 0.0277 mm, the pressing rate is 40%, and the gap between the fifth pair of rollers is 0.0250 mm, the pressing rate is 10%. After all settings are completed, check whether the strip is stable on the guide wheel. After checking that the strip is on the guide wheel, start the machine and roll it for 3m before removing it to check the strip width and thickness. The measurement uses a contact interferometer. After confirming that the gold strip size is within the tolerance range, continue processing. If it exceeds the range, adjust the rolling mill program parameters until a qualified gold strip is rolled out. After rolling, the finished gold strip is harvested.
[0017] Example 2
[0018] The target size of a bonding metal ribbon is: 0.0500 mm (width) × 0.0125 mm (thickness):
[0019] (1) Use gold wire with a diameter of 0.0273 mm as the rolled master wire, with a wire diameter tolerance of ±0.0005 mm and a surface finish of Ra0.002 um; the product surface should be clean, free of fingerprints, attachments and other contaminants; there should be no obvious defects exceeding the allowable deviation of its width, such as scratches and streaks; use a four-wire horizontal infrared baking annealing furnace to anneal the gold wire, and use linear annealing to eliminate stress; the annealing temperature is 240 ° C, and the annealing speed is 2m / s.
[0020] (2) The annealed wire is subjected to an elongation test of the mechanical properties of the wire using a universal material tensile testing instrument; the elongation of the wire is 5%, and the tensile speed during the test is 10 mm / min.
[0021] (3) The wire is rolled five times continuously to be processed into a gold strip of target size, with a width tolerance of ±0.5% and a thickness tolerance of ±0.0001 mm; the specific operation is to place the gold wire on the pay-off end of the precision rolling mill, automatically pay off the wire, and manually guide the gold wire through the first, second, third, fourth, and fifth rollers and the tension wheel and the guide wheel. After the manual wire guiding is completed, the wire is fixed on the take-up wheel of the take-up part; the rolling program is written on the rolling mill, the gap between the first pair of rollers is 0.0191 mm, the pressing rate is 30%, the gap between the second pair of rollers is 0.0172 mm, the pressing rate is 10%, the gap between the third pair of rollers is 0.0155 mm, the pressing rate is 10%, the gap between the fourth pair of rollers is 0.0139 mm, the pressing rate is 10%, and the gap between the fifth pair of rollers is 0.0125 mm, the pressing rate is 10%. After all settings are completed, check whether the strip is stable on the guide wheel. After checking that the strip is on the guide wheel, start the machine and roll it for 3m before removing it to check the strip width and thickness. The measurement uses a contact interferometer. After confirming that the gold strip size is within the tolerance range, continue processing. If it exceeds the range, adjust the rolling mill program parameters until a qualified gold strip is rolled out. After rolling, the finished gold strip is harvested.
[0022] Quality Inspection
[0023] 1. Gold belt surface quality inspection:
[0024] With reference to Appendix B of GB / T 8750-2022, the bonded gold ribbons prepared in Examples 1 and 2 were directly observed and inspected using a microscope.
[0025] Index requirements: The product surface should be clean, free of fingerprints, attachments and other contaminants; there should be no obvious defects that exceed the allowable deviation of its width, such as scratches and streaks.
[0026] Test results: The bonded gold strips of Examples 1 and 2 both meet the index requirements.
[0027] 2. Distortion detection:
[0028] Referring to Appendix H of GB / T 8750-2022, the bonding gold ribbons prepared in Examples 1 and 2 were lowered vertically from the spool for 1 m and visually observed for defects such as twisting.
[0029] Index requirements: The gold belt should not have obvious curling when it is freely dropped from the axis. The gold belt is allowed to have slight curling without reducing its use function; the gold belt should not be twisted.
[0030] Test results: The bonded gold strips of Examples 1 and 2 both meet the index requirements.
[0031] 3. Dimensions:
[0032] With reference to Appendix E of GB / T 8750-2022, the bonded gold ribbons prepared in Examples 1 and 2 were observed and inspected using an image measuring instrument.
[0033]
Claims
1. The bonding metal strip production rolling process is characterized by: a. Clean the surface of the gold wire rolling busbar with a diameter error of ±0.0005mm and a surface finish of Ra0.002um; b. Annealing the gold wire rolled busbar; c. Test the mechanical properties of the gold wire rolled busbar and select qualified gold wire rolled busbar; d. The selected gold wire rolling mother bar is rolled five times continuously, the first rolling reduction rate is in the range of 30% to 60%, the second, third and fourth rolling reduction rates are in the range of 10% to 40%, the fifth rolling reduction rate is 10% to 20%, and the wire taking-up speed is 1 to 3 m / s.
2. The calendering process for producing a bonded gold strip according to claim 1, characterized in that: In step b, the annealing temperature is 240-600° C., and the annealing speed is 0.5-2.5 m / s.
3. The calendering process for producing a bonded gold strip according to claim 1, characterized in that: The qualified standard of the test in step c is that the stretching speed is 10 mm / min and the wire elongation is 5% to 15%.
4. The calendering process for producing a bonded gold strip according to claim 1, characterized in that: During the fifth rolling in step d, a pattern is embossed on the surface of the gold wire.
Citation Information
Patent Citations
Method for calendering pure copper foil
CN101209457A
Forming method of high-flexibility ultrathin rolled copper foil
CN102716908A
Heat dissipation material for mobile phones and processing technology thereof
CN112706478A
High-strength bonding alloy belt and preparation method thereof
CN115029578A