Casting process for reducing casting defects of nodular iron casting by reducing materials and iron casting

By using internally cooled iron and specific spheroidizers in the manufacturing of ductile cast iron, the defects of cast iron parts caused by the riser are solved, the yield and material performance are improved, and more uniform cooling and higher processing pass rate are achieved.

CN118905174APending Publication Date: 2024-11-08CANGZHOU YONGXIN CASTING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410958637.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the manufacturing process of ductile cast iron, the use of risers can easily lead to defects in the processing of cast iron parts, which reduces the process yield rate and increases production costs, and has a high scrap rate.

Method used

By setting up internally cooled iron instead of the riser, the temperature of cold iron absorbs the iron, the cooling speed of cast iron parts is accelerated, and the uniformity of cooling speed is improved. Combined with the use of lanthanide rare earth composite spheroidizer and silicon barium inoculant, the spheroidization is controlled. Reaction and incubation treatment, reduce slag inclusion defects, and optimize casting speed and temperature control.

Benefits of technology

Effectively eliminate shrinkage holes and shrinkage defects, improve the yield and iron utilization rate of cast iron parts, and significantly improve the processing pass rate and the comprehensive performance of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905174A_ABST
    Figure CN118905174A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of casting, in particular to a casting process for reducing casting defects of a nodular iron casting through material reduction and the iron casting. The cold iron is subjected to shot blasting cleaning and drying, the dried cold iron is placed in a sand shell, a sand mold is obtained, and the manufactured sand mold is subjected to mold drying treatment; smelting molten iron and removing slag; spheroidizing and inoculating the molten iron; casting to obtain an iron casting crude product; and after the iron casting crude product is cooled to the room temperature, the sand mold is dismantled, sand grains on the surface of the casting are cleaned, and the iron casting is obtained. According to the casting process for reducing the casting defects of the nodular iron casting by reducing the materials and the iron casting, the defects of the nodular iron casting are eliminated by increasing and reducing the materials, the yield of the iron casting and the utilization rate of molten iron are improved, and the problem of high rejection rate in the prior art is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of casting, and in particular to a casting process and a cast iron part for reducing casting defects of ductile iron parts by reducing material. Background Art

[0002] Cast iron, as an iron-carbon alloy, has a carbon content greater than 2.11%. It is obtained by melting industrial pig iron, scrap steel and other steel and alloy materials at high temperatures and casting. In addition, the carbon in cast iron is also precipitated in other forms. If the precipitated graphite is in the form of strips, it is called gray cast iron or gray cast iron, if it is in the form of worms, it is called vermicular cast iron, and if it is in the form of balls, it is called ductile cast iron. Ductile cast iron is a high-strength cast iron material. Spheroidal graphite is obtained by spheroidization, making its comprehensive properties close to those of steel, effectively improving the mechanical properties of cast iron, and can be used to cast parts with complex forces and high requirements for strength, toughness and wear resistance.

[0003] In the manufacturing process of ductile iron, the molten metal liquid is poured into the mold, and the parts with the required shape and performance are obtained after cooling and solidification. The manufacturing cost is low, the process flexibility is large, and complex shapes and large cast iron parts can be obtained. Casting mainly includes: metal smelting, model making, pouring solidification and demoulding cleaning. In the process of model making, risers are usually set on the mold cavity of the model to store liquid metal, and supply metal when the cast iron parts are formed. It has the function of preventing shrinkage cavities, shrinkage, exhaust and slag collection. The main function of the riser is to compensate for shrinkage, but the use of risers can also easily cause defects in cast iron parts during processing, reducing the process yield, increasing production costs, and reducing the overall benefits of the foundry. Summary of the invention

[0004] The purpose of the present invention is to provide a casting process and a cast iron part that utilizes material reduction to reduce the casting defects of ductile iron castings. The defects of ductile iron castings are eliminated by increasing the material reduction method, thereby improving the finished product rate and molten iron utilization rate of the cast iron parts, and solving the problem of high scrap rate in the prior art.

[0005] To achieve the above object, the present invention provides a casting process for reducing casting defects of ductile iron castings by reducing material, comprising the following steps:

[0006] S1. Making a sand shell according to the shape and size of the cast iron part to be cast;

[0007] S2, shot blasting and drying the cold iron, placing the dried cold iron in a sand shell to obtain a sand mold, and baking the prepared sand mold;

[0008] S3, adding QT450-10 ductile iron into a medium frequency smelting furnace to obtain molten iron and remove slag, the smelting temperature is 1530-1550°C;

[0009] S4, spheroidizing agent, 1 / 3-1 / 2 of inoculant, and covering agent are sequentially spread in the detonation area of ​​the spheroidizing treatment bag, molten iron is poured into the spheroidizing treatment bag for spheroidizing treatment, the remaining inoculant is spread in the flat bottom bag, and the molten iron after the spheroidizing treatment is poured into the flat bottom bag for internal inoculation treatment;

[0010] S5, preheating the ladle to 750-850°C, transferring the molten iron after the inoculation treatment into the preheated ladle, and pouring the molten iron into the sand mold when the temperature of the molten iron is 1370-1420°C to obtain a rough iron casting;

[0011] S6. Separate the casting from the sand mold, cool the rough iron casting to room temperature, and clean the sand on the surface of the casting to obtain the iron casting.

[0012] The present invention controls the molten iron within the above temperature range before pouring, thereby preventing the temperature from being too high, reducing the cooling effect of the cold iron, and still causing shrinkage defects. If the temperature is too low, the casting will have cold shut defects.

[0013] Preferably, the baking treatment in S2 is to bake the sand core with a hot air blower for ≥ 8 hours, so that the temperature of the sand core reaches 80-100°C.

[0014] Preferably, two modules are provided on the sand mold in S2, each module is provided with a gate that semi-surrounds the cast iron part, a sand core is provided in the middle of the upper top of the module, and a chiller is arranged on one side of the sand core.

[0015] Preferably, the chiller in S2 is an inner chiller, the shape of the chiller is cylindrical, the diameter of the chiller is 10 mm, and the height is 30 mm.

[0016] In the present invention, the diameter of the chill is controlled to be 10 mm to prevent the chill from being too large, which affects the processing accuracy. If the chill is too small, it will not work. If the chill is pre-buried too shallowly, the effect is not ideal. If the chill is pre-buried too deeply, it will be difficult to demould.

[0017] Preferably, the S4 spheroidizer is a lanthanide rare earth composite spheroidizer, and the inoculant is a silicon-barium inoculant.

[0018] The invention uses silicon-barium inoculant to improve the tensile strength and elongation after fracture of ductile iron, so that the obtained cast iron part has better comprehensive performance.

[0019] Preferably, the lanthanide rare earth composite spheroidizer includes the following components: magnesium, iron, calcium, aluminum, and lanthanide elements.

[0020] The lanthanide rare earth composite spheroidizer used in the present invention has the characteristics of purifying molten iron, stabilizing spheroidization, resisting recession and resisting graphite distortion, and further improving the comprehensive mechanical properties of cast iron parts.

[0021] Preferably, during the spheroidization treatment in S4, the spheroidizer, 1 / 3-1 / 2 of the inoculant, and the covering agent are divided into three equal parts, and each part is spread on the bottom layer in the order of spheroidizer, inoculant, and covering agent, and each layer is smoothed with a tamping tool.

[0022] The present invention divides the spheroidizing agent, the inoculant and the covering agent into three equal parts and lays them in layers, thereby achieving accurate quantification of the spheroidizing agent, the inoculant and the covering agent, which can greatly improve the spheroidizing reaction effect of molten iron, improve the absorption rate of Mg, significantly reduce the amount of spheroidizing agent added, reduce the amount of smoke from the on-site spheroidizing reaction, improve the purity of molten iron, and reduce slag inclusion casting defects.

[0023] Preferably, the pouring in S5 is to quickly pour the molten iron into the sand mold, and the molten iron completes the filling of the mold by its own gravity, the pouring speed is controlled between 2.0 and 2.5 kg / s, and the pouring time is controlled between 40 and 50 seconds.

[0024] The present invention controls the pouring speed and the pouring time within the above range, so that the molten iron punching is more stable.

[0025] Preferably, the cooling in S6 is to keep the cast part in the sand mold for 4 hours, then shake out the sand and separate it, and cool it to room temperature in air.

[0026] The above-mentioned cast iron part is made by a casting process that utilizes material reduction to reduce casting defects of ductile iron parts, and includes a lower chassis, an upper boss and a cavity chamber, wherein the cavity chamber is located between the lower chassis and the upper boss, and the lower chassis is provided with a plurality of evenly distributed mounting holes, and the circumferential outer side of the upper boss is provided with a plurality of evenly distributed protrusions, and the outer side wall of the cavity chamber is provided with a plurality of supporting ribs, and the top of the supporting plate ribs extends to the upper boss and is connected to the protrusion as a whole, and the cold iron is located at the top of the protrusion.

[0027] Beneficial effects of the present invention:

[0028] The present invention provides a casting process for reducing the casting defects of ductile iron castings by reducing materials. The castings are processed by arranging an internal chiller instead of a riser, and the internal chiller absorbs the temperature of molten iron, thereby accelerating the cooling rate of the castings, improving the uniformity of the cooling rate of various parts of the castings, eliminating shrinkage cavities and shrinkage, improving the process yield, eliminating the processing defects of the castings, and thus improving the finished product rate of the castings and the utilization rate of molten iron.

[0029] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 is a schematic diagram of a sand mold in Example 1 of the present invention;

[0031] Figure 2is a schematic diagram of a cast iron part in Example 4 of the present invention;

[0032] Figure 3 It is a schematic diagram of the sand mold in Comparative Example 1 of the present invention.

[0033] Reference numerals:

[0034] 1. Sand mold; 2. Module; 3. Gate; 4. Sand core; 5. Chill; 6. Riser; 7. Lower chassis; 8. Upper boss; 9. Cavity; 10. Mounting hole; 11. Boss; 12. Support rib. DETAILED DESCRIPTION

[0035] The present invention is further described below in conjunction with the accompanying drawings and embodiments. Unless otherwise defined, the technical terms or scientific terms used in the present invention should be the common meanings understood by people with ordinary skills in the field to which the present invention belongs. The above-mentioned features or features mentioned in the specific examples mentioned in the present invention can be combined arbitrarily, and these specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0036] Example 1

[0037] Figure 1 Schematic diagram of the sand mold in Example 1 of the present invention, Figure 1 As shown, the present invention provides a casting process for reducing casting defects of ductile iron castings by reducing material, comprising the following steps:

[0038] S1. Make a sand shell according to the shape and size of the cast iron part to be cast.

[0039] S2. Shot blast and dry the cold iron 5, place the dried cold iron 5 in a sand shell to obtain a sand mold 1, and bake the sand shell cavity of the prepared sand mold 1 with a hot air blower for ≥8 hours to make the cavity temperature reach 80°C.

[0040] Two modules 2 are arranged on the sand mold 1, each module 2 is provided with a gate 3 which semi-surrounds the cast iron part, a sand core 4 is arranged in the middle of the upper top of the module 2, and a chill 5 is arranged on one side of the sand core 4. The chill 5 is an inner chill 5, and the shape of the chill 5 is cylindrical, and the diameter of the chill 5 is 10 mm and the height is 30 mm.

[0041] S3. Add QT450-10 ductile iron into a medium frequency smelting furnace to obtain molten iron and remove slag. The smelting temperature is 1530°C.

[0042] S4, divide the lanthanide rare earth composite spheroidizer, 1 / 2 of the silicon-barium inoculant, and the covering agent into three equal parts, and spread each part on the bottom layer of the blasting area of ​​the spheroidizing treatment bag in the order of the lanthanide rare earth composite spheroidizer, the silicon-barium inoculant, and the covering agent. After the first layer is laid, use a tamping tool to level it, and then lay the second layer. After the second layer is leveled with a tamping tool, lay the third layer. Pour the molten iron into the spheroidizing treatment bag for spheroidization treatment, lay the remaining inoculant in the flat-bottomed bag, and pour the molten iron after the spheroidization treatment into the flat-bottomed bag for internal inoculation treatment;

[0043] S5. Preheat the ladle to 750°C, transfer the molten iron after inoculation treatment to the preheated ladle, and when the molten iron temperature is 1370°C, quickly pour the molten iron into the sand mold 1. The molten iron completes the filling of the mold by its own gravity. The pouring speed is controlled between 2.0 and 2.5 kg / s, and the pouring time is controlled within 40 seconds to obtain a rough cast iron part.

[0044] S6. Keep the cast casting in the sand mold for 4 hours, then separate the sand by dropping out, cool it to room temperature in the air, and clean the sand on the surface of the casting to obtain the cast iron part.

[0045] Example 2

[0046] The present invention provides a casting process for reducing casting defects of ductile iron castings by reducing material, comprising the following steps:

[0047] S1. Make a sand shell according to the shape and size of the cast iron part to be cast.

[0048] S2. Shot blast and dry the cold iron 5, place the dried cold iron 5 in a sand shell to obtain a sand mold 1, and bake the sand shell cavity of the prepared sand mold 1 with a hot air blower for ≥8 hours to make the sand core temperature reach 90°C.

[0049] Two modules 2 are arranged on the sand mold 1, each module 2 is provided with a gate 3 which semi-surrounds the cast iron part, a sand core 4 is arranged in the middle of the upper top of the module 2, and a chill 5 is arranged on one side of the sand core 4. The chill 5 is an inner chill 5, and the shape of the chill 5 is cylindrical, and the diameter of the chill 5 is 10 mm and the height is 30 mm.

[0050] S3. Add QT450-10 ductile iron into a medium frequency smelting furnace to obtain molten iron and remove slag. The smelting temperature is 1540°C.

[0051] S4, divide the lanthanide rare earth composite spheroidizer, 1 / 2 of the silicon-barium inoculant, and the covering agent into three equal parts, and spread each part on the bottom layer of the blasting area of ​​the spheroidizing treatment bag in the order of the lanthanide rare earth composite spheroidizer, the silicon-barium inoculant, and the covering agent. After the first layer is laid, use a tamping tool to level it, and then lay the second layer. After the second layer is leveled with a tamping tool, lay the third layer. Pour the molten iron into the spheroidizing treatment bag for spheroidization treatment, lay the remaining inoculant in the flat-bottomed bag, and pour the molten iron after the spheroidization treatment into the flat-bottomed bag for internal inoculation treatment;

[0052] S5. Preheat the ladle to 800°C, transfer the molten iron after inoculation treatment to the preheated ladle, and when the molten iron temperature is 1400°C, quickly pour the molten iron into the sand mold 1. The molten iron completes the filling of the sand mold by its own gravity. The pouring speed is controlled between 2.0 and 2.5 kg / s, and the pouring time is controlled within 50 s to obtain a rough cast iron part.

[0053] S6. Keep the cast casting in the sand mold for 4 hours, then separate the sand by dropping out, cool it to room temperature in the air, and clean the sand on the surface of the casting to obtain the cast iron part.

[0054] Example 3

[0055] The present invention provides a casting process for reducing casting defects of ductile iron castings by reducing material, comprising the following steps:

[0056] S1. Make a sand shell according to the shape and size of the cast iron part to be cast.

[0057] S2. Shot blast and dry the cold iron 5, place the dried cold iron 5 in a sand shell to obtain a sand mold 1, and bake the sand shell cavity of the prepared sand mold 1 with a hot air blower for ≥8 hours to make the cavity temperature reach 100°C.

[0058] Two modules 2 are arranged on the sand mold 1, each module 2 is provided with a gate 3 which semi-surrounds the cast iron part, a sand core 4 is arranged in the middle of the upper top of the module 2, and a chill 5 is arranged on one side of the sand core 4. The chill 5 is an inner chill 5, and the shape of the chill 5 is cylindrical, and the diameter of the chill 5 is 10 mm and the height is 30 mm.

[0059] S3. Add QT450-10 ductile iron into a medium frequency smelting furnace to obtain molten iron and remove slag. The smelting temperature is 1550°C.

[0060] S4, divide the lanthanide rare earth composite spheroidizer, 1 / 2 of the silicon-barium inoculant, and the covering agent into three equal parts, and spread each part on the bottom layer of the blasting area of ​​the spheroidizing treatment bag in the order of the lanthanide rare earth composite spheroidizer, the silicon-barium inoculant, and the covering agent. After the first layer is laid, use a tamping tool to level it, and then lay the second layer. After the second layer is leveled with a tamping tool, lay the third layer. Pour the molten iron into the spheroidizing treatment bag for spheroidization treatment, lay the remaining inoculant in the flat-bottomed bag, and pour the molten iron after the spheroidization treatment into the flat-bottomed bag for internal inoculation treatment;

[0061] S5. Preheat the ladle to 850°C, transfer the molten iron after inoculation treatment to the preheated ladle, and when the molten iron temperature is 1420°C, quickly pour the molten iron into the sand mold 1. The molten iron completes the filling of the sand mold by its own gravity. The pouring speed is controlled between 2.0 and 2.5 kg / s, and the pouring time is 45 seconds to obtain a rough cast iron part.

[0062] S6. Keep the cast casting in the sand mold for 4 hours, then separate the sand by dropping out, cool it to room temperature in the air, and clean the sand on the surface of the casting to obtain the cast iron part.

[0063] Example 4

[0064] Figure 2 Schematic diagram of the cast iron part in Example 4 of the present invention, Figure 2 As shown, a cast iron part made by the casting process of reducing the casting defects of ductile iron parts by material reduction in Example 1 comprises a lower chassis 7, an upper boss 8 and a cavity 9, the cavity 9 is located between the lower chassis 7 and the upper boss 8, the lower chassis 7 is provided with a plurality of evenly distributed mounting holes 10, the outer side of the circumference of the upper boss 8 is provided with a plurality of evenly distributed protrusions 11, the outer side wall of the cavity 9 is provided with a plurality of supporting ribs 12, the top of the supporting ribs 12 extends to the upper boss 8 and is connected to the protrusion 11 as a whole, and the chill 5 is located at the top of the protrusion 11. After the cast iron part is cooled to room temperature, the inner chill 5 and the cast iron part are melted into an integrated structure, and the exposed part of the inner chill 5 is cut and then polished.

[0065] Comparative Example 1

[0066] Figure 3 Schematic diagram of the sand mold 1 in Comparative Example 1 of the present invention. As shown in the figure, a casting process of ductile iron castings comprises the following steps:

[0067] S1. Make a sand shell according to the shape and size of the cast iron part to be cast.

[0068] S2. A riser 6 is arranged on the top of the sand shell to obtain a sand mold 1, and the sand shell cavity of the prepared sand mold 1 is baked by a hot air blower for ≥ 8 hours to make the cavity temperature reach 80°C.

[0069] Two modules 2 are provided on the sand mold 1, each module 2 is provided with a gate 3 that semi-surrounds the cast iron part, a sand core 4 is provided in the middle of the upper top of the module 2, and risers 6 are evenly distributed on the outer side of the circumference of the sand core 4. The diameter of the riser 6 is 60 mm and the height is 30 mm.

[0070] S3. Add QT450-10 ductile iron into a medium frequency smelting furnace to obtain molten iron and remove slag. The smelting temperature is 1530°C.

[0071] S4, divide the lanthanide rare earth composite spheroidizer, 1 / 2 of the silicon-barium inoculant, and the covering agent into three equal parts, and spread each part on the bottom layer of the blasting area of ​​the spheroidizing treatment bag in the order of the lanthanide rare earth composite spheroidizer, the silicon-barium inoculant, and the covering agent. After the first layer is laid, use a tamping tool to level it, and then lay the second layer. After the second layer is leveled with a tamping tool, lay the third layer. Pour the molten iron into the spheroidizing treatment bag for spheroidization treatment, lay the remaining inoculant in the flat-bottomed bag, and pour the molten iron after the spheroidization treatment into the flat-bottomed bag for internal inoculation treatment;

[0072] S5. Preheat the ladle to 750°C, transfer the molten iron after inoculation treatment into the preheated ladle, and when the molten iron temperature reaches 1370°C, quickly pour the molten iron into the sand mold 1. The molten iron completes the filling of the mold by its own gravity. The pouring speed is controlled between 0.3m / s and the pouring time is controlled within 160s to obtain a rough cast iron part.

[0073] S6. Keep the cast casting in the sand mold for 4 hours, then separate the sand by dropping out, cool it to room temperature in the air, and clean the sand on the surface of the casting to obtain the cast iron.

[0074] The cast iron parts obtained in Examples 1-3 and Comparative Example 1 were machined, and 7 M16 thread holes were evenly drilled on the top of the cast iron parts (i.e., holes were drilled at the raised positions). The qualified rates of the products after drilling were compared, and the results are shown in Table 1.

[0075] Table 1 Processing qualification rate of iron castings of Examples 1-3 and Comparative Example 1

[0076] Processing qualification rate Example 1 Internal cooling iron 95% Example 2 Internal cooling iron 96% Example 3 Internal cooling iron 96% Comparative Example 1 Riser 70%

[0077] As can be seen from Table 1, the processing qualification rate of the cast iron parts obtained by the casting process of arranging the internal chiller instead of the riser in the present invention is significantly improved. This is because the internal chiller absorbs the temperature of the molten iron in the present invention, accelerates the cooling rate of the cast iron parts, improves the uniformity of the cooling rate of each part of the cast iron parts, eliminates shrinkage cavities and shrinkage, and improves the process yield.

[0078] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A casting process for reducing casting defects of ductile iron castings by reducing material, characterized in that: The following steps are involved: S1. Making a sand shell according to the shape and size of the cast iron part to be cast; S2, shot blasting and drying the cold iron, placing the dried cold iron in a sand shell to obtain a sand mold, and baking the prepared sand mold; S3, adding QT450-10 ductile iron into a medium frequency smelting furnace to obtain molten iron and remove slag, the smelting temperature is 1530-1550°C; S4, spheroidizing agent, 1 / 3-1 / 2 of inoculant, and covering agent are sequentially spread in the detonation area of ​​the spheroidizing treatment bag, molten iron is poured into the spheroidizing treatment bag for spheroidizing treatment, the remaining inoculant is spread in the flat bottom bag, and the molten iron after the spheroidizing treatment is poured into the flat bottom bag for internal inoculation treatment; S5, preheating the ladle to 750-850°C, transferring the molten iron after the inoculation treatment into the preheated ladle, and pouring the molten iron into the sand core mold when the temperature of the molten iron is 1370-1420°C to obtain a rough cast iron product; S6. Separate the casting from the sand mold, cool the rough iron casting to room temperature, and clean the sand on the surface of the casting to obtain the iron casting.

2. A casting process for reducing casting defects of ductile iron parts by reducing material according to claim 1, characterized in that: The mold baking treatment in S2 is to use a hot air blower to bake the sand mold for 8 hours or more, so that the temperature of the sand mold reaches 80-100°C.

3. A casting process for reducing casting defects of ductile iron parts by reducing material according to claim 1, characterized in that: The S2 medium sand mold is provided with two modules, each of which is provided with a gate that semi-surrounds the cast iron part, a sand core is provided in the middle of the upper top of the module, and a chiller is arranged on one side of the sand core.

4. A casting process for reducing casting defects of ductile iron parts by reducing material according to claim 1, characterized in that: The chiller in S2 is an inner chiller, the shape of the chiller is cylindrical, and the diameter of the chiller is 10 mm.

5. A casting process for reducing casting defects of ductile iron parts by reducing material according to claim 1, characterized in that: The spheroidizer in S4 is a lanthanide rare earth composite spheroidizer, and the inoculant is a silicon-barium inoculant.

6. A casting process for reducing casting defects of ductile iron parts by reducing material according to claim 5, characterized in that: The lanthanide rare earth composite spheroidizer includes the following components: magnesium, iron, calcium, aluminum, and lanthanide elements.

7. A casting process for reducing casting defects of ductile iron parts by reducing material according to claim 1, characterized in that: During the spheroidizing treatment in S4, the spheroidizing agent, 1 / 3-1 / 2 of the inoculant, and the covering agent are divided into three equal parts respectively, and each part is spread on the bottom layer in the order of spheroidizing agent, inoculant, and covering agent, and each layer is smoothed with a tamping tool.

8. The casting process for reducing casting defects of ductile iron parts by reducing material according to claim 1, characterized in that: The pouring in S5 is to quickly pour the molten iron into the sand mold. The molten iron completes the filling of the sand mold by its own gravity. The pouring speed is controlled between 2.0 and 2.5 kg / s, and the pouring time is controlled between 40 and 50 seconds.

9. A casting process for reducing casting defects of ductile iron parts by reducing material according to claim 1, characterized in that: The cooling in S6 is to keep the cast part in the sand mold for 4 hours, then separate the sand by falling out, and cool it to room temperature in the air.

10. A cast iron part produced by a casting process for reducing casting defects of ductile iron parts by reducing material as claimed in any one of claims 1 to 9, characterized in that: It includes a lower chassis, an upper boss and a cavity, the cavity is located between the lower chassis and the upper boss, the lower chassis is provided with a plurality of evenly distributed mounting holes, the circumferential outer side of the upper boss is provided with a plurality of evenly distributed protrusions, the outer side wall of the cavity is provided with a plurality of supporting ribs, the top of the supporting ribs extends to the upper boss and is connected with the protrusion as a whole, and the cold iron is located at the top of the protrusion.