Application of tussah silk fibroin in preparation of liquid metal nano-droplets, liquid metal nano-droplets and preparation method thereof
Through tussah silk fibroin as a dispersant and low-temperature ultrasonic treatment, stable liquid metal nanodroplets were prepared, solving the biocompatibility and stability of liquid metals in biological applications, and achieving efficient liquid metal nanodroplets Preparation, suitable for a variety of biological and electronic fields.
Patent Information
- Application Number
- CN202411010329.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
AI Technical Summary
Liquid metals have problems such as poor biocompatibility, unstable dispersion and low production efficiency in biological applications, and existing surfactants are difficult to meet the needs of biomedical and drug delivery fields.
Using tussah silk fibroin as the dispersant of liquid metal nano droplets, stable liquid metal nano droplets are prepared by low-temperature ultrasonic treatment, and the excellent biocompatibility and antioxidant ability of tussah silk fibroin ensures the dispersion of liquid metals and stability.
It has achieved high biocompatibility and good stability of liquid metal nanodroplets, suitable for bioengineering, drug delivery and flexible electronics, avoiding the oxidation and settlement of liquid metals, and improving production efficiency.
Smart Images

Figure CN118905231A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of biomaterial preparation, in particular to liquid metal droplets, a preparation method of liquid metal droplets and application of tussah silk fibroin in nano-preparation of liquid metal droplets. Background Art
[0002] Liquid metal is a metal or alloy that is liquid at room temperature and has the characteristics of deformability and low cytotoxicity. Liquid metal has excellent fluidity, high electrical conductivity and high thermal conductivity, and is increasingly widely used in flexible electronics, printed circuits, energy storage, sensing, etc., especially in the field of biomaterials. However, liquid metal also has obvious technical defects: high density and easy sedimentation; high surface tension and easy agglomeration; easy oxidation when exposed to water or air. These problems have become technical barriers to the further application and expansion of liquid metal.
[0003] In order to solve the technical problems existing in the properties of liquid metal, many researchers have tried to use various surfactants to study and prepare stable liquid metal nanodroplets. For example, the document Nanoscale, 2018, 10, 19871-19878 publicly records a method of using poly (1-octadecene-maleic anhydride) to prepare stable liquid metal droplets. However, most of these surfactants are various chemical substances with poor biocompatibility, making them difficult to apply to biomedicine, drug delivery and other fields; in addition, although these surfactants have good effects when dispersed, after being stored for a period of time, the liquid metal droplets precipitate and agglomerate seriously, making it difficult to maintain the particle size of the liquid metal droplets and the stability of the system.
[0004] Tussah silk fibroin is a natural protein with good biocompatibility. It and its degradation products are non-toxic to cells and the body, and will not or rarely cause inflammation and immune rejection reactions. It is widely used in food or cosmetic additives, but there are no reports on its role in the preparation of liquid metal dispersions. Summary of the invention
[0005] The purpose of the invention of this patent application is to solve the technical problems of poor biocompatibility, unstable dispersion and low production efficiency of existing liquid metal droplet products, and to provide an application of tussah silk fibroin to prepare liquid metal nanodroplets, liquid metal nanodroplets and their preparation method.
[0006] The application technology scheme of tussah silk fibroin for preparing metal nanodroplets provided in this patent application mainly includes:
[0007] The invention discloses an application of tussah silk fibroin to prepare liquid metal nano droplets. The tussah silk fibroin is used as a dispersant for preparing liquid metal nano droplets.
[0008] This patent application provides a technical solution for the preparation of liquid metal nanodroplets using tussah silk fibroin, and its main technical contents are:
[0009] A method for preparing liquid metal nanodroplets, the method steps comprising:
[0010] (1) Extracting tussah silk fibroin and preparing tussah silk fibroin aqueous solution;
[0011] (2) Add bulk liquid metal into the tussah silk fibroin aqueous solution and obtain liquid metal nanodroplets by low-temperature ultrasound.
[0012] Furthermore, the mass concentration of the tussah silk fibroin aqueous solution is 0.01wt% to 30wt%, preferably 0.1wt% to 10wt%.
[0013] Furthermore, the liquid metal is at least one of gallium, gallium-indium alloy, and gallium-indium-tin alloy, among which Ga70In30, Ga75In25, and Ga80In20 are preferred.
[0014] Furthermore, the mass ratio of the silk fibroin to the liquid metal is 1:(200-1), preferably 1:(20-1).
[0015] Furthermore, the pH value of the mixed solution of liquid metal and tussah silk fibroin water is 2-12, preferably 4-10.
[0016] Furthermore, in step (2), at a low temperature of -10 to 30°C, an ultrasonic power of 50 to 2000 W, and an ultrasonic time of ≥10 s; in order to further weaken the oxidation of the liquid metal droplets and to optimize energy consumption and time costs, it is preferred that: at a temperature of -5 to 5°C, an ultrasonic power of 300 to 1000 W, and an ultrasonic time of 5 to 120 min.
[0017] This patent application also provides a liquid metal nanodroplet obtained by the liquid metal nanodroplet preparation method.
[0018] The present patent application provides an application of tussah silk fibroin to prepare liquid metal nanodroplets, a technical solution for liquid metal nanodroplets and a preparation method thereof, wherein the silk fibroin is a natural protein, which itself and its degradation products are non-toxic to cells and organisms, and has excellent biocompatibility. The silk fibroin is selected as a dispersant for the preparation of liquid metal nanodroplets, which not only plays a role in dispersing liquid metal, but also protects the liquid metal nanodroplets from further oxidation, thereby solving the technical problems of difficult dispersion and poor stability in the existing preparation of liquid metal nanodroplets. The present technical solution uses non-toxic and harmless tussah silk fibroin as an aqueous dispersant for preparing liquid metal droplets. Compared with other liquid metal droplets that use chemical preparations or are dispersed in organic solvents, the present invention does not contain harmful substances and is a liquid metal nanodroplet that truly meets the requirements of biocompatibility, and can be widely used in bioengineering, drug delivery and release, flexible wearables, printed circuits, heat dissipation of electronic products and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 Schematic diagram of preparing liquid metal nanodroplets using tussah silk fibroin.
[0020] Figure 2a This is an optical photograph of liquid metal in water without any other treatment;
[0021] Figure 2b This is an optical photograph of liquid metal in water after ultrasonic treatment;
[0022] Figure 2c This is an optical photograph of ultrasound treatment using tussah silk fibroin as a dispersant.
[0023] Figure 3 This is a particle size distribution diagram of liquid metal nanodroplets obtained according to the preparation method of the present application, wherein the dot curve represents the initial particle size distribution state after preparation, and the square dot curve represents the particle size distribution state after standing for 15 days after preparation.
[0024] Figure 4 This is an electron microscope image of the liquid metal nanodroplets prepared in this application.
[0025] Figure 5 This is an electron microscope image of the liquid metal nanodroplets prepared in this application after being left to stand for 15 days. DETAILED DESCRIPTION
[0026] The technical contents of the present invention will be described in detail below through various embodiments, but the protection scope of the present invention is not limited to the embodiments.
[0027] Example 1
[0028] 1). Preparation of Tussah Silk Fibroin
[0029] (1) Cut tussah cocoon shells into pieces and immerse them in a 5 g / L sodium carbonate solution, heat and boil for 30 min, then wash them with deionized water, boil and wash them again, repeat three times until the tussah silk is degummed, and then dry them naturally. The mass ratio of tussah cocoon shells to sodium carbonate solution is preferably 1:50;
[0030] (2) The degummed tussah silk was dissolved in a 12 mol / L lithium thiocyanate solution to obtain a 5% by mass tussah silk fibroin solution, the tussah silk fibroin solution was placed in a 8000-14000 kDa dialysis bag, and the fibroin solution was dialyzed at 4°C for 72 h, and the precipitate was freeze-dried to obtain tussah silk fibroin.
[0031] 2). Preparation of liquid metal nanodroplets
[0032] Take 1g of tussah silk fibroin and dissolve it in deionized water to obtain a 1% tussah silk fibroin aqueous solution; dissolve 1g of liquid metal, in this embodiment, Ga 75 In 25 Add the tussah silk fibroin aqueous solution, adjust the solution pH to 5, and perform ultrasonic treatment for 30 minutes at an ambient temperature of 0° C. and a probe power of 300 W to obtain stable liquid metal nanodroplets.
[0033] Example 2
[0034] 1). The tussah silk fibroin used is prepared by the same method as in Example 1;
[0035] 2). Preparation of liquid metal nanodroplets
[0036] Take 2g of tussah silk fibroin and dissolve it in deionized water to obtain a 2% tussah silk fibroin aqueous solution; 75 In 25 Add it to the above-mentioned tussah silk fibroin aqueous solution, adjust the solution pH to 5, and perform ultrasonic treatment for 30 minutes at an ambient temperature of 0°C and a probe power of 300W to obtain stable liquid metal nanodroplets.
[0037] Example 3
[0038] The difference between this embodiment and embodiment 1 is that the pH of embodiment 1 is adjusted to 2.
[0039] Example 4
[0040] The difference between this embodiment and embodiment 1 is that the pH of embodiment 1 is adjusted to 9.
[0041] Example 5
[0042] The only difference between this embodiment and embodiment 1 is that the pH of embodiment 1 is adjusted to 12.
[0043] Example 6
[0044] The only difference between this embodiment and embodiment 4 is that the mass concentration of the tussah silk fibroin aqueous solution is 10%.
[0045] Example 7
[0046] The only difference between this embodiment and embodiment 1 is that the mass concentration of the tussah silk fibroin aqueous solution is 0.01%.
[0047] Example 8
[0048] The difference between this embodiment and embodiment 1 is that Ga 70 In 30 The liquid metal of Example 1 is replaced.
[0049] Example 9
[0050] The difference between this embodiment and embodiment 1 is that Ga 80 In 20 The liquid metal of Example 1 is replaced.
[0051] from Figure 3 and Figure 4 It can be seen that the liquid metal nanodroplets prepared using tussah silk fibroin as a dispersant generally have an initial particle size of 140nm. After standing for 15 days, the droplets still remain spherical, and the particle size only slightly increases to 190nm, and there is no obvious oxidation change, indicating that the preparation and dispersion application of liquid metal nanodroplets of tussah silk fibroin not only produces excellent dispersing effect, but also has excellent antioxidant capacity, which greatly improves the stability of the liquid metal nanodroplets.
[0052] Comparative Example 1
[0053] 1g Ga 75 In 25 Add to 100mL of deionized water, adjust the solution pH to 5, and ultrasonically treat for 30min at 0℃ ambient temperature and 300W probe power to obtain liquid metal nanodroplets. As shown in Figure 2, the liquid metal dispersion without adding dispersant is white and turbid, indicating that the liquid metal is not effectively dispersed. This application uses tussah silk fibroin as a dispersant for liquid metal nanodroplets, and the prepared droplets are in a uniform and stable dispersed state, that is, tussah silk fibroin plays an excellent dispersing role in the preparation of liquid metal nanodroplets.
[0054] In the above embodiments, the obtained liquid metal nanodroplets, including the combination of the mass concentration of the silk fibroin aqueous solution, the mass ratio of the tussah silk fibroin to the liquid metal, the pH value and the type of liquid metal specified in the present application, can achieve the following results: Figure 2c The status and Figure 3 , Figure 4 's effects, so I will not elaborate on them one by one.
Claims
1. Application of tussah silk fibroin in preparing liquid metal nanodroplets, It is characterized in that The tussah silk fibroin is used as a dispersant for preparing liquid metal nano droplets.
2. A method for preparing liquid metal nanodroplets using claim 1, It is characterized in that The method steps include: (1) Extracting tussah silk fibroin and preparing tussah silk fibroin aqueous solution; (2) Add bulk liquid metal into the tussah silk fibroin aqueous solution and obtain liquid metal nanodroplets by low-temperature ultrasound.
3. The method for preparing liquid metal nanodroplets according to claim 2, It is characterized in that The mass concentration of the tussah silk fibroin aqueous solution is 0.01wt% to 30wt%.
4. The method for preparing liquid metal nanodroplets according to claim 2, It is characterized in that The liquid metal is at least one of gallium, gallium-indium alloy, and gallium-indium-tin alloy.
5. The method for preparing liquid metal nanodroplets according to claim 2, It is characterized in that The mass ratio of the silk fibroin to the liquid metal is 1:(200-1).
6. The method for preparing liquid metal nanodroplets according to claim 5, It is characterized in that The mass ratio of the silk fibroin to the liquid metal is preferably 1:(20-1).
7. The method for preparing liquid metal nanodroplets according to claim 2, It is characterized in that The pH value of the mixed solution of liquid metal, tussah silk fibroin and water is 2-12.
8. The method for preparing liquid metal nanodroplets according to claim 2, It is characterized in that In the step (2), the temperature is -10 to 30°C, the ultrasonic power is 50 to 2000W, and the ultrasonic time is ≥10s.
9. The method for preparing liquid metal nanodroplets according to claim 8, It is characterized in that In the step (2), the temperature is -5 to 5°C, the ultrasonic power is 300 to 1000W, and the ultrasonic time is 5 to 120 minutes.
10. A liquid metal nanodroplet prepared by the method for preparing a liquid metal nanodroplet according to any one of claims 2 to 9.