Basalt fiber felt and polyphenylene sulfide compounded lightweight board and preparation method thereof

Through the alternating laying and hot pressing of basalt fiber felt and polyphenylene sulfide non-woven fabric, the problem of heavy weight of traditional composite sheets is solved, and lightweight sheets are prepared with excellent mechanical and thermal insulation properties, suitable for high-end fields , meet the needs of aerospace and other fields.

CN118906569APending Publication Date: 2024-11-08WUHAN TEXTILE UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410955445.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional composite sheets have a large weight, which limits their application in aerospace and other fields, especially in areas where light weight is required but excellent performance is guaranteed.

Method used

Basalt fiber felt and polyphenylene sulfide nonwoven fabric are alternately laid, and hot pressing is carried out below the melting point of polyphenylene sulfide. Lightweight plates are prepared by combining wet crumbing and sintering technology, and the hot pressing temperature and pressure are controlled to keep them small. Void structure reduces overall weight while improving mechanical properties.

Benefits of technology

It realizes lighter composite sheets while maintaining excellent mechanical properties, thermal insulation properties and flame retardant properties. It is suitable for high-end fields such as aerospace and construction, and is environmentally friendly and does not contain harmful substances.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a basalt fiber felt and polyphenylene sulfide compounded lightweight board and a preparation method thereof, and belongs to the field of composite materials. The method comprises the following steps: carrying out modification treatment on basalt chopped fibers, and then mixing the basalt chopped fibers with polyphenylene sulfide superfine and ultra-short fibers; the mixed fibers are dissociated and then poured into a dispersing agent to be evenly stirred, and then the basalt fiber felt is prepared through wet-process papermaking and sintering treatment; after the basalt fiber felt and the polyphenylene sulfide non-woven fabric are alternately laid, hot pressing treatment is carried out below the melting point of polyphenylene sulfide, and after cooling, the basalt fiber felt and polyphenylene sulfide composite light board is obtained. Therefore, hot pressing processing is carried out below the melting point of the polyphenylene sulfide, so that the basalt fiber felt and the polyphenylene sulfide are combined together, meanwhile, a large number of tiny gap structures existing in the basalt fiber felt are kept as much as possible, and therefore the light overall weight is achieved. Although the composite board is light, the composite board still shows excellent mechanical properties and has a good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of composite materials, and more specifically, relates to a lightweight plate composited with basalt fiber felt and polyphenylene sulfide and a preparation method thereof. Background Art

[0002] Traditional composite sheets are usually made by melting resin to fill the gaps inside the sheet to ensure good bonding between layers. However, this manufacturing method results in a heavy weight for the composite sheet, which limits its application in multi-layer stacking, especially in fields such as aerospace that require light weight but excellent performance.

[0003] To overcome this limitation, researchers have begun exploring lighter and stronger composite materials in recent years in order to reduce the overall weight without sacrificing structural strength, thereby expanding the application areas of composite panels. Summary of the invention

[0004] In view of the defects of the prior art and the need for improvement, the present invention provides a lightweight board material composited with basalt fiber felt and polyphenylene sulfide and a preparation method thereof, aiming to solve the technical problem that the traditional composite board material is heavy and has limited application areas.

[0005] To achieve the above object, in a first aspect, the present invention provides a method for preparing a lightweight plate material composited with basalt fiber felt and polyphenylene sulfide, the method comprising the following steps:

[0006] The basalt chopped fibers are modified and mixed with polyphenylene sulfide ultrafine and ultrashort fibers;

[0007] The mixed fibers are dissociated and poured into a dispersant and stirred evenly, and then wet-coated and sintered to form basalt fiber felt;

[0008] After basalt fiber felt and polyphenylene sulfide non-woven fabric are alternately laid, hot pressing treatment is performed below the melting point of polyphenylene sulfide, and after cooling, a lightweight board composed of basalt fiber felt and polyphenylene sulfide is obtained; wherein the uppermost layer and the lowermost layer of the lightweight board are both polyphenylene sulfide non-woven fabrics.

[0009] Furthermore, during the hot pressing process, the hot pressing temperature is 150-250° C., the hot pressing pressure is 15-25 MPa, the hot pressing times are 1-2 times, and the hot pressing time is 20-30 min.

[0010] Furthermore, the length of the basalt chopped fibers is 40-70 mm; the fineness of the polyphenylene sulfide ultrafine and ultrashort fibers is 0.1-0.5 dext and the length is 1-3 mm.

[0011] Furthermore, the modification treatment conditions are: hydrochloric acid concentration is 2.1 mol / L, modification time is 14 h, and modification temperature is 54.3°C.

[0012] Furthermore, the dissociation process is: pouring the mixed fiber into a fiber dissociator for fiber dissociation in 2-4 times, the rotation speed of the fiber dissociator is 4000-5040r / min, and the dissociation time is 20-40min.

[0013] Furthermore, the dispersant is prepared by mixing polyethylene oxide and anionic polyacrylamide in a mass ratio of 2:1-6:1, and stirring the mixture in a magnetic stirrer at 400-600 rpm for 4-6 hours.

[0014] Furthermore, the basalt fiber felt is made by wet papermaking and sintering, comprising:

[0015] The stirred fibers are poured into a paper sheet former to be formed, and wet basalt / polyphenylene sulfide composite paper base paper is obtained after dehydration, and the wet basalt / polyphenylene sulfide composite paper base paper is sintered to prepare basalt fiber felt;

[0016] The sintering temperature is 330-350°C, and the sintering time is 2-5 minutes.

[0017] Furthermore, the basalt fiber felt has a gram weight of 30-80 g / m 2 The weight of polyphenylene sulfide non-woven fabric is 20-110g / m 2 . .

[0018] Furthermore, the thickness of the lightweight plate is 1-10 mm.

[0019] In a second aspect, the present invention provides a lightweight board material composited with basalt fiber felt and polyphenylene sulfide, wherein the lightweight board material is prepared by the method for preparing a lightweight board material composited with basalt fiber felt and polyphenylene sulfide according to the first aspect.

[0020] In general, the above technical solutions conceived by the present invention can achieve the following beneficial effects:

[0021] 1. The present invention takes into account that basalt fiber has excellent high and low temperature resistance, excellent electrical insulation performance, good mechanical properties and chemical stability, and is low in price. At the same time, polyphenylene sulfide has excellent high temperature resistance and is a thermoplastic resin. After melting at high temperature, it forms bonding points and can well connect basalt fibers together. Therefore, basalt chopped fibers and polyphenylene sulfide ultrafine and ultrashort fibers are used to make basalt fiber felt.

[0022] 2. After the basalt fiber felt and the polyphenylene sulfide non-woven fabric are alternately laid, the present invention performs hot pressing processing below the melting point of polyphenylene sulfide. By controlling the temperature, pressure and time, the two are combined together while maintaining the large number of tiny void structures existing in the basalt fiber felt itself as much as possible, thereby achieving a lighter overall weight. Despite its lightness, the composite board still exhibits excellent mechanical properties, including excellent stiffness and strength, which makes it competent in various engineering applications. In addition, the material has excellent thermal insulation and flame retardant properties, which can effectively prevent the spread of fire and improve the safety of buildings. In terms of environmental protection, it does not contain harmful substances and meets the requirements of modern society for sustainable development. Therefore, it is increasingly favored in construction, aerospace and other high-end fields.

[0023] 3. In the process of alternately laying basalt fiber felt and polyphenylene sulfide non-woven fabric, the present invention selects polyphenylene sulfide non-woven fabric as the outermost layer of the composite board, thereby preventing the outermost layer of the board from adhering to the hot-pressed iron plate during the hot-pressing process and being difficult to separate. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0025] The experimental methods in the following examples, unless otherwise specified, are all conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial channels.

[0026] Example 1

[0027] Weigh 2.4g of polyethylene oxide and 1.2g of anionic polyacrylamide into a beaker containing 1.6L of water, and place the beaker in a magnetic stirrer and rotate at 400rpm for 4 hours to obtain a dispersant. Weigh 3.5g of basalt chopped fibers treated with hydrochloric acid (hydrochloric acid concentration is 2.1mol / L, modification time is 14h, and modification temperature is 54.3℃) and 8.07g of polyphenylene sulfide ultrafine short fibers into a beaker containing 1.2L of water to obtain basalt / polyphenylene sulfide mixed fibers, wherein the length of the basalt chopped fibers is 40mm, and the fineness of the polyphenylene sulfide ultrafine short fibers is 0.1dext and the length is 1mm. Pour the mixed fibers into a fiber disintegrator twice for fiber disintegration, the disintegrator speed is 4000r / min, each disintegration is 20 minutes, and the total disintegration time is 40 minutes. Pour the dissociated mixed fiber into the dispersant and stir evenly, then pour it into the paper sheet former to form it, dehydrate it to get the wet basalt / polyphenylene sulfide composite paper base, put it into an oven set at 330℃ for sintering for 2 minutes to get the homemade basalt fiber felt. Cut 70 layers of basalt fiber felt and 71 layers of polyphenylene sulfide non-woven fabric, the bottom layer is polyphenylene sulfide non-woven fabric, then lay the basalt fiber felt on the polyphenylene sulfide non-woven fabric, then lay a layer of polyphenylene sulfide non-woven fabric and then lay a layer of basalt fiber felt, and so on, until the top layer is polyphenylene sulfide non-woven fabric; among them, the gram weight of basalt fiber felt is 30g / m 2 , the weight of polyphenylene sulfide nonwoven fabric is 20g / m 2 Finally, hot pressing was performed. The hot pressing parameters on the hot pressing machine were: hot pressing temperature of 150°C, hot pressing pressure of 15MPa, hot pressing times of 1 time, and hot pressing time of 20min, to obtain a lightweight board composed of basalt fiber felt and polyphenylene sulfide. The prepared lightweight board has a tensile strength of 176Mpa, a bending strength of 140Mpa, and an impact strength of 90kg / m 2 .

[0028] Example 2

[0029] Weigh 2.4g of polyethylene oxide and 0.6g of anionic polyacrylamide into a beaker containing 1.6L of water, and place the beaker in a magnetic stirrer and rotate at 500rpm for 5 hours to obtain a dispersant. Weigh 5.76g of basalt short fibers treated with hydrochloric acid (hydrochloric acid concentration is 2.1mol / L, modification time is 14h, and modification temperature is 54.3℃) and 5.76g of polyphenylene sulfide ultrafine short fibers into a beaker containing 1.2L of water to obtain basalt / polyphenylene sulfide mixed fibers, wherein the length of the basalt short fibers is 55mm, and the fineness of the polyphenylene sulfide ultrafine short fibers is 0.3dext and the length is 2mm. Pour the mixed fibers into a fiber disintegrator for fiber disintegration in 3 times, the disintegrator speed is 4500r / min, each disintegration is 30 minutes, and the total disintegration time is 90 minutes. Pour the dissociated mixed fiber into the dispersant and stir evenly, then pour it into the paper sheet former to form it, and after dehydration, obtain the wet basalt / polyphenylene sulfide composite paper base paper, which is placed in an oven set at 340°C for sintering for 3 minutes to obtain a homemade basalt fiber felt. Cut 70 layers of basalt fiber felt and 71 layers of polyphenylene sulfide non-woven fabric, the bottom layer is polyphenylene sulfide non-woven fabric, and then lay the basalt fiber felt on the polyphenylene sulfide non-woven fabric, and then lay a layer of polyphenylene sulfide non-woven fabric and then a layer of basalt fiber felt, and so on, until the top layer is polyphenylene sulfide non-woven fabric; among them, the gram weight of basalt fiber felt is 55g / m 2 The weight of polyphenylene sulfide nonwoven fabric is 65g / m 2 Finally, hot pressing was performed. The hot pressing parameters on the hot pressing machine were: hot pressing temperature of 200°C, hot pressing pressure of 20MPa, hot pressing times of 2 times, and hot pressing time of 25min. A lightweight board composed of basalt fiber felt and polyphenylene sulfide was obtained. The prepared lightweight board has a tensile strength of 232Mpa, a bending strength of 179Mpa, and an impact strength of 120kg / m 2 .

[0030] Example 3

[0031] Weigh 2.4g of polyethylene oxide and 0.4g of anionic polyacrylamide into a beaker containing 1.6L of water, and place the beaker in a magnetic stirrer and rotate at 600rpm for 6 hours to obtain a dispersant. Weigh 8.07g of basalt short fibers treated with hydrochloric acid (hydrochloric acid concentration is 2.1mol / L, modification time is 14h, and modification temperature is 54.3℃) and 3.5g of polyphenylene sulfide ultrafine short fibers into a beaker containing 1.2L of water to obtain basalt / polyphenylene sulfide mixed fibers, wherein the length of the basalt short fibers is 70mm, and the fineness of the polyphenylene sulfide ultrafine short fibers is 0.5dext and the length is 3mm. Pour the mixed fibers into a fiber disintegrator for fiber disintegration in 4 times, the disintegrator speed is 5040r / min, each disintegration takes 40 minutes, and the total disintegration takes 160 minutes. Pour the dissociated mixed fiber into the dispersant and stir evenly, then pour it into the paper sheet former to form it, dehydrate it to get the wet basalt / polyphenylene sulfide composite paper base paper, put it into an oven set at 350℃ for sintering for 5 minutes to get the homemade basalt fiber felt. Cut 70 layers of basalt fiber felt and 71 layers of polyphenylene sulfide non-woven fabric, the bottom layer is polyphenylene sulfide non-woven fabric, then lay the basalt fiber felt on the polyphenylene sulfide non-woven fabric, then lay a layer of polyphenylene sulfide non-woven fabric and then lay a layer of basalt fiber felt, and so on, until the top layer is polyphenylene sulfide non-woven fabric; among them, the gram weight of basalt fiber felt is 80g / m 2 , the weight of polyphenylene sulfide nonwoven fabric is 110g / m 2 Finally, hot pressing was performed. The hot pressing parameters on the hot pressing machine were: hot pressing temperature of 250°C, hot pressing pressure of 25MPa, hot pressing times of 2 times, and hot pressing time of 30min, to obtain a lightweight board composed of basalt fiber felt and polyphenylene sulfide. The prepared lightweight board has a tensile strength of 252Mpa, a bending strength of 185Mpa, and an impact strength of 129kg / m 2 .

[0032] Embodiment 4-5

[0033] Examples 4-5 all repeat Example 1, the only difference is that in Example 1, 3.5g of basalt chopped fibers treated with hydrochloric acid (hydrochloric acid concentration is 2.1mol / L, modification time is 14h, modification temperature is 54.3℃) and 8.07g of polyphenylene sulfide ultrafine short fibers are weighed and put into a beaker containing 1.2L of water, while in Example 4, 5.76g of basalt chopped fibers and 5.76g of polyphenylene sulfide ultrafine short fibers are weighed, and in Example 5, 8.07g of basalt chopped fibers and 3.5g of polyphenylene sulfide ultrafine short fibers are weighed. The performance test data of the prepared lightweight board are shown in Table 1.

[0034] Embodiment 6-7

[0035] Examples 6-7 repeat Example 1, the only difference is that the hot pressing temperature in Example 1 is 150° C., while the hot pressing temperature in Example 6 is 200° C., and the hot pressing temperature in Example 7 is 250° C. See Table 1 for the performance test data of the prepared lightweight board.

[0036] Embodiment 8-9

[0037] Examples 8-9 are the same as Example 1, with the only difference being that the hot pressing pressure in Example 1 is 15 MPa, while the hot pressing pressure in Example 8 is 20 MPa, and the hot pressing pressure in Example 9 is 25 MPa. The performance test data of the prepared lightweight board are shown in Table 1.

[0038] Table 1 Performance test data of lightweight panels prepared in Examples 1, 4-9

[0039] Example Tensile strength(Mpa) Bending strength(Mpa) <![CDATA[Impact strength (kg / m 2 )]]> Example 1 176 140 90 Example 4 182 146 97 Example 5 170 133 86 Example 6 223 162 119 Example 7 278 196 132 Example 8 247 170 124 Example 9 301 199 144

[0040] By comparing the above-mentioned embodiments 1, 4, and 5, it can be seen that as the basalt content in the basalt fiber felt increases, the tensile properties, bending properties, and impact properties of the composite board first increase and then decrease slightly. Excessive basalt fibers will destroy the internal structure of the composite board due to their cylindrical structure.

[0041] By comparing the above-mentioned Examples 1, 6, 7 with Examples 1, 8, 9, it can be seen that with the increase of temperature and pressure in the hot pressing treatment, the tensile properties, bending properties and impact properties of the composite board are significantly improved. This method can be used to prepare basalt fiber / polyphenylene sulfide composite boards with excellent performance.

[0042] It should be noted that in the above embodiments 1 to 9, the thickness of the composite board is 5 mm, requiring 70 layers of basalt fiber felt and 71 layers of polyphenylene sulfide non-woven fabric. In practical applications, the thickness of the composite board can generally be 1-10 mm, and those skilled in the art can determine the number of layers of basalt fiber felt and polyphenylene sulfide non-woven fabric according to actual needs.

[0043] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a lightweight board composited with basalt fiber felt and polyphenylene sulfide, characterized in that: The method comprises the following steps: The basalt chopped fibers are modified and mixed with polyphenylene sulfide ultrafine and ultrashort fibers; The mixed fibers are dissociated and poured into a dispersant and stirred evenly, and then wet-coated and sintered to form basalt fiber felt; After basalt fiber felt and polyphenylene sulfide non-woven fabric are alternately laid, hot pressing treatment is performed below the melting point of polyphenylene sulfide, and after cooling, a lightweight board composed of basalt fiber felt and polyphenylene sulfide is obtained; wherein the uppermost layer and the lowermost layer of the lightweight board are both polyphenylene sulfide non-woven fabrics.

2. The method for preparing a lightweight board composed of basalt fiber felt and polyphenylene sulfide according to claim 1, characterized in that: During the hot pressing process, the hot pressing temperature is 150-250° C., the hot pressing pressure is 15-25 MPa, the hot pressing times are 1-2 times, and the hot pressing time is 20-30 min.

3. The method for preparing a lightweight board composed of basalt fiber felt and polyphenylene sulfide according to claim 1, characterized in that: The length of the basalt chopped fibers is 40-70 mm; the fineness of the polyphenylene sulfide ultrafine and ultrashort fibers is 0.1-0.5 dext and the length is 1-3 mm.

4. The method for preparing a lightweight board composed of basalt fiber felt and polyphenylene sulfide according to claim 1, characterized in that: The modification treatment conditions are: hydrochloric acid concentration is 2.1 mol / L, modification time is 14 h, and modification temperature is 54.3°C.

5. The method for preparing a lightweight board composited with basalt fiber felt and polyphenylene sulfide according to claim 1, characterized in that: The dissociation process is as follows: the mixed fibers are poured into a fiber dissociator for fiber dissociation in 2-4 times, the rotation speed of the fiber dissociator is 4000-5040 r / min, and the dissociation time is 20-40 min.

6. The method for preparing a lightweight plate composited with basalt fiber felt and polyphenylene sulfide according to claim 1, characterized in that: The dispersant is prepared by mixing polyethylene oxide and anionic polyacrylamide at a mass ratio of 2:1-6:1 and stirring the mixture in a magnetic stirrer at 400-600 rpm for 4-6 hours.

7. The method for preparing a lightweight board composited with basalt fiber felt and polyphenylene sulfide according to claim 1, characterized in that: The basalt fiber felt is made by wet papermaking and sintering, comprising: The stirred fibers are poured into a paper sheet former to be formed, and wet basalt / polyphenylene sulfide composite paper base paper is obtained after dehydration, and the wet basalt / polyphenylene sulfide composite paper base paper is sintered to prepare basalt fiber felt; The sintering temperature is 330-350°C, and the sintering time is 2-5 minutes.

8. The method for preparing a lightweight board composited with basalt fiber felt and polyphenylene sulfide according to claim 1, characterized in that: The basalt fiber felt has a gram weight of 30-80 g / m 2 The weight of polyphenylene sulfide non-woven fabric is 20-110g / m 2 .

9. The method for preparing a lightweight board composed of basalt fiber felt and polyphenylene sulfide according to claim 1, characterized in that: The thickness of the lightweight plate is 1-10 mm.

10. A lightweight board composed of basalt fiber felt and polyphenylene sulfide, characterized in that: The lightweight board is prepared by the method for preparing a lightweight board composited with basalt fiber felt and polyphenylene sulfide according to any one of claims 1 to 9.