Mould-pressing foaming-formed polypropylene composite foamed sheet as well as preparation method and application of mould-pressing foaming-formed polypropylene composite foamed sheet

By using a laminated structure of high-strength polypropylene composite sheet and foamed sheet and a random copolymer polypropylene composition in the polypropylene composite foamed sheet, the problems of thickness and mechanical properties of the polypropylene foamed sheet are solved, and the problem of thickness and mechanical properties of the polypropylene foamed sheet is realized. High compression strength and thermal insulation performance, and good recyclability, avoiding the use of thermal adhesives.

CN118906603AActive Publication Date: 2024-11-08CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310513099.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-08
Estimated Expiration
2043-05-08

AI Technical Summary

Technical Problem

While improving physical properties, existing polypropylene foamed sheets are difficult to meet the thickness and mechanical properties requirements, and are difficult to recover. Conventional reinforced sheets have compatibility problems and high energy consumption problems.

Method used

High-strength, high-impact polypropylene composite sheet and polypropylene foamed sheet are used to form a laminated structure through molding and foaming, and combine random copolymer polypropylene composition to achieve high compression strength and good thermal insulation performance without heat required Adhesion reinforcement has good recyclability.

Benefits of technology

The high compression strength, excellent thermal insulation performance and good thermal insulation performance of polypropylene composite foamed sheets are achieved, and they can be directly crushed and melted and recovered, reducing recycling costs and improving compatibility with other materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004218608150000231
    Figure BDA0004218608150000231
Patent Text Reader

Abstract

The invention belongs to the technical field of high polymer materials, and particularly relates to a polypropylene composite foamed sheet formed by mould pressing foaming and a preparation method and application thereof. The polypropylene composite foamed sheet has a laminated structure and comprises at least one layer of reinforced composite sheet and at least one layer of polypropylene foamed sheet bonded with the reinforced composite sheet through mould pressing foaming, each layer of reinforced composite sheet comprises at least one layer of polypropylene sheet / fabric; the polypropylene sheet comprises a layer A and layers B and B'located on the two sides of the layer A, and the structure of the polypropylene sheet is BAB '; wherein the melting point of the polypropylene composition A is greater than the melting points of the polypropylene B and the polypropylene B ', and the mould pressing foaming is physical foaming. The polypropylene composite foamed sheet adopts mould pressing foaming, has a plurality of production advantages, has higher compression strength, and is convenient to recycle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a polypropylene composite foaming plate formed by compression foaming, and a preparation method and application thereof. Background Art

[0002] The global polypropylene foam sheet (thickness above 25mm is called sheet) material market will grow at an annual rate of 6.9% between 2018 and 2023, from US$751.0 million in 2018 to US$1,048.8 million in 2023. Based on the type of foam material: the low-density segment is expected to lead the foam sheet market. The growth in demand for automotive, protective packaging and insulation applications has driven the growth of this segment. The automotive industry dominates the consumption of low-density polypropylene foam sheets, which helps cars to be more impact-resistant and reduce body weight. This also requires further improvement of the physical properties of polypropylene foam sheets while minimizing the increase in production costs during molding. At present, the mature and stable foaming processes for preparing low-density polypropylene sheets at home and abroad are mainly divided into extrusion foaming and compression foaming.

[0003] The extrusion foaming method is to put polypropylene particles into an extruder, use carbon dioxide, hydrocarbons, chemical foaming agents or cross-linking agents as needed, melt-mix under heating and pressure, and then extrude and foam. However, due to the limitation of die design, it is difficult to make the thickness of the polypropylene foam sheet obtained by using carbon dioxide as a foaming agent more than 25mm, the pore diameter is large (about 500μm), the open porosity is high (≥50%), and the mechanical properties are poor; the polypropylene foam sheet obtained by using a chemical foaming agent has a low foaming ratio (about 5 times), no obvious weight loss, uneven pore shape, and is also difficult to cut.

[0004] The compression foaming method is to put the polypropylene sheet into a molding machine, introduce a foaming agent such as carbon dioxide, increase the temperature and pressurize it so that the foaming agent is saturated in the sheet, and then quickly release the pressure and cool it down to obtain a polypropylene foam sheet. It can be processed using an ordinary hot press. The process equipment is simple, the conditions are mild, the equipment requirements are low, and the production cost is low. The advantage of this foaming process is that after the motherboard is extruded, the supercritical fluid foaming agent can be fully impregnated in the mold, and the pressure can be quickly released and the mold can be opened in one time to produce a large surface area foam sheet, and the three-dimensional size can reach 2400mm*1200mm*100mm. The foaming ratio is wide, and by adjusting the process conditions, 5 to 35 times of foaming materials can be obtained to meet different application requirements. In the compression foaming method, because the foaming agent is fully saturated and impregnated in the production, it is very evenly dispersed in the polypropylene resin. When the pressure is released and foamed, it can serve as a heterogeneous nucleation point for multiple bubbles, promoting the rapid and large growth of the pores instead of merging and becoming larger. Therefore, the molded foamed polypropylene material has a uniform and fine pore structure with a diameter of less than 50μm, which can be called a microporous material, which brings better mechanical properties, thermal insulation properties and processing properties to the foamed material. It is currently the most ideal processing method for thick foamed polypropylene sheets.

[0005] Traditional methods such as optimizing raw materials and processes are no longer able to meet the needs of the market. The use of filler modification can effectively improve the physical properties of polypropylene foam sheets, but it will also significantly weaken the foaming molding ability of special materials and the weight reduction effect of the appearance quality of products; by designing and adjusting the types and contents of catalysts and comonomers to optimize the molecular structure of special materials for polypropylene foam sheets, the physical properties of polypropylene foam sheet products can be improved while also improving the foaming molding ability, but the production promotion cycle is long and the cost is high; optimizing the foaming molding process conditions of polypropylene foam sheets requires upstream and downstream enterprises of polypropylene foam products to adjust the production process parameters and even equipment, which is difficult for manufacturers to accept.

[0006] In order to further improve the physical properties of polypropylene foam sheet products, it has become a new process solution to composite inorganic or organic reinforcing sheets on the surface of polypropylene foam sheets. The reinforced sheets composited in the existing technology have high requirements for mechanical properties, and mainly use composite materials such as glass fiber / carbon fiber reinforced thermoplastic resins. These reinforced sheets are prone to compatibility problems with polypropylene foam sheets, which makes it difficult to achieve ideal physical properties such as compression and thermal insulation. Even if a polypropylene foam sheet product that meets the product performance is successfully obtained, the presence of the reinforced sheet brings about problems such as high apparent density, long molding time and high energy consumption. In addition, the existing polypropylene foam sheet obtained by using composite materials such as glass fiber / carbon fiber reinforced thermoplastic resins as reinforced sheets needs to separate the reinforced sheets when recycling, and cannot be directly crushed and melted, making it difficult to recycle.

[0007] Conventional polypropylene sheets used as reinforcing plates either fail to meet the strength requirements and cannot produce polypropylene composite foam plates with compressive strength that meets the requirements, or are not suitable for compression foaming and cannot produce composite foam plates of qualified quality.

[0008] In summary, how to provide a polypropylene composite foam board that can use polypropylene sheets as reinforced boards, meet the compression strength requirements and be easy to recycle, while also being able to utilize the advantages of compression foaming molding, is the goal of the present invention. Summary of the invention

[0009] In view of the deficiencies of the above-mentioned prior art, the present invention provides a polypropylene composite foamed board formed by compression foaming, and a preparation method and application thereof. The polypropylene composite foamed board uses a high-strength and high-impact polypropylene composite sheet as a composite sheet, which can not only adopt compression foaming and have many production advantages, but also has high compression strength. In addition, the polypropylene composite foamed board of the present invention has excellent apparent density, physical properties and thermal insulation properties without adding a thermal bonding enhancer, and compared with other pre-reinforced boards made of non-polypropylene materials on the market, the compatibility is greatly improved, and no separation treatment is required during recycling, and it can be directly crushed and melted, and then granulated and used again, which has broad market prospects in the field of polypropylene foamed board technology.

[0010] In the first aspect, the purpose of the present invention is to provide a polypropylene composite foamed board material having a laminated structure, comprising at least one layer of reinforced composite sheet and at least one layer of polypropylene foamed sheet bonded to the reinforced composite sheet by molded foaming; each layer of the reinforced composite sheet comprises at least one layer of polypropylene sheet and / or at least one layer of polypropylene fabric woven from polypropylene sheets; wherein the polypropylene sheet comprises layer A and layers B and B' located on both sides of layer A, and the structure is BAB'; wherein layer A contains a polypropylene composition A, wherein the polypropylene composition A comprises homopolymer polypropylene a and impact copolymer polypropylene b; layer B is the same as or different from layer B', and each correspondingly contains a polypropylene composition B and a polypropylene composition B', wherein the polypropylene composition B and the polypropylene composition B' each comprise a random copolymer polypropylene x; wherein the melting point of the polypropylene composition A is greater than the melting point of the polypropylene composition B and the polypropylene composition B'; and the molded foaming is physical foaming.

[0011] In some preferred embodiments of the present invention, the melting point of the homopolymerized polypropylene a in the polypropylene composition A is greater than the melting point of the random copolymerized polypropylene x in the polypropylene compositions B and B', and preferably the temperature difference of the corresponding melting points is greater than or equal to 10 degrees. In this preferred embodiment, the inventors of the present invention surprisingly found that the obtained polypropylene composite foamed sheet has higher compressive strength.

[0012] In some preferred embodiments of the present invention, the polypropylene composition B and the polypropylene composition B' are each 100% of the random copolymerized polypropylene x.

[0013] In some preferred embodiments of the present invention, based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 50-99wt% of homopolypropylene a and 1-50wt% of impact copolymer polypropylene b; preferably, the polypropylene composition A comprises 70-90wt% of homopolypropylene a and 10-30wt% of impact copolymer polypropylene b.

[0014] According to the present invention, the layers B and B' on both sides of the layer A are the same or different. In a preferred embodiment of the present invention, the layers B and B' on both sides of the layer A are the same.

[0015] In some preferred embodiments of the present invention, based on the total thickness of the polypropylene sheet, the thickness of the layer A accounts for 51%-89% of the total thickness, preferably 71%-89%, and more preferably 71%-80%.

[0016] The thicknesses of the layers B and B' on both sides of the layer A may be the same or different, but are preferably the same.

[0017] The present invention does not limit the thickness of the polypropylene sheet, and can be selected in a wide range according to its practical application field. Preferably, the thickness of the polypropylene sheet can be 10-1000 μm, preferably 30-500 μm, and more preferably 50-300 μm.

[0018] According to the present invention, the thickness of layer A, layer B, and layer B' can be controlled by the melt pump of the extruder during the processing.

[0019] In some preferred embodiments of the present invention, the homopolypropylene a has:

[0020] The melting point is 150-170°C, preferably 160-170°C; and / or,

[0021] The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or,

[0022] The isotacticity (mm) is not less than 96%.

[0023] In some preferred embodiments of the present invention, the impact-resistant copolymer polypropylene b has: the melting point of the impact-resistant copolymer polypropylene b is 150-170°C: and / or the monomer copolymerized between the impact-resistant copolymer polypropylene b and propylene is ethylene or butene; more preferably, the monomer copolymerized between the high-impact copolymer polypropylene b and propylene is ethylene or butene, and the ethylene or butene content is 2-50%wt, preferably 3-20%wt, and further preferably 5-15%wt.

[0024] In some preferred embodiments of the present invention, the melt flow rate of the impact-resistant copolymer polypropylene b at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or the cantilever beam impact strength of the impact-resistant copolymer polypropylene b is not less than 20 KJ / m 2 (Test conditions: 23℃).

[0025] In some preferred embodiments of the present invention, the polypropylene composition B and the polypropylene composition B' are each selected from random copolymer polypropylene x; and / or the random copolymer polypropylene x has: a melting point of 110-150°C, preferably 120-140°C; and / or a melt flow rate at 230°C and a load of 2.16 kg of 0.5-50 g / 10 min, preferably 1-20 g / 10 min, further preferably 3-18 g / 10 min; and / or a molecular weight distribution Mw / Mn of 5-12, preferably 7-10; and / or the random copolymer polypropylene x is a copolymer of propylene and ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene binary copolymer.

[0026] According to the research conducted by the inventors, when the melt mass flow rate and the polypropylene composition ratio of the polypropylene composition A are within the above preferred ranges, the high impact copolymer polypropylene b in the composition can absorb impact energy well, meet the requirements of impact performance, and make the sheet have good impact performance. At the same time, since the macromolecular segments in the homopolymer polypropylene a are relatively regular, crystallization occurs during the preparation of the sheet, so the sheet also has good tensile properties.

[0027] According to research conducted by the present inventors, when the melt mass flow rate and the polypropylene composition ratio of the polypropylene composition B and the polypropylene composition B' are within a preferred range, good adhesion performance can be provided to the sheet material, and the interlayer peeling strength can be further improved.

[0028] In some preferred embodiments of the present invention, the layer A further contains a β-crystalline nucleating agent; preferably,

[0029] The β-crystal nucleating agent is selected from at least one of condensed ring aromatic hydrocarbons, group IIA two-component complexes, aromatic diamides, rare earth compounds and cyclic dicarboxylates.

[0030] In some preferred embodiments of the present invention, the content of the β-crystal nucleating agent in layer A is 0.01-0.5 parts by weight relative to 100 parts by weight of the polypropylene composition A. For example, the content of the β-crystal nucleating agent may be 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, or 0.5 parts by weight.

[0031] According to research conducted by the present inventors, when the melt mass flow rate, polypropylene composition ratio and thickness distribution of layer A of the polypropylene composition A, the polypropylene composition B and the polypropylene composition B' are within a preferred range, the sheet preparation process can be smoother, thereby making the sheet have better uniformity and higher compressive strength.

[0032] The BAB' sheet structure of the polypropylene sheet can be prepared by a variety of methods. In a preferred embodiment of the present invention, the BAB' sheet structure of the polypropylene sheet is obtained by co-extruding components including a polypropylene composition A and polypropylene compositions B and B'. Preferably, the BAB' sheet structure of the polypropylene sheet is obtained by co-extruding, casting or calendering, and stretching components including a polypropylene composition A and polypropylene compositions B and B' to obtain the polypropylene sheet.

[0033] In a preferred embodiment of the present invention, the preparation of the polypropylene composition A comprises melt blending the components including the homopolypropylene a and the impact copolymer polypropylene b; and / or, the preparation of the polypropylene compositions B and B' comprises melt blending the components including the random copolymer polypropylene x; and / or, the temperatures of the coextrusion and casting are independently selected from 200-240°C; and / or, the temperature of the calendering roll is 50-70°C; and / or, the stretching conditions include: the stretching temperature is 90-165°C, preferably 90-140°C, and more preferably 90-119°C; the stretching ratio is 1-15 times; preferably 2-9 times.

[0034] The process of the extrusion calendering method may include sequentially passing the coextruded polypropylene sheet through a calendering roller and a traction roller, and then solid phase stretching, trimming and winding to obtain the sheet. The temperature of the extrusion casting is 200-230° C., and the temperature of the calendering roller is 50-70° C. The specific process of preparing the film by the extrusion calendering method is a common choice in the art and will not be repeated here.

[0035] The polypropylene fabric is woven from a polypropylene sheet, preferably a three-dimensional polypropylene fabric woven from the polypropylene sheet as described above; more preferably, the polypropylene fabric has a three-dimensional structure of plain, twill and / or satin.

[0036] In order to facilitate weaving, the polypropylene sheet is preferably cut into polypropylene sheets with a width of 2-5 mm, and then the polypropylene fabric is obtained by weaving.

[0037] In a more preferred embodiment of the present invention, the polypropylene fabric is a plain, twill, satin or three-dimensional polypropylene fabric obtained by weaving three-layer co-extruded polypropylene stretch flat tape, and the three-layer co-extruded polypropylene stretch flat tape includes layer A formed by a high-melting point polypropylene combination A and layers B, B' formed by low-melting point polypropylene compositions B, B', wherein the polypropylene composition A includes homopolymer polypropylene a and impact copolymer polypropylene b; the polypropylene compositions B, B' include random copolymer polypropylene x, and the three-layer polypropylene fabric structure is BAB' from bottom to top.

[0038] According to the present invention, "and / or" means that it can be a situation where any one of the conditions exists alone, or it can be a situation where both conditions exist.

[0039] According to the present invention, the foam sheet (i.e., polypropylene foam motherboard) in the polypropylene composite foam board is also made of polypropylene. In some preferred embodiments of the present invention, the polypropylene foam sheet contains a polypropylene composition, preferably the polypropylene foam sheet contains at least one of the polypropylene composition A, the polypropylene composition B, and the polypropylene composition B', and optional auxiliary agents; preferably, the auxiliary agent is selected from one or more of antioxidants, antistatic agents, lubricants, anti-aging agents, flame retardants, and color powders.

[0040] In the polypropylene composition, the polypropylene composition A and the polypropylene composition B and the polypropylene composition B' can be mixed in any ratio between 0-100.

[0041] The composition may also contain one or more of the following processing aids commonly used in polypropylene foaming processes, such as but not limited to:

[0042] Graphite toner: added amount 1%-8%, preferably 2-5%; antioxidant: added amount 0.1-15‰, preferably 0.1-5‰; antistatic agent: added amount 0.1-10%, preferably 0.5-5%; lubricant: added amount 0.1-10%, preferably 0.5-3%; anti-aging agent: added amount 0.01-5%, preferably 0.1-2%. Flame retardant: added amount 0.1-25%, preferably 1-20%. The content of processing aids is well known in the industry and will not be repeated here.

[0043] According to the present invention, the polypropylene composite foam board has a laminated structure, including at least one layer of reinforced composite sheet and at least one layer of polypropylene foam sheet bonded to the reinforced composite sheet by compression foaming, and the compression foaming is physical foaming.

[0044] In some preferred embodiments of the present invention, the polypropylene foam sheet is foamed by an inorganic physical foaming agent and / or an organic physical foaming agent; preferably, the inorganic physical foaming agent is selected from at least one of air, nitrogen, carbon dioxide, oxygen and water, and / or the organic physical foaming agent is selected from at least one of an aliphatic hydrocarbon foaming agent, an alicyclic hydrocarbon foaming agent, and a halogenated hydrocarbon foaming agent.

[0045] For ease of understanding, as an illustration, the physical foaming agent may be an organic physical foaming agent or an inorganic physical foaming agent. Organic physical foaming agents include but are not limited to aliphatic hydrocarbons such as propane, butane, pentane, hexane and heptane, alicyclic hydrocarbons such as cyclobutane and cyclohexane, and halogenated hydrocarbons such as chlorofluoromethane, trifluoromethane, 1,2-difluoroethane, 1,2,2,2-tetrafluoroethane, methyl chloride, ethyl chloride and dichloromethane. The inorganic physical foaming agent includes but is not limited to at least one of air, nitrogen, carbon dioxide, oxygen and water.

[0046] In some preferred embodiments of the present invention, based on the total thickness of the polypropylene composite foamed board material, the total thickness of the reinforced composite sheet material accounts for 0.5%-5%, preferably 1%-3% of the total thickness of the polypropylene composite foamed board material.

[0047] According to some preferred embodiments of the present invention, the polypropylene composite foam board is prepared by extruding multiple layers of the above-mentioned polypropylene sheet or / and the above-mentioned polypropylene fabric, and the raw material of the polypropylene foam sheet (i.e., the polypropylene foam motherboard raw material), which are jointly prepared by a compression molding foaming process.

[0048] Preferably, the polypropylene fabric and / or the polypropylene sheet are stacked at 0-90° between the warp directions from top to bottom. The polypropylene foam motherboard is stacked at 0-90° along the respective machine directions from top to bottom.

[0049] In a preferred embodiment of the present invention, the polypropylene composition A contained in each stacked layer of polypropylene fabric or polypropylene sheet may be the same or different, and the polypropylene fabric A contained in each layer may be independently selected, and preferably the polypropylene composition A of each layer is the same.

[0050] According to the present invention, the reinforced composite sheet includes at least one layer of polypropylene sheet and / or at least one layer of polypropylene fabric woven from polypropylene sheets, that is, the material formed by the polypropylene sheet and the polypropylene fabric located on one side of the polypropylene foam sheet or between two polypropylene foam sheets is a reinforced composite sheet.

[0051] In some preferred embodiments of the present invention, the polypropylene composite foam board includes a layer of reinforced composite sheet and a layer of polypropylene foam sheet, or the polypropylene composite foam board includes multiple layers of reinforced composite sheets and at least one layer of polypropylene foam sheet; preferably, the outer layers of the polypropylene composite foam board are all reinforced composite sheets.

[0052] In some preferred embodiments of the present invention, the total number of laminated layers of all the polypropylene sheets, polypropylene fabrics and polypropylene foam sheets is 6-35 layers, more preferably 10-20 layers.

[0053] In some preferred embodiments of the present invention, the polypropylene foam sheets are stacked from top to bottom at an angle of 0-90° along their respective machine directions, preferably with 1 to 4 layers, more preferably 1 to 2 layers.

[0054] In some preferred embodiments of the present invention, the reinforced composite sheets are stacked from top to bottom in a 0-90° angle along their respective machine directions, and preferably the total number of layers of polypropylene sheets and polypropylene fabrics in each layer of the reinforced composite sheet is greater than or equal to 5 layers, more preferably 5-30 layers, and more preferably 5-15 layers.

[0055] In some preferred embodiments of the present invention, each layer of the reinforced composite sheet comprises a plurality of sequentially stacked polypropylene sheet unit groups; each polypropylene sheet unit group comprises at least one identical or different polypropylene sheet unit, and each polypropylene sheet unit comprises a core layer A i and located in the core layer A i The outer layer B on both sides i , B' i , structure B i A i B' i The structure of the reinforced composite sheet is nth group...ith group...2nd group, 1st group, 2nd group...ith group...nth group from bottom to top, and the total number of stacked groups of polypropylene sheet unit groups is 2n-1; i and n are both integers not less than 2, and i≤n;

[0056] Among them, the core layer A in the polypropylene sheet unit i Containing polypropylene composition A i , outer layer B i With outer layer B' i The same or different, each corresponding to a polypropylene composition Bi , polypropylene composition B' i ,

[0057] The polypropylene composition A i The melting point is greater than that of the polypropylene composition B i , the polypropylene composition B' i The average melting point of all outer layers in the i-th group is greater than or equal to the average melting point of all outer layers in the i-1-th group.

[0058] According to the present invention, in the structure of the reinforced composite sheet, the upper i-th group and the lower i-th group may be the same or different.

[0059] In some preferred embodiments of the present invention, the polypropylene composition A i Melting point and polypropylene composition B i The difference in melting points, polypropylene composition A i The melting point of polypropylene composition B' i The difference in melting points is respectively greater than or equal to 5°C, preferably greater than or equal to 10°C, more preferably greater than or equal to 20°C; more preferably 20-60°C.

[0060] In some preferred embodiments of the present invention, the difference between the average melting point of all outer layers in the i-th group and the average melting point of all outer layers in the i-1-th group is the same or different, and is each 1-40°C, preferably 1-10°C, and more preferably 1-5°C.

[0061] In some preferred embodiments of the present invention, the total number of stacked polypropylene sheet unit groups is 2n-1, 3≤n≤16, preferably, 3≤n≤8.

[0062] In some preferred embodiments of the present invention, each polypropylene sheet unit group, independently, comprises 1 to 10, preferably 1 to 5 identical or different polypropylene sheet units, more preferably 1 to 3 identical or different polypropylene sheet units, more preferably 1 polypropylene sheet unit. Preferably, the number of polypropylene sheet units included in each polypropylene sheet unit group is the same.

[0063] Preferably, but not necessarily, the melting point of any outer layer in each group is within ±10°C, within ±5°C, preferably within ±3°C, more preferably within ±1°C of the average melting point of all outer layers in the group.

[0064] In the embodiment where each polypropylene sheet unit group includes only one polypropylene sheet unit, for example, the structure of the reinforced composite sheet can be B from bottom to top. n A n B' n ……B i Ai B' i ……B 2 A 2 B' 2 , B 1 A 1 B' 1 , B 2 A 2 B' 2 ……B i A i B' i ……B n A n B' n , the total number of stacked layers of the polypropylene sheet unit is 2n-1; i and n are both integers not less than 2, and i≤n.

[0065] In the embodiment where each polypropylene ply unit group includes 2 or more polypropylene ply units, for example, the structure of the i-th polypropylene ply unit group is B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip The structure of the reinforced composite sheet can be as follows from bottom to top: n1 A n1 B' n1 , B n2 A n2 B' n2 ……B nq A nq B' nq )……(B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip )……(B 21 A 21 B' 21 , B 22 A 22 B' 22 ……B 2k A 2k B' 2k )(B 11 A 11 B' 11 , B 12 A 12 B'12 ……B 1j A 1j B' 1j )(B 21 A 21 B' 21 , B 22 A 22 B' 22 ……B 2k A 2k B' 2k )……(B i1 A i1 B' i1 , B i2 A i2 B' i2 ……B ip A ip B' ip )……(B n1 A n1 B' n1 , B n2 A n2 B' n2 ……B nq A nq B' nq ), the total number of stacked polypropylene sheet units is j+2k+...2p+...2q; j, k, p, q are each independently an integer not less than 2, preferably an integer from 2 to 10, more preferably from 2 to 5, and more preferably from 2 to 3.

[0066] As a preferred embodiment of the polypropylene composite foamed board provided by the present invention, the preparation method of the foamed board comprises: compression foaming, in which a plurality of layers of the above-mentioned polypropylene sheets and / or the above-mentioned polypropylene fabrics are laid on the upper and lower surfaces or a single surface of a board prepared by extruding the above-mentioned polypropylene foam sheet motherboard raw material in a compression foaming device, the layers are stacked in sequence, a physical foaming agent is added under a certain temperature and pressure, and the composite foamed board is foamed.

[0067] That is, the polypropylene composite foam board is prepared by the following method: at least one group of the polypropylene sheets and / or the polypropylene fabrics are stacked with at least one motherboard of the polypropylene foam sheet, and subjected to a compression foaming treatment to obtain the polypropylene composite foam board; the compression foaming treatment adopts physical foaming; wherein each group of the polypropylene sheets and / or the polypropylene fabrics are stacked in the order of forming the corresponding layers of reinforced composite sheets.

[0068] In the present invention, "the polypropylene sheet and / or the polypropylene fabric" refers to one or both of the polypropylene sheet and the polypropylene fabric.

[0069] In some preferred embodiments of the present invention, the conditions for the compression molding and foaming include: a temperature of 140-170°C, preferably 150-163°C, and further preferably 154-159°C; and / or, a pressure of the compression molding and foaming of 4-16MPa, preferably 8-12MPa; and / or, a saturated immersion time of the compression molding and foaming of 0.1-3 hours, preferably 0.3-1.5 hours.

[0070] In some preferred embodiments of the present invention, the polypropylene composite foamed sheet has at least one of the following characteristics:

[0071] The apparent density of the multi-layer polypropylene composite foamed board of the present invention is ≤300 g / l, more preferably ≤90 g / l; most preferably ≤75 g / l. The thickness is between 5 mm and 150 mm, most preferably 20 mm and 100 mm, and most preferably 30 mm and 75 mm.

[0072] According to some embodiments of the present invention, the polypropylene composite foamed board has an apparent density of 60±2 g / l and a thickness of 60±2 mm.

[0073] When the apparent density of the polypropylene composite foamed board is about 60 g / l and the thickness is about 60 mm, the compressive strength (deformation 50%) is ≥ 1 MPa, preferably ≥ 1.2 MPa. The compressive strength is measured according to the method specified in GB / T 8813-2020, and the thickness of the sample is the thickness of the prepared product.

[0074] The thermal insulation capacity of the composite foamed board is compared with the composite foamed board without reinforcement prepared by the same process, and the thermal conductivity is increased by no more than 20%, preferably no more than 10%, and compared with the composite sheet with other reinforcement methods, the thermal conductivity is reduced by 25%, preferably by 40%. Test method: The thermal conductivity is measured according to the method specified in GB / T 10294.

[0075] In the second aspect, the purpose of the present invention is to provide a method for preparing the polypropylene composite foam board material described in the first aspect, comprising laminating the polypropylene sheet material and / or the polypropylene fabric with the base material of the polypropylene foam sheet, and subjecting the laminate to a compression foaming treatment to obtain the polypropylene composite foam board material; the compression foaming treatment adopts physical foaming, wherein all the polypropylene sheets and the polypropylene fabrics are grouped and laminated in the order of forming the reinforced composite sheets of the corresponding layers.

[0076] Preferably, the conditions of the compression foaming treatment are controlled so that the base material of the polypropylene foam sheet is foamed to obtain the polypropylene foam sheet, and preferably the polypropylene sheet and / or the polypropylene fabric are not foamed.

[0077] More preferably, by adding a physical foaming agent during the molding and foaming process, the polypropylene sheet / fabric does not foam but the parent material of the polypropylene foam sheet foams, thereby producing a composite foamed board.

[0078] In a preferred embodiment of the present invention, the temperature of the compression foaming is 140-170°C, preferably 150-162°C, and more preferably 154-159°C.

[0079] In a preferred embodiment of the present invention, the pressure of the compression foaming is 4-16 MPa, preferably 8-12 MPa.

[0080] In a preferred embodiment of the present invention, the saturated immersion time of the compression foaming is 0.1-3 hours, preferably 0.3-1.5 hours.

[0081] In some preferred embodiments of the present invention, the conditions for the compression foaming include: the compression foaming temperature is 140-170°C, preferably 150-163°C, more preferably 150-162°C, and further preferably 154-159°C; and / or, the compression foaming pressure is 4-16MPa, preferably 8-12MPa; and / or,

[0082] The saturated immersion time of the compression foaming is 0.1-3 hours, preferably 0.3-1.5 hours.

[0083] In a preferred embodiment of the present invention, adjacent layers of the polypropylene sheet laminate are placed at 0-90° along respective machine directions, wherein the machine direction is the stretching direction (MD).

[0084] In a preferred embodiment of the present invention, adjacent layers of the polypropylene fabric laminate are placed at an angle of 0-90° along the warp direction.

[0085] Preferably, the total number of layers of all the polypropylene sheets and polypropylene fabrics and the polypropylene foam motherboard is 6-35 layers; more preferably, it is 10-20 layers.

[0086] According to the present invention, preferably, the method for preparing the polypropylene sheet comprises co-extruding, casting or calendering, and stretching the polypropylene composition A, the polypropylene composition B, and the polypropylene composition B' according to the BAB' structure to obtain the polypropylene sheet.

[0087] In a preferred embodiment of the present invention, the preparation of the polypropylene composition A comprises melt blending the components including the homopolypropylene a and the impact copolymer polypropylene b; and / or, the preparation of the polypropylene compositions B and B' comprises melt blending the components including the random copolymer polypropylene x; and / or, the temperatures of the coextrusion and casting are independently selected from 200-240°C; and / or, the temperature of the calendering roll is 50-70°C; and / or, the stretching conditions include: the stretching temperature is 90-165°C, preferably 90-140°C, and more preferably 90-119°C; the stretching ratio is 1-20 times; preferably 1-15 times.

[0088] According to some embodiments of the present invention, polypropylene composition A, polypropylene composition B, polypropylene composition B', according to the BAB' structure, are co-extruded and cast or calendered to obtain a polypropylene co-extruded sheet. The process of the extrusion calendering method may include passing the co-extruded polypropylene sheet through a calendering roller, a traction roller, and then solid phase stretching, trimming and winding to obtain the sheet. The temperature of the extrusion casting is 200-230°C, and the temperature of the calendering roller is 50-70°C. The specific process of preparing the film by the extrusion calendering method is a commonly used choice in the art and will not be repeated here.

[0089] According to the present invention, preferably, the polypropylene fabric is a three-dimensional polypropylene fabric obtained by weaving the polypropylene sheet as described above; preferably, the polypropylene fabric has a three-dimensional structure of plain, twill and / or satin.

[0090] In order to facilitate weaving, the polypropylene sheet is preferably cut into polypropylene sheets with a width of 2-5 mm, and then the polypropylene fabric is obtained by weaving.

[0091] In a more preferred embodiment of the present invention, the polypropylene fabric is a plain, twill, satin or three-dimensional polypropylene fabric obtained by weaving three-layer co-extruded polypropylene stretch flat tape, and the three-layer co-extruded polypropylene stretch flat tape includes layer A formed by a high-melting point polypropylene combination A and layers B, B' formed by low-melting point polypropylene compositions B, B', wherein the polypropylene composition A includes homopolymer polypropylene a and impact copolymer polypropylene b; the polypropylene compositions B, B' include random copolymer polypropylene x, and the three-layer polypropylene fabric structure is BAB' from bottom to top.

[0092] The third aspect of the present invention is to provide an application of the polypropylene composite foamed board described in the first aspect or the polypropylene composite foamed board prepared by the preparation method described in the second aspect in materials used in at least one of the following fields: automobiles, communications, aircraft, logistics, insulation, precision machinery and electronic turnover, and packaging.

[0093] As described in the background technology, compression molding physical foaming has many advantages, but the physical properties of the polypropylene foamed board obtained by compression molding physical foaming of a simple polypropylene base material need to be further optimized to improve the physical properties of the polypropylene foamed board products. At present, compounding inorganic or organic reinforced boards (such as glass fiber / carbon fiber reinforced thermoplastic resin) on the surface of polypropylene foamed boards is an existing recommended means. However, this type of polypropylene foamed composite board has many problems. Conventional polypropylene sheets as reinforced boards either do not meet the requirements in strength and cannot obtain polypropylene composite foamed boards with compression strength that meets the requirements, or are not suitable for compression molding foaming. For example, the overall properties change during compression molding foaming, and a composite foamed board of qualified quality cannot be obtained. After research, the inventors of the present invention unexpectedly found that the present invention forms a reinforced composite sheet through a specific polypropylene sheet / fabric, and unexpectedly obtains a composite foamed board with better performance through specific compression molding physical foaming, and no additional thermal bonding enhancer is required. As described above, the polypropylene composite foamed board material of the present invention has a laminated structure, including at least one layer of reinforced composite sheet and at least one layer of polypropylene foamed sheet bonded to the reinforced composite sheet by compression foaming; each layer of the reinforced composite sheet includes at least one layer of polypropylene sheet and / or at least one layer of polypropylene fabric woven from polypropylene sheets; wherein the polypropylene sheet includes layer A and layers B and B' located on both sides of layer A, and the structure is BAB'; wherein layer A contains a polypropylene composition A, wherein the polypropylene composition A includes homopolymer polypropylene a and impact copolymer polypropylene b; layer B is the same as or different from layer B', and each correspondingly contains a polypropylene composition B and a polypropylene composition B', wherein the polypropylene composition B and the polypropylene composition B' each include a random copolymer polypropylene x; wherein the melting point of the polypropylene composition A is greater than the melting point of the polypropylene composition B and the polypropylene composition B'; and the compression foaming is physical foaming.

[0094] According to the above technical scheme, the present invention utilizes the technical characteristics of the molded foaming process, and the reinforced sheet (i.e., the reinforced composite sheet) is overlapped with the foamed motherboard (i.e., the motherboard of the polypropylene foamed sheet) before compounding, and the reinforced sheet and the foamed motherboard undergo physical foaming together, preferably undergoing an impregnation process of carbon dioxide under a certain temperature and pressure, and preferably by controlling the production conditions, the crystallization and orientation of the polypropylene reinforced composite sheet are maintained while the motherboard is foaming, and only thermal fusion occurs at the junction of the reinforced composite sheet and the polypropylene foamed sheet. The present invention forms a reinforced composite sheet through a specific polypropylene sheet / fabric, and realizes the foaming of the motherboard of the polypropylene foamed sheet through specific molded physical foaming, while plasticizing the surface of the above-mentioned reinforced composite sheet, thereby obtaining a composite foamed board with better performance, and no additional thermal bonding enhancer needs to be added. And because the raw materials of the composite foamed board are uniform, it can be directly crushed, melted and reused, reducing the recycling cost.

[0095] Compared with the prior art, the present invention has the following beneficial effects:

[0096] (1) The polypropylene composite foamed board provided by the present invention is a board made of a high-strength and high-impact polypropylene sheet and a foamed board through a molding foaming process, so that the polypropylene sheet / sheet composition / fabric does not foam but the board prepared by the polypropylene composition foams, and the polypropylene sheet / fabric and the foamed board have good compressive strength at the same time; the polypropylene composite foamed board has the following characteristics:

[0097] When the polypropylene composite foamed board is obtained by molding and foaming 10 layers of polypropylene fabric and 1 layer of polypropylene foamed board motherboard, and the thickness is about 60mm, the compression strength (deformation 50%) is ≥1MPa, preferably ≥1.2MPa; and it has excellent thermal insulation performance.

[0098] The multi-layer polypropylene composite foamed board of the present invention has an apparent density of ≤300 g / l, more preferably ≤90 g / l, and most preferably ≤75 g / l. The thickness is between 5 mm and 150 mm, most preferably 20 mm and 100 mm, and most preferably 30 mm and 75 mm.

[0099] The thermal insulation capacity of the composite foamed board is compared with the unreinforced board composite foamed board prepared by the same process, and the thermal conductivity coefficient is increased by no more than 20%, preferably no more than 10%. Compared with composite sheets with other reinforcement methods, the thermal conductivity coefficient is reduced by 25%, preferably 40%.

[0100] (2) Compared with the glass fiber nylon composite pre-formed board or metal board reinforced molded body used in the currently common composite reinforced polypropylene composite foam board, the compatibility between the pre-formed board and the matrix resin is greatly improved, which can effectively reduce the apparent density and thermal conductivity of the product.

[0101] (3) Compared with the currently common polypropylene composite sheet reinforced polypropylene composite foam board, the present invention does not require the addition of an additional adhesion enhancer, and thus can have more ideal physical properties.

[0102] (4) The polypropylene foamed board of the present invention can be prepared by using existing foaming and molding processes, and can be prepared with different properties by using different process methods and different types of foaming agents according to the needs of downstream applications.

[0103] (5) The polypropylene composite foamed board of the present invention is a uniform component and does not require separation treatment during recycling. It can be directly used in other processing and application fields after crushing, melting and granulation.

[0104] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0105] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0106] In the following examples and comparative examples:

[0107] The extrusion calender and solid phase drawing equipment were purchased from Tianjin Hengrui Company, and the model is HRPC-800 three-layer co-extrusion plastic stretching sheet production line.

[0108] The polypropylene composition and sheet properties are tested according to the following methods:

[0109] The test results of composite sheets are shown in Table 1:

[0110] (1) Melt flow rate (MFR): measured according to the method specified in GB / T 3682, where the test temperature is 230°C and the load is 2.16 kg;

[0111] (2) Density: measured according to the methods specified in GB / T 1033.1 and GB / T 6343;

[0112] (3) Melting point: measured according to the method specified in GB / T 28724;

[0113] (4) Test method for thermal insulation capacity of the composite foam board: The thermal conductivity is measured according to the method specified in GB / T 10294.

[0114] In the following examples, the β-crystal nucleating agent with the brand name VP101B is sourced from Beijing Research Institute of Chemical Industry of Sinopec Corporation; the sources of some raw materials are described in the examples, and the other raw materials are commercially available unless otherwise specified.

[0115] Example 1

[0116] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition and polypropylene composition composite foamed board provided by the present invention.

[0117] (1) Preparation of polypropylene composition A:

[0118] Component a is a homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 160°C, a melt flow rate (melt mass flow rate) of 3.2g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry, with an ethylene content of 11wt%, a melting point of 155°C, and an Izod impact strength of 23KJ / m 2 (23°C), the melt flow rate is 2.0 g / 10 min. The components prepared above are weighed and mixed according to the proportions, wherein the mass fraction Wa of component a is 80 parts by weight, and the mass fraction Wb of component b is 20 parts by weight.

[0119] 0.05 parts by weight of a β-crystal nucleating agent of grade VP101B was added. The mixture was then added to a high-speed stirrer for uniform mixing, and then the mixed material was added to the feeder of a twin-screw extruder manufactured by W&P Company, and the material entered the twin screw through the feeder. During the processing, the temperature of the screw was maintained between 200-230° C. The screw was melt-mixed uniformly, extruded, granulated and dried to obtain a polypropylene composition pellet A. The melting point of the polypropylene composition pellet A was found to be 157° C.

[0120] (2) Polypropylene composition B i Preparation:

[0121] Component x1 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution Mw / Mn of 8.9, a melt flow rate of 8.1 g / 10 min and a melting point of 130°C; component x2 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution Mw / Mn of 7.6, a melt flow rate of 7.2 g / 10 min and a melting point of 135°C; component x3 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution Mw / Mn of 7.3, a melt flow rate of 6.6 g / 10 min and a melting point of 140°C.

[0122] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0123] The polypropylene composition A and the polypropylene composition B obtained in the above steps (1) and (2) are i The pellets are dried, and then the polypropylene composition A is added to the core layer extruder of the multi-layer extrusion calendering, and the polypropylene composition B is added to the core layer extruder of the multi-layer extrusion calendering. i Add the pellets to the upper and lower surface extruders of the multi-layer extrusion casting machine. After the pellets are co-extruded and compounded through the extruder die, they pass through the calendering roller and the traction roller in sequence, and then undergo solid phase stretching, trimming and winding to obtain sheet B. 1 AB1 , B 2 AB 2 , B 3 AB 3 The temperature of the extrusion casting was 230°C, and the temperature of the calendering roller was 58°C. The temperature during the solid phase stretching process was 140°C, the stretching rate was 2m / min, and the stretching ratio was 7 times.

[0124] The composite film (polypropylene sheet) made by stretching and rolling is composed of the upper surface layer (the outer layer of the film B i ), core layer (film A) and lower surface layer (outer film B i The thickness of the composite film is 80 μm, wherein the thickness of the film layer A accounts for 80% of the total thickness of the sheet.

[0125] (4) Preparation of polypropylene fabric:

[0126] The three-layer co-extruded polypropylene sheet obtained in the above step (3) was cut by a high-speed slitting machine with multiple blades to obtain an oriented polypropylene flat ribbon with a width of 3 mm; the oriented flat ribbon was woven by a commercial weaving machine according to the designed fabric structure to obtain a plain weave polypropylene fabric B 1 AB 1 , B 2 AB 2 , B 3 AB 3 .

[0127] (5) Preparation of polypropylene composition for foamed sheet:

[0128] 5 kg of the polypropylene composition A prepared in step (1) and 5 kg of the polypropylene B3 pellets prepared in step (2) were added with 30 g of antioxidant 1010, 100 g of 2000 mesh commercial talc as a nucleating agent, and 200 g of commercial graphite color powder, and mixed in a high-speed mixer for 3 minutes. The mixture was extruded and pelletized using a twin-screw extruder at a die temperature of 220° C., a screw speed of 300 rpm, and a torque of 60% to obtain a polypropylene mixture AB. i -1. Its melt mass flow rate MFRB was detected to be 5 g / 10 min, and its melting point was 151° C. The above composition was extruded by a single screw or twin screw extruder to obtain a molded foamed motherboard with a specification of 1000 mm*500 mm*20 mm.

[0129] (6) Preparation of composite polypropylene foamed sheet

[0130] The mold installed between the molding machines is heated to a foaming temperature of 158°C, a foamed motherboard prepared by extruding the polypropylene composition in step (5) is placed therein, and the polypropylene fabrics prepared in step (4) are stacked in sequence, from bottom to top, B 3 AB3 , B 2 AB 2 , B 1 AB 1 , B 2 AB 2 , B 3 AB 3 The total number of stacked layers is 5, and the upper and lower motherboards are covered with a group of 2000mm*1200mm 5-layer stacked polypropylene fabrics, and the placement direction is 90° between the warp and the warp. The molding machine is closed and the mold is sealed. Supercritical carbon dioxide is diffused into the polypropylene composition resin sheet as a foaming agent, and the foaming pressure is 10.5MPa. After reaching the process temperature and pressure, constant temperature and constant pressure saturation for 1 hour, the diffusion equilibrium is reached, and the pressure is released once through the pressure relief valve to open the mold for foaming, cooled and shaped, and the uneven four sides are cut off to obtain a composite polypropylene foam sheet with a thickness of 60.11mm and a density of 60.0g / L. Among them, the total thickness of the reinforced composite sheet is 0.77mm.

[0131] Example 2

[0132] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition and polypropylene composition composite foamed board provided by the present invention.

[0133] (1) Preparation of polypropylene composition A:

[0134] Component a is homopolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, with a melting point of 165°C, a melt flow rate of 8.1g / 10min, and an isotacticity of 97%; component b is a polypropylene impact copolymer produced by Sinopec Beijing Research Institute of Chemical Industry, with an ethylene content of 8wt%, a melting point of 155°C, a melt flow rate of 3.2g / 10min, and an cantilever beam impact strength of 25KJ / m 2 (23°C). The above-prepared components are weighed and mixed according to the proportion, wherein the mass fraction Wa of component a is 70 parts by weight, and the mass fraction Wbn of component b is 30 parts by weight. 0.05 parts by weight of β-crystal nucleating agent with the grade VP101B is added. Then the mixture is added to a high-speed stirrer and mixed evenly, and then the mixed material is added to the feeder of a twin-screw extruder manufactured by W&P. The material enters the twin screw through the feeder. During the processing, the temperature of the screw is maintained between 200-230°C. After the screw is melt-mixed evenly, extruded, granulated and dried, a polypropylene composition pellet A is obtained. After testing, the melting point of the polypropylene composition pellet A is 161°C.

[0135] (2) Polypropylene composition B i Preparation:

[0136] Component x1 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution of Mw / Mn of 8.4, a melting point of 128°C, and a melt flow rate of 7.8 g / 10 min; component x2 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution of Mw / Mn of 7.6, a melting point of 134°C, and a melt flow rate of 6.9 g / 10 min; component x3 is a random copolymer polypropylene produced by Sinopec Beijing Research Institute of Chemical Industry, which is an ethylene-propylene-butene terpolymer with a molecular weight distribution of Mw / Mn of 7.1, a melting point of 142°C, and a melt flow rate of 5.2 g / 10 min.

[0137] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0138] The preparation process is the same as step (3) of Example 1.

[0139] (4) Preparation of polypropylene fabric:

[0140] The preparation process is the same as step (4) of Example 1.

[0141] (5) Preparation of polypropylene composite materials:

[0142] The preparation process is the same as step (5) of Example 1.

[0143] The thickness of the prepared polypropylene composite material is close to that of Example 1.

[0144] (5) Preparation of polypropylene composition for foamed sheet:

[0145] The preparation process is the same as step (5) of Example 1 to obtain a polypropylene mixture ABi-2, wherein B i In this embodiment, B 3 The melt mass flow rate MFRB was detected to be 6.8 g / 10 min and the melting point was 158°C.

[0146] (6) Preparation of composite polypropylene foamed sheet

[0147] The preparation process is the same as step (6) of Example 1, except that the polypropylene composition AB prepared in step (6) is i -2 is the base resin. The thickness and density of the prepared composite polypropylene foamed board are close to those in Example 1.

[0148] Example 3

[0149] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition and polypropylene composition composite foamed board provided by the present invention.

[0150] (1) Preparation of polypropylene composition A:

[0151] The preparation process is the same as step (1) of Example 1.

[0152] (2) Polypropylene B i Preparation:

[0153] The preparation process is the same as step (2) of Example 1.

[0154] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0155] The main steps are the same as those of Example 1. The thickness of the polypropylene sheet is 80 μm, wherein the thickness of the film layer A accounts for 90% of the total thickness of the sheet.

[0156] (4) Preparation of polypropylene fabric:

[0157] The preparation process is the same as step (4) of Example 1.

[0158] (5) Preparation of polypropylene composition for foamed sheet:

[0159] The preparation process is the same as step (5) of Example 1.

[0160] (6) Preparation of composite polypropylene foamed sheet

[0161] The preparation process is the same as step (6) of Example 1. The thickness and density of the prepared polypropylene composite foamed board are close to those of Example 1.

[0162] Example 4

[0163] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition and polypropylene composition composite foamed board provided by the present invention.

[0164] (1) Polypropylene composition A i Preparation:

[0165] The preparation process is the same as step (1) of Example 1.

[0166] (2) Polypropylene B i Preparation:

[0167] The preparation process is the same as step (2) of Example 1.

[0168] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0169] The main preparation process is the same as step (3) of Example 1, wherein the stretching ratio of the plate is 10 times.

[0170] (4) Preparation of polypropylene fabric:

[0171] The preparation process is the same as step (4) of Example 1.

[0172] (5) Preparation of polypropylene composition for foamed sheet:

[0173] The preparation process is the same as step (5) of Example 1.

[0174] (6) Preparation of composite polypropylene foamed sheet

[0175] The preparation process is the same as step (6) of Example 1. The thickness and density of the prepared polypropylene composite foamed board are close to those of Example 1.

[0176] Example 5

[0177] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition and polypropylene composition composite foamed board provided by the present invention.

[0178] (1) Polypropylene composition A i Preparation:

[0179] The preparation process is the same as step (1) of Example 1.

[0180] (2) Polypropylene B i Preparation:

[0181] The preparation process is the same as step (2) of Example 1.

[0182] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0183] The preparation process is the same as step (3) of Example 1.

[0184] (4) Preparation of polypropylene fabric:

[0185] The preparation process is the same as step (4) of Example 1.

[0186] (5) Preparation of polypropylene composition for foamed sheet:

[0187] The preparation process is the same as step (5) of Example 1, except that the foamed mother board prepared from the composition of step (5) is prepared with a specification of 1000mm*500mm*10mm.

[0188] (6) Preparation of composite polypropylene foamed sheet

[0189] The preparation process is the same as step (6) of Example 1. The difference is that the polypropylene fabrics obtained in step (4) are stacked in order, from bottom to top: B 3 AB 3 , B 2 AB 2 , B 1 AB 1 , B 2 AB 2 , B 3 AB 3 The total number of stacked layers is 5. A group of 2000mm*1200mm 5-layer stacked polypropylene fabrics are covered in the middle and lower parts of the two motherboards, and the placement direction is 90° between the warp and the warp. The molding machine is closed and the mold is sealed. Supercritical carbon dioxide is used as a foaming agent to diffuse into the polypropylene composition resin sheet: temperature 160℃, foaming pressure 12MPa. After reaching the process temperature and pressure, constant temperature and constant pressure saturation for 1.3 hours, diffusion equilibrium is reached, and the pressure is released once through the pressure relief valve to open the mold for foaming, cooled and shaped, and the uneven four sides are cut off to obtain a composite polypropylene foam sheet with a thickness of 61.2mm and a density of 61.8g / L. Among them, the total thickness of the reinforced composite sheet is 1.13mm.

[0190] Example 6

[0191] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition and polypropylene composition composite foamed board provided by the present invention.

[0192] (1) Polypropylene composition A i Preparation:

[0193] The preparation process is the same as step (1) of Example 1.

[0194] (2) Polypropylene B i Preparation:

[0195] The preparation process is the same as step (2) of Example 1.

[0196] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0197] The preparation process is the same as step (3) of Example 1.

[0198] (4) Preparation of polypropylene composition for foamed sheet:

[0199] The preparation process is the same as step (5) of Example 1.

[0200] (5) Preparation of polypropylene composite foamed sheet:

[0201] The preparation process is the same as step (6) of Example 1.

[0202] Instead of preparing the polypropylene fabric, the three-layer co-extruded polypropylene sheet prepared in step (3) was used to replace the polypropylene fabric obtained in step (4) of Example 1, and the three-layer co-extruded polypropylene sheet was laminated in sequence according to step (5) of Example 1 and then subjected to compression foaming. The thickness and density of the prepared polypropylene composite foamed board were close to those of Example 1.

[0203] Example 7

[0204] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition and polypropylene composition composite foamed board provided by the present invention.

[0205] (1) Preparation of polypropylene composition A:

[0206] The preparation process is the same as step (1) of Example 1.

[0207] (2) Polypropylene B i Preparation:

[0208] The preparation process is the same as step (2) of Example 1.

[0209] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0210] The preparation process is the same as step (3) of Example 1.

[0211] (4) Preparation of polypropylene fabric:

[0212] The preparation process is the same as step (4) of Example 1.

[0213] (5) Preparation of polypropylene composition for foamed sheet:

[0214] The preparation process is the same as step (5) of Example 1. The preparation process is the same as step (6) of Example 1, except that 0.5 kg of the polypropylene composition A prepared in step (1) and 9.5 kg of the polypropylene B3 pellets prepared in step (2) are taken. The melt mass flow rate MFRA is detected to be 6.0 g / 10 min; the melting point of the polypropylene composition Abi-3 is 141°C.

[0215] (6) Preparation of composite polypropylene foamed sheet

[0216] The preparation process is the same as step (6) of Example 1. The difference is that the compression foaming conditions used are: temperature 150°C, pressure 7MPa, and saturated immersion time 30 minutes. The thickness and density of the prepared polypropylene composite foamed board are close to those of Example 1.

[0217] Example 8

[0218] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition and polypropylene composition composite foamed board provided by the present invention.

[0219] (1) Preparation of polypropylene composition A:

[0220] The preparation process is the same as step (1) of Example 1.

[0221] (2) Polypropylene B i Preparation:

[0222] The preparation process is the same as step (2) of Example 1.

[0223] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0224] The preparation process is the same as step (3) of Example 1.

[0225] (4) Preparation of polypropylene fabric:

[0226] The preparation process is the same as step (4) of Example 1.

[0227] (5) Preparation of polypropylene composition for foamed sheet:

[0228] The preparation process is the same as step (6) of Example 1, except that 9.5 kg of the polypropylene composition A prepared in step (1) and the polypropylene B prepared in step (2) are taken. i The pellets weigh 0.5 kg and the melt mass flow rate MFR is 5.2 g / 10 min. The melting point of the polypropylene composition Abi-4 is 156°C.

[0229] (6) Preparation of composite polypropylene foamed sheet

[0230] The preparation process is the same as step (6) of Example 1. The difference is that the compression foaming conditions used are: temperature 161°C, pressure 13 MPa, and saturated immersion time 75 minutes. The thickness and density of the prepared polypropylene composite foamed board are close to those of Example 1.

[0231] Example 9

[0232] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition and polypropylene composition composite foamed board provided by the present invention.

[0233] (1) Preparation of polypropylene composition A:

[0234] The preparation process is the same as step (1) of Example 1.

[0235] (2) Polypropylene Bi Preparation:

[0236] The preparation process is the same as step (2) of Example 1.

[0237] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0238] The preparation process is the same as step (3) of Example 1.

[0239] (4) Preparation of polypropylene fabric:

[0240] The preparation process is the same as step (4) of Example 1.

[0241] (5) Preparation of polypropylene composition for foamed sheet:

[0242] The preparation process is the same as step (5) of Example 1, except that the foamed mother board prepared from the composition of step (5) is prepared with a specification of 1000mm*500mm*5mm.

[0243] (6) Preparation of composite polypropylene foamed sheet

[0244] The preparation process is the same as step (6) of Example 1. The difference is that four foamed mother boards prepared in step 5 of this example are taken and the polypropylene fabrics prepared in step (4) are stacked in sequence, from bottom to top, B 3 AB 3 , B 2 AB 2 , B 1 AB 1 , B 2 AB 2 , B 3 AB 3 , the total number of stacked layers is 5, four motherboards are cross-stacked with 5 groups of 2000mm*1200mm 5-layer stacked polypropylene fabrics, and the placement direction is 90° between the warp and the warp. The molding machine is closed and the mold is sealed. Supercritical carbon dioxide is diffused into the polypropylene composite resin sheet as a foaming agent: temperature 162℃, foaming pressure 13MPa. After reaching the process temperature and pressure, constant temperature and constant pressure saturation for 1.4 hours, diffusion equilibrium is reached, and the pressure is released once through the pressure relief valve to open the mold for foaming, cooled and shaped, and the uneven four sides are cut off to obtain a composite polypropylene foam sheet with a thickness of 61.0mm and a density of 64.1g / L. Among them, the total thickness of the reinforced composite sheet is 1.92mm. .

[0245] Example 10

[0246] This example is used to illustrate the preparation of the polypropylene composition, three-layer co-extruded polypropylene sheet, polypropylene fabric, polypropylene composite material, polypropylene composition and polypropylene composition composite foamed board provided by the present invention.

[0247] (1) Preparation of polypropylene composition A:

[0248] The preparation process is the same as step (1) of Example 1.

[0249] (2) Polypropylene B i Preparation:

[0250] The preparation process is the same as step (2) of Example 1.

[0251] (3) Preparation of three-layer co-extruded polypropylene sheet:

[0252] The preparation process is the same as step (3) of Example 1.

[0253] (4) Preparation of polypropylene fabric:

[0254] The preparation process is the same as step (4) of Example 1.

[0255] (5) Preparation of polypropylene composition for foamed sheet:

[0256] The preparation process is the same as step (5) of Example 1.

[0257] (6) Preparation of composite polypropylene foamed sheet

[0258] The preparation process is the same as step (6) of Example 1.

[0259] (7) Preparation of polypropylene composite foamed sheet:

[0260] The preparation process is the same as step (7) of Example 1. The difference is that 10 pieces of polypropylene fabric are prepared in step (4), with B 3 AB 3 , B 2 AB 2 , B 1 AB 1 , B 2 AB 2 , B 3 AB 3 , B 3 AB 3 , B 2 AB 2 , B 1 AB 1 , B 2 AB 2 , B 3 AB 3 The thickness and density of the prepared polypropylene composite foamed board are close to those in Example 1.

[0261] Comparative Example 1

[0262] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 1, except that only the polypropylene composition A was used for extrusion casting into a single-layer film with a thickness of 80 μm.

[0263] Polypropylene fabric was prepared according to the method of Example 1.

[0264] The preparation process of the polypropylene composition for foaming board is the same as step (5) of Example 1, except that only polypropylene composition A is used. i The preparation process of the composite polypropylene foamed sheet is the same as step (6) of Example 1, and the compression foaming conditions are: temperature 160°C, pressure 13MPa, and saturation immersion time 1 hour. The thickness and density of the prepared composite polypropylene foamed sheet are close to those of Example 1.

[0265] Comparative Example 2

[0266] A three-layer co-extruded polypropylene sheet was prepared according to the method of Example 1. i The extrusion casting was a single-layer film with a thickness of 80 μm.

[0267] Polypropylene fabric was prepared according to the method of Example 1.

[0268] The preparation process of the polypropylene composition for foaming board is the same as step (5) of Example 1, except that only polypropylene B is used. 3 The preparation process of the composite polypropylene foamed board is the same as step (6) of Example 1, but a qualified composite polypropylene foamed board cannot be obtained.

[0269] Comparative Example 3

[0270] A three-layer coextruded polypropylene sheet was prepared according to the method of Example 1, except that the polypropylene composition A contained only component b.

[0271] Polypropylene fabric was prepared according to the method of Example 1.

[0272] The preparation process of the polypropylene composition for foaming board is the same as step (5) of Example 1, except that only polypropylene composition A is used. i The composite polypropylene foamed sheet is prepared in the same manner as step (6) of Example 1 to obtain a composite polypropylene foamed sheet having a thickness and density close to those of Example 1.

[0273] Comparative Example 4

[0274] According to the method of Example 1, a three-layer co-extruded polypropylene sheet and a polypropylene fabric were prepared.

[0275] The preparation process of the polypropylene composition for the foamed board is the same as step (5) of Example 1, and the preparation process of the composite polypropylene foamed board is the same as step (6) of Example 1. The mold compression foaming conditions adopted are: temperature 138°C, pressure 3.5MPa, and saturation immersion time 3 hours. As a result, the mother board failed to foam and no qualified product could be obtained.

[0276] Comparative Example 5

[0277] According to the method of Example 1, a three-layer co-extruded polypropylene sheet and a polypropylene fabric were prepared.

[0278] The preparation process of the polypropylene composition for the foamed board was the same as step (5) of Example 1, and the preparation process of the composite polypropylene foamed board was the same as step (6) of Example 1. The mold foaming conditions adopted were: temperature 172°C, pressure 18 MPa, and saturation immersion time 30 minutes. As a result, the polypropylene fabric and the mother board were completely melted, and no qualified products could be obtained.

[0279] Comparative Example 6

[0280] According to the method of Example 1, a three-layer co-extruded polypropylene sheet and a polypropylene fabric were prepared.

[0281] The preparation process of the polypropylene composition for the foamed plate is the same as step (5) of Example 1, and the preparation process of the composite polypropylene foamed plate is the same as step (6) of Example 1. The mold foaming conditions adopted are: temperature 165°C, pressure 15MPa, and saturation immersion time 200 minutes. As a result, the polypropylene fabric is completely melted, and the apparent density is 27.6g / l. The surface is uneven, with the highest point being 71mm and the lowest point being 54mm. The relatively flat position of the foamed product is selected for sampling.

[0282] Comparative Example 7

[0283] The preparation process of the polypropylene composition for the foamed plate is the same as step (5) of Example 1, and the preparation process of the composite polypropylene foamed plate is the same as step (6) of Example 1, except that no sheet is added. The polypropylene composition foamed plate is prepared by step (6), and the mold foaming conditions adopted are: temperature 156°C, pressure 9MPa, and saturated immersion time 1 hour. The thickness and density of the prepared polypropylene composite foamed plate are close to those of Example 1. The thickness and density are close to those of Example 1.

[0284] Comparative Example 8

[0285] According to the method of Example 1, a three-layer co-extruded polypropylene sheet and a polypropylene fabric were prepared.

[0286] The preparation process of the polypropylene composition for foaming board is the same as step (5) of Example 1, except that 8 parts of chemical AC foaming agent (Cellcom AC7000F, Korea Jinyang, decomposition temperature 210°C) are added when the mother board is extruded, and the preparation process of the composite polypropylene foaming board is the same as step (6) of Example 1. The mold compression foaming conditions adopted are: temperature 159°C, pressure 12MPa, saturation immersion time 90 minutes. As a result, the foaming agent was not decomposed and the mother board failed to foam.

[0287] Comparative Example 9

[0288] According to the method of Example 1, a three-layer co-extruded polypropylene sheet and a polypropylene fabric were prepared.

[0289] The preparation process of the polypropylene composition for foaming board is the same as step (5) of Example 1, except that 8 parts of chemical AC foaming agent (Cellcom AC7000F, Korea Jinyang) are added when the mother board is extruded, and the preparation process of the composite polypropylene foaming board is the same as step (6) of Example 1. The mold compression foaming conditions adopted are: temperature 210°C, pressure 8MPa, and saturation immersion time 30 minutes. As a result, the foaming mother board was completely melted at the process temperature, the foaming failed, and no qualified product could be obtained.

[0290] Comparative Example 10

[0291] The preparation process of the polypropylene composition for the foamed board is the same as step (5) of Example 1, and the preparation process of the composite polypropylene foamed board is the same as step (6) of Example 1, except that two square glass fiber / nylon composite sheets with a thickness of 1.7 mm are placed above and below a polypropylene composition motherboard prepared in step (5), to obtain a polypropylene composition composite foamed board, the thickness and density of which are close to those in Example 1, but the glass fiber / nylon composite sheet is not composited with the foamed board, and a composite material cannot be obtained.

[0292] Comparative Example 11

[0293] A polypropylene foam plate with an apparent density of 60.2 g / l and a thickness of 60.2 mm was prepared in the manner of Comparative Example 7. Two square glass fiber / nylon composite sheets with a thickness of 1.7 mm were placed above and below the sheet and composited by hot pressing (the process is well known in the industry and will not be described in detail) to obtain a composite polypropylene foam plate with a density of 97.5 g / l and a thickness of 63.0 mm.

[0294] Comparative Example 12

[0295] According to the method of Example 1, a three-layer co-extruded polypropylene sheet and a polypropylene fabric were prepared.

[0296] According to the method of comparative example 7, a polypropylene foam plate with an apparent density of 52.0 g / l and a thickness of 59.4 mm was prepared. The woven fabrics were placed above and below them respectively, and a composite polypropylene foam plate with a density of 56.2 g / l and a thickness of 60.2 mm was obtained by hot pressing (the process is well known in the industry and will not be described in detail). It can be seen with the naked eye that there are obvious gaps between the fabrics and between the fabrics and the foam plate.

[0297] Comparative Example 13

[0298] According to the method of Example 9, a three-layer coextruded polypropylene sheet and a polypropylene fabric were prepared.

[0299] The preparation process of the polypropylene composition for the foamed board is the same as step (5) of Example 9, and the preparation process of the composite polypropylene foamed board is the same as step (6) of Example 9. The difference is that 5 foamed mother boards are cross-stacked with 6 groups of 2000mm*1200mm 5-layer laminated polypropylene fabrics. As a result, it can be seen with the naked eye that there are obvious gaps between different layers of fabric and the foamed mother board, and the foamed mother board cannot be uniformly foamed, and a qualified composite material is not obtained.

[0300] Experimental example

[0301] The polypropylene composite foamed board obtained in the above examples and comparative examples was tested according to the following method. The test results are shown in Table 1.

[0302] (1) Compression strength: measured according to the method specified in GB / TGB / T 8813-2020.

[0303] (2) The apparent density of the composite foam board shall be prepared and measured according to the method specified in GB / T6343.

[0304] (3) The thermal conductivity of composite foamed board shall be prepared and measured according to the method specified in GB / T 10294.

[0305] Table 1

[0306]

[0307]

[0308] From the results of the examples in Table 1, it can be seen that compared with the common foamed board without composite reinforcement in Comparative Example 7, the composite polypropylene foamed board prepared according to the present invention has good compression resistance after one-time molding by the compression foaming process, and its thermal insulation capacity will not be significantly reduced. i The ratio has no significant effect on the performance of the final product.

[0309] It can be seen from Comparative Examples 1-3 that only using a single-layer board structure, a single polypropylene component or using an interlayer ratio outside the scope of the embodiment will lead to a decrease in the performance of the laminated polypropylene sheet or fabric, thereby causing a decrease in various properties of the final composite foam board.

[0310] From Examples 5, 6, and 9, it can be seen that the amount of polypropylene fabric and the amount of foamed sheet have a significant impact on the final product. As the amount of fabric and the amount of foamed sheet increase, the physical properties are improved. From Comparative Example 13, it can be seen that when the number of added sheets is too high, it is difficult to obtain a foamed product of qualified quality.

[0311] It can be seen from Example 10 that changing the stacking order of the polypropylene fabric and the foamed board has little effect on the physical properties of the composite foamed board.

[0312] It can be seen from Comparative Examples 4, 5, and 6 that the molding foaming temperature, pressure, and immersion time all need to be controlled within an ideal range. If the temperature and pressure are too low, the motherboard cannot foam. If the temperature and pressure are too high, the sheet and the motherboard will melt at the same time. If the immersion time is too long, the polypropylene fabric will melt, and it will be impossible to obtain a composite foamed board of qualified quality.

[0313] It can be seen from Comparative Examples 8 and 9 that the processing window of the chemical foaming agent and the polypropylene compression foaming process do not overlap at all, and the present invention can only use physical foaming agents.

[0314] From Comparative Examples 10 and 11, it can be seen that other types of reinforced sheets cannot be compounded through the compression foaming process. Although they can be compounded through conventional hot pressing processes and have excellent tensile and compression resistance, the weight reduction effect and thermal insulation capacity will be greatly reduced.

[0315] From Comparative Example 12, it can be seen that the conventional hot pressing process is used to compound the reinforced sheet of the present invention and the blank foamed board without adding the bonding enhancer, and the effect is not ideal, and all the properties are greatly reduced. In the mold pressing foaming process of this patent, carbon dioxide can plasticize the surface of the multilayer sheet under high temperature and high pressure, so it can be formed without the addition of the thermal bonding enhancer.

[0316] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

[0317] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

Claims

1. A polypropylene composite foamed board having a laminated structure, comprising at least one layer of a reinforced composite sheet and at least one layer of a polypropylene foamed sheet bonded to the reinforced composite sheet by molded foaming; Each layer of the reinforced composite sheet comprises at least one layer of polypropylene sheet and / or at least one layer of polypropylene fabric woven from polypropylene sheets; wherein, The polypropylene sheet comprises a layer A and layers B and B' located on both sides of the layer A, and has a structure of BAB'; wherein layer A comprises a polypropylene composition A, wherein the polypropylene composition A comprises a homopolymer polypropylene a and an impact copolymer polypropylene b; Layer B and layer B' are the same as or different from each other, and each layer contains a polypropylene composition B and a polypropylene composition B', and the polypropylene composition B and the polypropylene composition B' each contain a random copolymer polypropylene x; Wherein, the melting point of the polypropylene composition A is greater than the melting points of the polypropylene composition B and the polypropylene composition B'; and the compression foaming is physical foaming.

2. The polypropylene composite foamed sheet according to claim 1, characterized in that: The melting point of the homopolymer polypropylene a in the polypropylene composition A is greater than the melting point of the random copolymer polypropylene x in the polypropylene compositions B and B', and the temperature difference of the corresponding melting points is preferably greater than or equal to 10 degrees; and / or, Based on the total weight of the polypropylene composition A, the polypropylene composition A comprises 50-99wt% of homopolypropylene a and 1-50wt% of impact copolymer polypropylene b; preferably, the polypropylene composition A comprises 70-90wt% of homopolypropylene a and 10-30wt% of impact copolymer polypropylene b.

3. The polypropylene composite foamed sheet according to claim 1, characterized in that: Based on the total thickness of the polypropylene sheet, the thickness of the layer A accounts for 51%-89% of the total thickness, preferably 71%-89%, and more preferably 71%-80%.

4. The polypropylene composite foamed board according to claim 1, characterized in that: The homopolymer polypropylene a has: The melting point is 150-170°C, preferably 160-170°C; and / or, The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or, The isotacticity (mm) is not less than 96%.

5. The polypropylene composite foamed board according to claim 1, characterized in that: The melting point of the impact-resistant copolymer polypropylene b is 150-170° C.: and / or, The monomer of the impact copolymer polypropylene b and propylene copolymer is ethylene or butene, preferably butene; and / or, The impact copolymer polypropylene b has a melt flow rate of 0.5-50 g / 10 min at 230° C. and a load of 2.16 kg, preferably 1-20 g / 10 min, and more preferably 2.5-18 g / 10 min; and / or, The cantilever beam impact strength of the impact-resistant copolymer polypropylene b is not less than 20KJ / m 2 .

6. The polypropylene composite foamed board according to claim 1, characterized in that: The polypropylene composition B and the polypropylene composition B' are each selected from random copolymer polypropylene x; and / or the random copolymer polypropylene x has: The melting point is 110-150°C, preferably 120-140°C; and / or, The melt flow rate at 230°C and 2.16 kg load is 0.5-50 g / 10 min, preferably 1-20 g / 10 min, and more preferably 3-18 g / 10 min; and / or, The molecular weight distribution Mw / Mn is 5-12, preferably 7-10; and / or, It is a copolymer of propylene and ethylene and / or butene, preferably an ethylene-propylene-butene terpolymer and / or a propylene-ethylene binary copolymer.

7. The polypropylene composite foamed board according to claim 1, characterized in that: The layer A also contains a β-crystalline nucleating agent; preferably, The β-crystal nucleating agent is at least one selected from the group consisting of condensed aromatic hydrocarbons, group IIA two-component complexes, aromatic diamides, rare earth compounds and cyclic dicarboxylates; and / or, Relative to 100 parts by weight of the polypropylene composition A, the content of the β-crystal nucleating agent in layer A is 0.01-0.5 parts by weight.

8. The polypropylene composite foamed board according to any one of claims 1 to 7, characterized in that: The polypropylene foam sheet contains a polypropylene composition, preferably the polypropylene foam sheet contains at least one of the polypropylene composition A, the polypropylene composition B, and the polypropylene composition B', and an optional auxiliary agent; preferably, the auxiliary agent is selected from one or more of an antioxidant, an antistatic agent, a lubricant, an anti-aging agent, a flame retardant, and a toner; and / or, The polypropylene foam sheet is foamed by an inorganic physical foaming agent and / or an organic physical foaming agent; preferably, the inorganic physical foaming agent is selected from at least one of air, nitrogen, carbon dioxide, oxygen and water, and / or the organic physical foaming agent is selected from at least one of an aliphatic hydrocarbon foaming agent, an alicyclic hydrocarbon foaming agent, and a halogenated hydrocarbon foaming agent.

9. The polypropylene composite foamed board according to any one of claims 1 to 7, characterized in that: Based on the total thickness of the polypropylene composite foamed board, the total thickness of the reinforced composite sheet accounts for 0.5%-5%, preferably 1%-3% of the total thickness of the polypropylene composite foamed board; and / or, The polypropylene composite foam board includes a layer of reinforced composite sheet and a layer of polypropylene foam sheet, or the polypropylene composite foam board includes multiple layers of reinforced composite sheets and at least one layer of polypropylene foam sheet; preferably, the outer layers of the polypropylene composite foam board are all reinforced composite sheets.

10. The polypropylene composite foamed board according to any one of claims 1 to 7, characterized in that: The total number of layers of all the polypropylene sheets, polypropylene fabrics and polypropylene foam sheets is 6-35 layers, more preferably 10-20 layers; and / or, The polypropylene foam sheets are stacked in order from top to bottom at 0-90 degrees along their respective machine directions, preferably with 1-4 layers, more preferably 1-2 layers; and / or, The reinforced composite sheets are stacked from top to bottom in the direction of 0-90° along their respective machine directions. Preferably, the total number of polypropylene sheets and polypropylene fabrics in each layer of the reinforced composite sheet is greater than or equal to 5 layers, more preferably 5-30 layers, and more preferably 5-15 layers.

11. The polypropylene composite foamed board according to any one of claims 1 to 7, characterized in that: Each layer of the reinforced composite sheet comprises a plurality of sequentially stacked polypropylene sheet unit groups; each polypropylene sheet unit group comprises at least one identical or different polypropylene sheet unit, each polypropylene sheet unit comprises a core layer A i and located in the core layer A i The outer layer B on both sides i , B' i , structure B i A i B' i The structure of the reinforced composite sheet is nth group...ith group...2nd group, 1st group, 2nd group...ith group...nth group from bottom to top, and the total number of stacked groups of polypropylene sheet unit groups is 2n-1; i and n are both integers not less than 2, and i≤n; Among them, the core layer A in the polypropylene sheet unit i Containing polypropylene composition A i , outer layer B i With outer layer B' i The same or different, each corresponding to a polypropylene composition B i , polypropylene composition B' i , The polypropylene composition A i The melting point is greater than that of the polypropylene composition B i , the polypropylene composition B' i The average melting point of all outer layers in the i-th group is greater than or equal to the average melting point of all outer layers in the i-1-th group; preferably, Polypropylene composition A i Melting point and polypropylene composition B i The difference in melting points, polypropylene composition A i The melting point of polypropylene composition B' i The difference in melting points of each is greater than or equal to 5°C, preferably greater than or equal to 10°C, more preferably greater than or equal to 20°C; and / or, The difference between the average melting point of all outer layers in the i-th group and the average melting point of all outer layers in the i-1th group is the same or different, and is 1-40°C, preferably 1-10°C, more preferably 1-5°C; and / or, 3≤n≤16, preferably, 3≤n≤8; and / or, Each group of polypropylene ply units, independently of one another, comprises 1 to 10, preferably 1 to 5, identical or different polypropylene ply units.

12. The polypropylene composite foamed board according to any one of claims 1 to 7, characterized in that: The polypropylene composite foamed board is prepared by the following method: laminating at least one group of the polypropylene sheets and / or the polypropylene fabric with at least one motherboard of the polypropylene foamed sheet, and subjecting the motherboard to a compression foaming treatment to obtain the polypropylene composite foamed board; the compression foaming treatment adopts physical foaming; Wherein, each group of the polypropylene sheets and / or the polypropylene fabrics are stacked in the order of forming the reinforced composite sheets of the corresponding layers; and / or, The temperature of the compression foaming is 140-170°C, preferably 150-163°C, more preferably 154-159°C; and / or, The pressure of the compression foaming is 4-16 MPa, preferably 8-12 MPa; and / or, The saturated immersion time of the compression foaming is 0.1-3 hours, preferably 0.3-1.5 hours.

13. A method for preparing the polypropylene composite foamed board according to any one of claims 1 to 12, comprising laminating the polypropylene sheet and / or the polypropylene fabric with the parent material of the polypropylene foamed sheet, and subjecting the laminate to a compression foaming treatment to obtain the polypropylene composite foamed board; the compression foaming treatment adopts physical foaming; wherein, All the polypropylene sheets and the polypropylene fabrics are stacked in groups in the order that they form the corresponding layers of reinforced composite sheets; preferably, The conditions of the compression molding and foaming treatment are controlled so that the base material of the polypropylene foam sheet is foamed to obtain the polypropylene foam sheet. Preferably, the polypropylene sheet and / or the polypropylene fabric are not foamed.

14. The preparation method according to claim 13, characterized in that: The temperature of the compression foaming is 140-170°C, preferably 150-163°C, more preferably 154-159°C; and / or, The pressure of the compression foaming is 4-16 MPa, preferably 8-12 MPa; and / or, The saturated immersion time of the molded foaming is 0.1-3 hours, preferably 0.3-1.5 hours; and / or, The total number of layers of all the polypropylene sheets and polypropylene fabrics and the polypropylene foam motherboard is 6-35 layers, and more preferably 10-20 layers.

15. Use of the polypropylene composite foamed board as described in any one of claims 1 to 12 or the polypropylene composite foamed board prepared by the preparation method of any one of claims 13 to 14 in materials used in at least one of the following fields: automobiles, communications, aircraft, logistics, thermal insulation, precision machinery and electronic turnover, and packaging.

Citation Information

Patent Citations

  • Propylene-ethylene-butylene high-melt-strength polypropylene foamed board or sheet and preparation method thereof

    CN103665582A

  • Propylene-ethylene high-melt-strength polypropylene foamed board or sheet and preparation method thereof

    CN103665584A

  • Polypropylene self-reinforced composite and preparation method thereof

    CN105563976A

  • High-melt-strength anti-impact polypropylene foamed board and preparation and application thereof

    CN106280018A

  • Polypropylene foam material with gradient pore structure and preparation method thereof

    CN108164814A