Manufacturing process of solid wood anti-deformation cabinet door plate
The solid wood door panel made by short wooden vertical strip tooth joint splicing and hot pressing process, combined with the pressing of the middle plate and the balance layer, solves the deformation problem of the wooden board, and achieves the high bending strength and flatness of the door panel, which significantly increases the thickness of the door panel. Reduces water absorption and expansion.
Patent Information
- Application Number
- CN202411422397.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The deformation problems caused by the expansion and shrinkage of moisture in wooden boards during climate change can only be alleviated but cannot be fundamentally eliminated, affecting the appearance and functionality of furniture.
Short wooden strips are spliced into long wooden strips to form substrate plates of different widths, and sawing and hot pressing along the thickness direction, solid wood strips are made by combining glue coating and hot pressing processes, and further through the middle plate and The pressing of the balance layer enhances the door panel's resistance to deformation.
It significantly prevents the door panel from deforming, reduces the water absorption and expansion coefficient, improves the bending strength and nail grip force, ensures the flatness of the door panel, and effectively solves the deformation problem.
Smart Images

Figure CN118906174A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of panels, and in particular to a manufacturing process of a solid wood anti-deformation cabinet door panel. Background Art
[0002] The deformation problem of wood panels has always troubled the custom home furnishing industry. When wood produces moisture due to factors such as weather changes, its volume will expand, and when the sunlight causes moisture to evaporate, the volume of the wood will shrink. Therefore, in this long-term process of continuous expansion and contraction, wood will deform. Whether it is solid wood or artificial board door panels, they have a large area and few fixing points. In addition, the climate and environment change greatly, so they will deform over time. These deformations not only affect the appearance and service life of the furniture, but may also affect its functionality.
[0003] There are many factors that affect the stability and deformation of the board, including the wood species and properties, the precision of production and processing, the installation process, and the temperature and humidity changes in the use space. In order to solve the problem of door panel deformation, various home furnishing companies have adopted many methods, such as using high-strength materials, controlling humidity, and grooving on the back of the door panel, adding metal strips or using special glue, etc., which can enhance the door panel's ability to resist deformation. However, these measures can often only alleviate such problems, but cannot fundamentally eliminate the risk of deformation. There are areas that can be improved in the existing technology. Summary of the invention
[0004] In view of the above existing situation, the present invention provides a manufacturing process of a solid wood anti-deformation cabinet door panel, comprising the following steps: Step 1, pressing the substrate board: the board includes a substrate layer, a balancing layer and a decorative layer arranged on both sides of the substrate layer. After the short wooden strips are dried, the ends of the short wooden strips are toothed, the short wooden strips are spliced into long wooden strips along the length direction of the short wooden strips, the long wooden strips are spliced into a first substrate board and a second substrate board pressed on both sides of the first substrate board along the width direction, the first substrate board is pressed between the two second substrate boards, the width of the short wooden strips in the first substrate board is different from the width of the short wooden strips in the second substrate board, and the splicing between the long wooden strips in the first substrate board and the splicing between the long wooden strips in the second substrate board are not on the same plane; Step 2: sawing: sawing the pressed first substrate board and the second substrate board into solid wood strips along the thickness direction; Step 3: Lamination of the substrate layer: laminating the solid wood strips along the thickness direction by gluing and hot pressing; Step 4, laminating the middle board: laminating a layer of middle board 4 on both sides of the laminated solid wood strips by gluing and hot pressing to obtain a base material layer; Step 5, pressing and pasting the balancing layer and the decorative layer: the balancing layer is pressed and pasted by cold pressing and hot pressing, and the decorative layer is pressed and pasted by gluing and flat pasting; Step 6: Let it stand: Let it stand horizontally for more than 7 days after pressing the balancing layer, and let it stand for 5-7 days after pressing the decorative layer.
[0005] Preferably, the widths of the short wooden strips are 40 mm, 50 mm and 60 mm respectively.
[0006] Preferably, in step one, the first substrate board and the second substrate board are prepared by gluing and hot pressing processes, the glue is formaldehyde-free glue such as plant soybean glue, the hot pressing temperature is 135-140°C, the hot pressing time is 120s-130s, and the unit pressure is 1.0-1.2Mpa.
[0007] Preferably, in step three, the hot pressing temperature is 130-140° C., the hot pressing time is 120 s-140 s, and the unit pressure is 0.8-1.2 MPa.
[0008] Preferably, the middle board in step 4 is eucalyptus or poplar, and the thickness of the middle board is 2.8-4.0 mm.
[0009] Preferably, the balancing layer in step five is technological veneer or high-density fiberboard with a thickness of 0.4-2.0 mm, and the decorative layer is decorative adhesive paper or decorative adhesive paper plus resin film, and the thickness of the resin film is 0.15-0.40 mm.
[0010] Preferably, grooves penetrating the two sides of the substrate layer are respectively provided on both sides of the substrate layer, and the grooves on both sides of the substrate layer are alternately arranged in sequence along the length direction of the substrate layer. The grooves are filled with putty powder, and a layer of middle plate is pressed on both sides of the substrate layer, and the thickness of the middle plate is 1.5-1.7mm.
[0011] Preferably, in step 4, the amount of glue applied is 1.2-1.3 kg / sheet, the sheets are aged for 120 min after gluing, cold pressed for 40-120 min, the cold pressed pressure is 0.6-0.8 MPa, and then hot pressed, the hot pressed temperature is 120°C, the hot pressed time is 16 min, and the hot pressed pressure is 0.6-0.9 MPa.
[0012] Compared with the prior art, the short wooden strips in the present invention are spliced into long wooden strips through the vertical strip tooth joint process, and then the long wooden strips of different widths are spliced into a first substrate board and a second substrate board respectively, the first substrate board is pressed between the two second substrate boards, and after being sawed into solid wooden strips along the thickness direction, the solid wooden strips are pressed together along the thickness direction, so that the joints on adjacent solid wooden strips are not on the same plane, the deformation prevention is significant, the water absorption expansion coefficient is small, the bending and compressive strength is high, the nail holding force is strong, the flatness of the door panel is good, and the deformation problem of the existing door panel is effectively solved. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 It is a schematic diagram of the structure after the first substrate plate and the second substrate plate are pressed together.
[0014] Figure 2 Schematic diagram of the structure of the substrate layer in Example 1.
[0015] Figure 3 Schematic diagram of the structure of the substrate layer in Example 2.
[0016] Figure 4 for Figure 1 Enlarged view of point A in the middle.
[0017] Figure 5 for Figure 3 Enlarged view of point B in the middle.
[0018] Figure 6 for Figure 2 Enlarged view of point C in the middle.
[0019] Markings in the figure: 1, short wooden strip; 2, first base material board; 3, second base material board; 4, middle board; 5, groove. DETAILED DESCRIPTION
[0020] The present invention will be further described below with reference to the embodiments shown in the accompanying drawings.
[0021] Example 1: Figure 1 , Figure 2 , Figure 4 and Figure 6 As shown, a manufacturing process of a solid wood anti-deformation cabinet door panel includes the following steps: Step 1, pressing of substrate board: the board includes a substrate layer, a balancing layer and a decorative layer arranged on both sides of the substrate layer. After the short wooden strips 1 are dried, the ends of the short wooden strips 1 are toothed, the short wooden strips 1 are spliced into long wooden strips along the length direction of the short wooden strips 1, and the long wooden strips are spliced into a first substrate board 2 and a second substrate board 3 pressed on both sides of the first substrate board 2 along the width direction, and the first substrate board 2 is pressed between the two second substrate boards 3. The width of the short wooden strips 1 in the first substrate board 2 is different from the width of the short wooden strips 1 in the second substrate board 3, and the splicing between the long wooden strips in the first substrate board 2 and the splicing between the long wooden strips in the second substrate board 3 are not on the same plane; Step 2: sawing: sawing the laminated first substrate board 2 and the second substrate board 3 into solid wood strips along the thickness direction; Figure 4 As shown by the arrow D in the middle, the laminated first substrate plate 2 and the second substrate plate 3 are sawn along the direction of the arrow D, and the sawing plane is parallel to the thickness direction of the laminated first substrate plate 2 and the second substrate plate 3; Step 3: Pressing the base material board: Press the solid wood strips along the thickness direction by gluing and hot pressing. Figure 4 As shown by the middle arrow D, the sawed first substrate plate 2 and the second substrate plate 3 are stacked and pressed along the direction of the arrow D; Step 4, laminating the middle board: laminating a layer of middle board 4 on both sides of the laminated solid wood strips by gluing and hot pressing to obtain a base material layer; Step 5, pressing and pasting the balancing layer and the decorative layer: the balancing layer is pressed and pasted by cold pressing and hot pressing, and the decorative layer is pressed and pasted by gluing and flat pasting; Step 6: Let it stand: Let it stand horizontally for more than 7 days after pressing the balancing layer, and let it stand for 6 days after pressing the decorative layer.
[0022] The width of the short wood strip 1 in the first substrate board 2 is 60mm, and the width of the short wood strip 1 in the second substrate board 3 is 50mm. In step one, the first substrate board 2 and the second substrate board 3 are made by gluing and hot pressing process. The glue is formaldehyde-free glue such as plant soybean glue, the hot pressing temperature is 140°C, the hot pressing time is 130s, and the unit pressure is 1.0Mpa. In step three, the hot pressing temperature is 130°C, the hot pressing time is 120s, and the unit pressure is 0.8MPa. The middle board 4 in step four is eucalyptus, and the thickness of the middle board 4 is 3.4mm. In step four, the amount of glue is 1.2kg / sheet, and after gluing, it is aged for 120min, cold pressed for 80min, the cold pressing pressure is 0.7MPa, and then hot pressed, the hot pressing temperature is 120°C, the hot pressing time is 16min, and the hot pressing pressure is 0.8Mpa. The balancing layer described in step five is a technical veneer with a thickness of 1.2mm, and the decorative layer is a decorative adhesive paper plus a resin film, and the thickness of the resin film is 0.2mm. Short wooden strips 1 are spliced into long wooden strips through a vertical strip toothing process, and then long wooden strips of different widths are spliced into a first substrate board 2 and a second substrate board 3 respectively. The first substrate board 2 is pressed between the two second substrate boards 3, and after being sawed into solid wooden strips along the thickness direction, the solid wooden strips are pressed along the thickness direction so that the joints on adjacent solid wooden strips are not on the same plane, with significant anti-deformation, small water absorption expansion coefficient, high bending and compressive strength, strong nail holding force, and good flatness of the door panel, which effectively solves the problem of deformation of existing door panels.
[0023] Embodiment 2: The difference from Embodiment 1 is that Figure 3 and Figure 5 As shown, grooves 5 penetrating the two sides of the substrate layer are respectively provided on both sides of the substrate layer, and the grooves 5 on both sides of the substrate layer are arranged alternately in sequence along the length direction of the substrate layer, and the grooves 5 are filled with putty powder. A layer of middle plate 4 is pressed on both sides of the substrate layer, and the thickness of the middle plate 4 is 1.6 mm. The grooves 5 can further release the internal stress of the plate itself, reduce the influence caused by temperature and humidity changes, and improve its anti-deformation ability, which is simple to operate and has good effect.
[0024] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. However, the obvious changes or changes in the description derived therefrom are still within the scope of protection of the present invention.
Claims
1. A manufacturing process for solid wood anti-deformation cabinet door panels, It is characterized in that The following steps are involved: Step 1, pressing the substrate board: the board comprises a substrate layer, a balancing layer and a decorative layer arranged on both sides of the substrate layer. After the short wooden strips (1) are dried, the ends of the short wooden strips (1) are toothed, the short wooden strips (1) are spliced into long wooden strips along the length direction of the short wooden strips (1), the long wooden strips are spliced into a first substrate board (2) and a second substrate board (3) pressed on both sides of the first substrate board (2) along the width direction, the first substrate board (2) is pressed between the two second substrate boards (3), the width of the short wooden strips (1) in the first substrate board (2) is different from the width of the short wooden strips (1) in the second substrate board (3), and the splicing point between the long wooden strips in the first substrate board (2) and the splicing point between the long wooden strips in the second substrate board (3) are not on the same plane; Step 2: sawing: sawing the pressed first substrate board (2) and the second substrate board (3) into solid wood strips along the thickness direction; Step 3: Pressing the base material board: Pressing the solid wood strips along the thickness direction by gluing and hot pressing; Step 4, laminating the middle plate (4): laminating a layer of the middle plate (4) on both sides of the laminated solid wood strips by gluing and hot pressing to obtain a base material layer; Step 5, pressing and pasting the balancing layer and the decorative layer: the balancing layer is pressed and pasted by cold pressing and hot pressing, and the decorative layer is pressed and pasted by gluing and flat pasting; Step 6: Let it stand: Let it stand horizontally for more than 7 days after pressing the balancing layer, and let it stand for 5-7 days after pressing the decorative layer.
2. According to the manufacturing process of the solid wood anti-deformation cabinet door panel according to claim 1, It is characterized in that The widths of the short wooden strips (1) are 40 mm, 50 mm and 60 mm respectively.
3. The manufacturing process of the solid wood anti-deformation cabinet door panel according to claim 1, It is characterized in that In step 1, a first substrate plate (2) and a second substrate plate (3) are prepared by a gluing and hot pressing process, the glue is a formaldehyde-free glue such as plant soybean glue, the hot pressing temperature is 135-140° C., the hot pressing time is 120 s-130 s, and the unit pressure is 1.0-1.2 Mpa.
4. The manufacturing process of the solid wood anti-deformation cabinet door panel according to claim 1, It is characterized in that In step 3, the hot pressing temperature is 130-140° C., the hot pressing time is 120s-140s, and the unit pressure is 0.8-1.2MPa.
5. The manufacturing process of the solid wood anti-deformation cabinet door panel according to claim 1, It is characterized in that The middle board (4) in step 4 is eucalyptus or poplar, and the thickness of the middle board (4) is 2.8-4.0 mm.
6. The manufacturing process of the solid wood anti-deformation cabinet door panel according to claim 1, It is characterized in that In step 5, the balancing layer is technical wood veneer or high-density fiberboard with a thickness of 0.4-2.0 mm, and the decorative layer is decorative adhesive paper or decorative adhesive paper plus resin film, and the thickness of the resin film is 0.15-0.40 mm.
7. The manufacturing process of the solid wood anti-deformation cabinet door panel according to claim 1, It is characterized in that In step 4, the amount of glue applied is 1.2-1.3 kg / sheet. After gluing, the sheets are aged for 120 minutes, cold pressed for 40-120 minutes, the cold pressed pressure is 0.6-0.8 MPa, and then hot pressed. The hot pressed temperature is 120°C, the hot pressed time is 16 minutes, and the hot pressed pressure is 0.6-0.9 MPa.
8. The manufacturing process of the solid wood anti-deformation cabinet door panel according to claim 1, It is characterized in that Grooves (5) penetrating through the two sides of the substrate layer are respectively provided on both sides of the substrate layer. The grooves (5) on both sides of the substrate layer are arranged alternately in sequence along the length direction of the substrate layer. The grooves (5) are filled with putty powder. A layer of middle plate (4) is respectively pressed on both sides of the substrate layer. The thickness of the middle plate (4) is 1.5-1.7 mm.
Citation Information
Patent Citations
Groove type solid wood medium plate and composite plate with same
CN102352682A
Process for manufacturing high-strength laminated wood board
CN102371603A
Method for producing laminated woods with small-diameter logs and produced laminated wood
CN102463606A
Method for manufacturing environment-friendly high-strength anti-deformation solid wood composite door
CN103128823A
Processing method of non-deforming sheet material and non-deforming plate thereof
CN109366636A