Surface group adjustable Nb2CTx catalyst doped MgH2 composite hydrogen storage material, preparation method and application thereof

By introducing an Nb2CTx catalyst with adjustable surface groups into MgH2, the problem of MgH2 kinetic barriers is solved, and its hydrogen release performance is significantly improved. It is suitable for portable power supplies and fuel cells, achieving low-cost and efficient hydrogen storage and release .

CN118908148APending Publication Date: 2024-11-08SUZHOU HAINAGU HYDROGEN NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410481473.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The strong metal hydrogen bonds and high kinetic barriers of MgH2 limit their further development and application as solid hydrogen storage material. The existing catalytic modification methods are difficult to effectively reduce the energy barrier of H2 adsorption/dissociation, affecting its dynamic characteristics.

Method used

The Nb2CTx catalyst with adjustable surface groups is used to doplate MgH2 composite hydrogen storage material. The Nb2CTx powder is combined with MgH2 through the preparation method. The preparation process includes HF treatment, KOH treatment and high-temperature annealing to form Nb2CTx, Nb2CTx-OH and Nb2CTx-O catalysts. , are non-precious metal materials and have good catalytic properties.

Benefits of technology

It significantly improves the hydrogen discharge performance of MgH2, reduces the initial hydrogen discharge temperature, improves the hydrogen release rate and efficiency, and is suitable for portable power supplies and fuel cells, with commercial application prospects and large-scale development potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908148A_ABST
    Figure CN118908148A_ABST
Patent Text Reader

Abstract

The invention discloses an Nb2CTx catalyst doped MgH2 composite hydrogen storage material capable of adjusting surface groups, a preparation method and application thereof. The preparation method comprises the following steps: slowly adding an Nb2AlC precursor into a 49wt% HF solution, and stirring at room temperature; after the reaction is finished, centrifuging suspension liquid, washing the suspension liquid with deionized water for multiple times, drying the suspension liquid to obtain Nb2CTx, dispersing the Nb2CTx in a KOH aqueous solution, stirring the Nb2CTx in the KOH aqueous solution at room temperature, and drying the Nb2CTx to obtain Nb2CTx-OH; the Nb2CTx-OH subjected to KOH treatment is subjected to annealing in argon, and Nb2CTx-O is obtained; and carrying out ball milling on MgH2 and the Nb2CTx catalyst doped MgH2 composite hydrogen storage material with adjustable surface groups in an argon atmosphere to obtain the composite hydrogen storage material. The initial hydrogen desorption temperature and hydrogen desorption rate of the composite hydrogen storage material are improved, the preparation method is simple, safe and efficient, and the hydrogen storage dynamics of MgH2 is remarkably optimized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of hydrogen storage materials, and in particular to a Nb2CT with adjustable surface groups. x Catalyst-doped MgH2 composite hydrogen storage material, preparation method and application thereof. Background Art

[0002] Due to the depletion of fossil resources and people's increasing concern about environmental issues, the demand for clean energy is increasing day by day. Hydrogen energy has attracted widespread attention due to its high combustion calorific value and abundant sources. The safe and efficient storage of hydrogen has received particular attention because it plays a key role between hydrogen production and application. Due to the excellent volume density (110.0kg-m-3) and mass density (7.6wt%) of MgH2, it has been widely studied as a safe and efficient solid-state hydrogen storage material.

[0003] However, strong metal-hydrogen bonds and high kinetic barriers limit its further development and practical application. To address the above challenges, researchers have investigated various strategies to improve the hydrogen storage performance of MgH2, among which catalytic modification is a feasible method to improve the kinetic properties of MgH2 by reducing the energy barrier of H2 adsorption / dissociation.

[0004] In recent years, two-dimensional MXene has emerged as an efficient magnesium-based hydrogen storage material catalyst. MXene compounds, such as M2CT x (M: transition metal; T x :anionic groups), due to the layered structure, it exhibits high surface area characteristics, making its nanosheets uniformly dispersed on Mg / MgH2. The lattice of MXene contains transition metals such as Ti, V and Nb. These metals act as effective catalytic active centers and can increase the dehydrogenation rate by reducing the activation energy. It is worth noting that MXene compounds have abundant anionic surface groups, usually expressed as T x , relevant studies have shown that T x Defects play a key role in controlling the reaction, although T x The role of defects in hydrogen dissociation and diffusion processes is still unclear, but their effectiveness in controlling reactant adsorption, dissociation, and diffusion processes has greatly motivated us to apply this strategy to magnesium-based hydrogen storage materials. Summary of the invention

[0005] In order to overcome the shortcomings of the prior art, the present invention aims to provide a Nb2CT with adjustable surface groups. x Catalyst-doped MgH2 composite hydrogen storage materials, preparation methods and applications thereof are low-cost, have a wide range of raw materials, and are simple to prepare. They have high commercial application prospects and can be used in portable power devices, hydrogen sources for fuel cells, etc., and are also suitable for large-scale development and application.

[0006] In order to solve the above technical problems, a technical solution adopted by the present invention is: a Nb2CT x Catalyst-doped MgH2 composite hydrogen storage materials, including Nb2CT with tunable surface groups x powder and MgH2, the adjustable surface groups of Nb2CT x The powder accounts for 3-20wt% of the total mass of the composite hydrogen storage material.

[0007] In a preferred embodiment of the present invention, the Nb2CT x The surface groups Tx of the catalyst are controllable.

[0008] The present invention discloses a Nb2CT with adjustable surface groups x The preparation method of the catalyst-doped MgH2 composite hydrogen storage material comprises the following steps:

[0009] Step 1: slowly add 2g Nb2AlC precursor into 30ml 49wt% HF solution and stir at room temperature for 2 days. After the reaction is completed, centrifuge the suspension, wash it with deionized water several times and dry it to obtain Nb2CT x ;

[0010] Step 2: Nb2CT obtained in step 1 x Dispersed in KOH aqueous solution, stirred at room temperature for 12 to 36 hours, washed and dried to obtain Nb2CT x -OH;

[0011] Step 3: Nb2CT obtained in step 2 x -OH is calcined at 400-600°C for 1-3 hours under a protective atmosphere to obtain Nb2CT x -O catalyst.

[0012] Furthermore, in step 1, the ratio of Nb2AlC to HF is: 15 ml HF for every 1 g Nb2AlC. The mixture is washed with deionized water until the pH reaches 6 before drying.

[0013] Further, in step 2, every 100 mg Nb2CT x Corresponding to 5 ml of 10 wt% KOH aqueous solution. Wash with deionized water until pH reaches 6 before drying.

[0014] Furthermore, in step three, the protective atmosphere is argon, and the heating rate is 2 to 8°C / min.

[0015] The MgH2 used in the present invention can be prepared by a known method. Specifically, MgH2 is prepared by mechanical ball milling and hydrogenation heat treatment. The specific steps are as follows:

[0016] (a) Mg powder was heated from room temperature to 450°C at a rate of 2°C / min, hydrogen was absorbed under a hydrogen pressure of 65 bar, and then ball milled at a speed of 450 rpm, with a ball-to-powder ratio of 40:1 and a ball milling time of 5 h;

[0017] (b) heating the material obtained in step (a) from room temperature to 450° C. at a rate of 2° C. / min, performing a hydrogenation heat treatment under a hydrogen pressure of 65 bar, and then ball milling at a rotation speed of 450 rpm for 5 times, each time for 1 hour;

[0018] (c) The material obtained in step (b) is heated from room temperature to 450°C at a rate of 2°C / min, and then subjected to hydrogenation heat treatment under a hydrogen pressure of 65 bar to obtain MgH2.

[0019] Another aspect of the present invention is a Nb2CT with adjustable surface groups. x The preparation method of the catalyst-doped MgH2 composite hydrogen storage material and the catalyst-doped MgH2 composite hydrogen storage material comprises the following steps:

[0020] 10wt% Nb2CT x 、Nb2CT x -OH and Nb2CT x -O and 90wt% MgH2 were ball milled at a ball-to-material ratio of 40:1 at a speed of 400r / min for 6h.

[0021] Another aspect of the present invention provides application of the above composite hydrogen storage material in hydrogen storage.

[0022] Beneficial effects: Compared with the prior art, the present invention has the following significant features:

[0023] 1. The preparation method is simple and has high commercial application prospects. It can be used in portable power supply devices, hydrogen supply sources for fuel cells, etc., and is also suitable for large-scale development and application;

[0024] 3. Nb2CT x 、Nb2CT x -OH and Nb2CT x -O are all non-precious metal materials, low in price and widely available.

[0025] 2. Prepared Nb2CT x 、Nb2CT x -OH and Nb2CT x -O have good catalytic performance for MgH2, among which Nb2CT x -OH can provide the most active sites and the best performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The precursor Nb2AlC and the obtained Nb2CT in Example 1 of the present invention are x XRD pattern of

[0027] Figure 2 The Nb2CT obtained in Example 2 of the present invention x 、Nb2CT x -OH, Nb2CT x -XRD pattern of O;

[0028] Figure 3 It is the Nb2CT obtained in Example 3 of the present invention. x SEM images of

[0029] Figure 4 It is the Nb2CT obtained in Example 3 of the present invention. x SEM image of -OH;

[0030] Figure 5 It is the Nb2CT obtained in Example 3 of the present invention. x -SEM image of O;

[0031] Figure 6 is the temperature increase hydrogen release curve obtained in Example 4 of the present invention;

[0032] Figure 7 is a comparative curve of hydrogen release at elevated temperature obtained in Example 5 of the present invention;

[0033] Figure 8 This is a constant temperature hydrogen release comparison curve obtained in Example 6 of the present invention. DETAILED DESCRIPTION

[0034] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Example 1

[0036] Preparation of Nb2CT from Nb2AlC x The method comprises the following steps:

[0037] a. Slowly add 2 g of Nb2AlC precursor into 30 ml of 49 wt% HF solution and stir at room temperature for 2 days. After the reaction is completed, centrifuge the suspension, wash with deionized water until the pH value reaches 6, and dry to obtain Nb2CT x ;

[0038] b. For Nb2AlC and Nb2CT x Conduct XRD phase characterization, which is performed using an X-ray diffractometer;

[0039] XRD characterization results show that after HF etching, the peak of Nb2AlC disappears completely, and the peak of Nb2CT x The (002) and (100) faces of Nb2CT x Successful preparation.

[0040] Example 2

[0041] A Nb2CT with adjustable surface groups x The preparation method of the catalyst and the XRD characterization include the following steps:

[0042] a. Slowly add 2 g of Nb2AlC precursor into 30 ml of 49 wt% HF solution and stir at room temperature for 2 days. After the reaction is completed, centrifuge the suspension, wash with deionized water until the pH value reaches 6, and then dry to obtain Nb2CT x ;

[0043] b. Take 500 mg of Nb2CT obtained in step a x Dispersed in 25 ml of 10 wt% KOH aqueous solution, stirred at room temperature for 24 h, washed until the pH value reached 6, and dried to obtain Nb2CT x -OH;

[0044] c. The Nb2CT obtained in step b x -OH was heated to 500°C at a rate of 5°C / min under an argon atmosphere and kept at 500°C for 3 hours to obtain Nb2CT x -O catalyst;

[0045] d. Nb2CT x 、Nb2CT x -OH and Nb2CT x -O was subjected to XRD phase characterization, which was carried out using an X-ray diffractometer.

[0046] XRD characterization results show that after KOH treatment, the (002) peak gradually shifts to a smaller angle, indicating that K+ intercalation occurs, and -OH and interlayer water increase. In contrast, after annealing, the (002) peak shifts to a higher angle, indicating the removal of interlayer water and -OH.

[0047] Example 3

[0048] A Nb2CT with adjustable surface groups x The preparation method and SEM characterization of the catalyst include the following steps:

[0049] a. Slowly add 2 g of Nb2AlC precursor into 30 ml of 49 wt% HF solution and stir at room temperature for 2 days. After the reaction is completed, centrifuge the suspension, wash with deionized water until the pH value reaches 6, and then dry to obtain Nb2CT x ;

[0050] b. Take 500 mg of Nb2CT obtained in step a x Dispersed in 25 ml of 10 wt% KOH aqueous solution, stirred at room temperature for 24 h, washed until the pH value reached 6, and dried to obtain Nb2CT x -OH;

[0051] c. The Nb2CT obtained in step b x -OH was heated to 500°C at a rate of 5°C / min under an argon atmosphere and kept at 500°C for 2 hours to obtain Nb2CT x -O catalyst;

[0052] d. Nb2CT x 、Nb2CT x -OH and Nb2CT x -O SEM characterization. This characterization was performed using a cold field emission scanning electron microscope;

[0053] SEM characterization results show that the original Nb2CT x The relaxed accordion-like structure is shown, indicating that the Al layer has been successfully removed. After KOH and annealing treatment, all morphologies remain intact, indicating that KOH and annealing treatments have not damaged the Nb2CT x structure.

[0054] Example 4

[0055] Doped Nb2CT x Improve the hydrogen release performance of MgH2 at elevated temperature:

[0056] Weigh Nb2CT in the box x The sample of MgH2-doped composite hydrogen storage material is 150-250 mg. After the sample is placed in the device, evacuate the air, check for leaks, start the test, and heat up to 450°C at a rate of 2°C / min through the program.

[0057] The comparison of hydrogen release curves shows that Nb2CT x The dehydrogenation performance of MgH2 is significantly improved, and the initial dehydrogenation temperature is reduced from 350°C to 200°C. At 350°C, 6.55wt% of hydrogen can be released, while the original MgH2 has just begun to dehydrogenate.

[0058] Example 5

[0059] Nb2CT doped with adjustable surface groupsx Improve the hydrogen release performance of MgH2 at elevated temperature:

[0060] Weigh Nb2CT in the box x 、Nb2CT x -OH and Nb2CT x A sample of 150-250 mg of -O doped MgH2 composite hydrogen storage material is placed in the device, evacuated, leaks are detected, and the test is started. The temperature is raised to 450°C at a rate of 2°C / min through the program.

[0061] The comparison of hydrogen release curves shows that Nb2CT x -OH and Nb2CT x -O improves the hydrogen desorption performance of MgH2 compared with the original Nb2CT x With further improvement, Nb2CT x -OH has the best catalytic performance.

[0062] Example 6

[0063] Nb2CT doped with adjustable surface groups x Improve the isothermal hydrogen desorption performance of MgH2 at 250°C:

[0064] Take 150-250 mg of sample from the glove box and put it into the device, evacuate, check for leaks, start the test, introduce 32-33 bar of hydrogen, and heat to 250°C at a rate of 5°C / min through the program, and keep warm for 85 minutes. Turn on the vacuum pump, vent to below 7 bar, close the reactor, start evacuation for 10 seconds, start low transmission for 7 seconds, start expansion for 8 seconds, turn off evacuation for 9 seconds, turn off the reactor for 10 seconds, and then record the test.

[0065] The constant volume-pressure difference method was used to measure the constant temperature dehydrogenation performance of the composite hydrogen storage material. After constant temperature dehydrogenation at 250°C, it can be seen that Nb2CT x The kinetic performance of MgH2 catalyzed by -OH was the best, releasing 6.55 wt% of hydrogen within 5 min, followed by Nb2CT x -O, 6.06wt% hydrogen can be released within 5min, and the original Nb2CT x , only 3.80wt% of hydrogen can be released within 5 minutes.

[0066] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A Nb2CT with adjustable surface groups x Catalyst doped MgH2 composite hydrogen storage material, characterized in that: Nb2CT including tunable surface groups x powder and MgH2, the adjustable surface groups of Nb2CT x The powder accounts for 3-20wt% of the total mass of the composite hydrogen storage material.

2. The Nb2CT with adjustable surface groups according to claim 1 x Catalyst doped MgH2 composite hydrogen storage material, characterized in that: The Nb2CT x The surface groups Tx of the catalyst are controllable.

3. A Nb2CT with adjustable surface groups x The method for preparing a catalyst-doped MgH2 composite hydrogen storage material is characterized in that: The following steps are involved: (1) The Nb2AlC precursor was slowly added to a 49 wt% HF solution and stirred at room temperature for 2 days. After the reaction was completed, the suspension was centrifuged, washed several times with deionized water, and dried to obtain Nb2CT x ; (2) The Nb2CT obtained in step 1 x Dispersed in KOH aqueous solution, stirred at room temperature for 12 to 36 hours, washed and dried to obtain Nb2CT x -OH; (3) The Nb2CT obtained in step 2 x -OH is calcined at 400-600°C for 1-3 hours under a protective atmosphere to obtain Nb2CT x -O catalyst. (4) Reaction of MgH2 and Nb2CT x 、Nb2CT x -OH and Nb2CT x -O ball milling, always maintaining argon atmosphere, and ball milling at a speed of 300-500 r / min for 2-10 hours.

4. The Nb2CT with adjustable surface groups according to claim 3 x The method for preparing a catalyst-doped MgH2 composite hydrogen storage material is characterized by: In step 1, the ratio of Nb2AlC to HF is: 15 ml HF for every 1 g Nb2AlC.

5. The Nb2CT with adjustable surface groups according to claim 3 x The method for preparing a catalyst-doped MgH2 composite hydrogen storage material is characterized by: In step 1, the product is washed with deionized water until the pH reaches 6 before drying.

6. The Nb2CT with adjustable surface groups according to claim 3 x The method for preparing a catalyst-doped MgH2 composite hydrogen storage material is characterized by: In the step 2, every 100 mg Nb2CT x Corresponding to 5 ml of 10wt% KOH aqueous solution.

7. The Nb2CT with adjustable surface groups according to claim 3 x The method for preparing a catalyst-doped MgH2 composite hydrogen storage material is characterized by: In the step 2, the product is washed with deionized water until the pH reaches 6 before drying.

8. The Nb2CT with adjustable surface groups according to claim 3 x The method for preparing a catalyst-doped MgH2 composite hydrogen storage material is characterized by: In step three, the protective atmosphere is argon.

9. The Nb2CT with adjustable surface groups according to claim 3 x The method for preparing a catalyst-doped MgH2 composite hydrogen storage material is characterized by: In step three, the heating rate is 2-8°C / min.