Preparation method of lithium iron manganese phosphate positive electrode material, electrode and lithium battery

By preparing iron and manganese-containing precursors separately and adjusting their proportions, a stable lithium manganese phosphate positive electrode material is solved, and the problem of insufficient discharge specific capacity of lithium manganese phosphate materials in the prior art is improved, and the electrochemistry of lithium batteries is improved Performance and discharge specific capacity.

CN118908173APending Publication Date: 2024-11-08HUNAN YUNENG NEW ENERGY BATTERY MATERIALS CO LTD

Patent Information

Application Number
CN202410953574.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, when preparing lithium manganese iron phosphate materials, the discharge specific capacity obtained is still a certain gap from the theoretical specific capacity, and cannot meet market demand.

Method used

Iron-containing precursors and manganese-containing precursors are prepared separately, and their morphology, crystal form and particle size are controlled by adjusting the synthesis conditions, reactant ratio and precipitation process to ensure accurate elemental ratios, and then sintered in a nitrogen atmosphere to form The lithium manganese iron phosphate positive electrode material adjusts the iron-manganese ratio to form a more stable crystal structure and improves conductivity and electrochemical properties.

Benefits of technology

The conductivity and electrochemical performance of lithium manganese iron phosphate cathode material has been improved, and the first discharge specific capacity of lithium batteries is increased to 165.9mAh/g for 0.1C ratio, meeting market demand.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908173A_ABST
    Figure CN118908173A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium batteries, and particularly relates to a preparation method of a lithium iron manganese phosphate positive electrode material, an electrode and a lithium battery, the method comprises the following steps: S1, carrying out a chemical reaction based on an iron source, a first acid radical precipitator and a first dispersant to obtain an iron-containing precursor; s2, performing chemical reaction based on a manganese source, a second acid radical precipitator and a second dispersant to obtain a manganese-containing precursor; s3, mixing and grinding the iron-containing precursor, the manganese-containing precursor, a lithium source, a phosphorus source and a carbon source to obtain a precursor mixture; and S4, sintering the precursor mixture in a nitrogen atmosphere to obtain the lithium iron manganese phosphate positive electrode material. The structural general formula of the lithium manganese iron phosphate positive electrode material is LiMnxFe (1-x) PO4, 0.3 lt, xlt; and 0.45%. Compared with the prior art, as the iron-containing precursor and the manganese-containing precursor are respectively prepared and the ratio of iron to manganese is controlled, the conductivity of the lithium iron manganese phosphate positive electrode material is improved, and the specific discharge capacity of a lithium battery prepared from the lithium iron manganese phosphate positive electrode material is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of lithium batteries, and in particular, relates to a method for preparing a lithium manganese iron phosphate positive electrode material, an electrode, and a lithium battery. Background Art

[0002] Lithium iron phosphate (LiFePO4) material has an olivine structure, a large theoretical specific capacity of 170mAh / g and a stable charge and discharge platform. The insertion and extraction potential of lithium iron phosphate material in aqueous electrolyte is within the stable potential window of water, which is beneficial to the long-term stability of the system and has huge application potential.

[0003] At present, in order to improve the performance of lithium iron phosphate materials, the existing technology often adopts a solid phase method to mix and grind the lithium source, iron source, manganese source, phosphorus source and carbon source and then sinter them. However, the discharge specific capacity of the doped lithium iron phosphate material obtained by the current preparation method is still a certain distance away from the theoretical specific capacity and cannot meet the market demand.

[0004] The existing preparation method has the problem that the discharge specific capacity of the obtained lithium manganese iron phosphate material cannot meet the demand. Summary of the invention

[0005] The embodiments of the present application provide a method for preparing a lithium iron manganese phosphate positive electrode material, an electrode and a lithium battery, which aim to solve the problem that the discharge specific capacity of the lithium iron manganese phosphate material obtained by the preparation method cannot meet the demand to a certain extent.

[0006] In a first aspect, an embodiment of the present application provides a method for preparing a lithium manganese iron phosphate positive electrode material, comprising:

[0007] S1, chemically reacting an iron source, a first acid radical precipitant and a first dispersant to obtain an iron-containing precursor;

[0008] S2, chemically reacting a manganese source, a second acid radical precipitant and a second dispersant to obtain a manganese-containing precursor;

[0009] S3, mixing and grinding an iron-containing precursor, a manganese-containing precursor, a lithium source, a phosphorus source and a carbon source to obtain a precursor mixture;

[0010] S4, sintering the precursor mixture in a nitrogen atmosphere to obtain a lithium manganese iron phosphate positive electrode material;

[0011] Among them, the general structural formula of lithium manganese iron phosphate positive electrode material is LiMn x Fe (1-x) PO4, 0.3 <X<0.45。

[0012] The present application provides a method for preparing a lithium iron manganese phosphate positive electrode material. By separately preparing an iron-containing precursor, an iron-containing precursor with high purity and accurate element ratio can be obtained, and the morphology, crystal form and particle size and other characteristics of the iron-containing precursor are controlled by adjusting the synthesis conditions, reactant ratio and precipitation process, thereby improving the conductivity of the lithium iron manganese phosphate positive electrode material; and by separately preparing a manganese-containing precursor with accurate element ratio, manganese ions can be uniformly dispersed in a solution, which is conducive to the subsequent preparation of a uniformly dispersed lithium iron manganese phosphate positive electrode material, thereby improving the electrochemical performance and stability of the lithium iron manganese phosphate positive electrode material, and the crystal form and crystal structure of the manganese-containing precursor are controlled by adjusting the reaction conditions, dispersant and precipitation process, thereby improving the lithium iron manganese phosphate. The voltage of the voltage platform of the positive electrode material; and then sintering to form a lithium iron manganese phosphate positive electrode material by adjusting the ratio of iron in the iron-containing precursor and manganese in the manganese-containing precursor; compared with the solid phase method preparation in the prior art, due to the separate preparation of the iron-containing precursor and the manganese-containing precursor and the accurate control of the iron-manganese ratio, the evenly mixed manganese iron can form a more stable crystal structure, thereby increasing the number of active lithium ions, thereby increasing the conductivity of the lithium iron manganese phosphate positive electrode material, and then increasing the discharge specific capacity of the lithium battery made of the lithium iron manganese phosphate positive electrode material. Experimental verification shows that the first discharge specific capacity of the lithium battery made of the lithium iron manganese phosphate positive electrode material prepared in the present application at a rate of 0.1C can reach 165.9mAh / g.

[0013] In a second aspect, an embodiment of the present application provides an electrode comprising a lithium manganese iron phosphate positive electrode material obtained by the preparation method described in any one of the contents of the first aspect.

[0014] The embodiment of the present application uses a lithium iron manganese phosphate positive electrode material obtained by separately preparing an iron-containing precursor and a manganese-containing precursor and controlling the iron-manganese ratio to make an electrode, thereby improving the conductivity of the lithium iron manganese phosphate material and further improving the discharge specific capacity of the lithium battery made of the lithium iron manganese phosphate positive electrode material.

[0015] In a third aspect, an embodiment of the present application provides a lithium battery, wherein the positive electrode of the lithium battery is made of the lithium iron manganese phosphate positive electrode material described in the second aspect.

[0016] The embodiment of the present application uses a lithium iron manganese phosphate positive electrode material obtained by separately preparing an iron-containing precursor and a manganese-containing precursor and controlling the iron-manganese ratio to make an electrode for a lithium battery, thereby improving the conductivity of the lithium iron manganese phosphate material and further improving the discharge specific capacity of the lithium battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0018] Figure 1 It is a schematic flow chart of a method for preparing a lithium iron manganese phosphate positive electrode material provided in one embodiment of the present application. DETAILED DESCRIPTION

[0019] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0020] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0021] In the present application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, a~b (i.e. a and b), a~c, b~c, or a~b~c, where a, b, c can be single or multiple, respectively.

[0022] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. For example, without departing from the scope of the implementation regulations of this application, the first XX can also be called the second XX, and similarly, the second XX can also be called the first XX. Therefore, the features defined as "first" and "second" can explicitly or implicitly include one or more of the features.

[0023] The terms used in the embodiments of the present application are only for the purpose of describing specific implementation rules, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the implementation rules of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0024] It should be understood that in the various embodiments of the present application, the size of the serial number of each process does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the implementation regulations of this application.

[0025] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0026] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0027] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0028] Lithium-ion batteries are rechargeable batteries that rely on the movement of lithium ions between the negative electrode and the positive electrode. The positive electrode material is an important component of lithium-ion batteries, and its structure and properties have an important impact on the overall performance of lithium-ion batteries.

[0029] The most commonly used positive electrode materials for lithium-ion batteries currently include two-dimensional layered structures of LiNiO2 and LiMnO2, three-dimensional framework structures of LiMn2O4 and Li3V2(PO4)3, and one-dimensional tunnel structure of LiMnPO4.

[0030] Lithium iron phosphate (LiFePO4) material has an olivine structure, a large theoretical specific capacity of 170mAh / g and a stable charge and discharge platform. The insertion and extraction potential of lithium iron phosphate material in aqueous electrolyte is within the stable potential window of water, which is beneficial to the long-term stability of the system and has huge application potential.

[0031] In order to improve the performance of lithium iron phosphate materials, the existing technology often adopts a solid phase method to mix and grind a lithium source, an iron source, a manganese source, a phosphorus source and a carbon source and then sinter them. However, the discharge specific capacity of the doped lithium iron phosphate material obtained by the current preparation method is still a certain distance away from the theoretical specific capacity and cannot meet market demand.

[0032] In order to solve the problem that the discharge capacity of the lithium manganese iron phosphate material obtained by the preparation method cannot meet the demand to a certain extent, Figure 1 As shown, the first aspect of the embodiment of the present application provides a method for preparing a lithium manganese iron phosphate positive electrode material, comprising:

[0033] S1, chemically reacting an iron source, a first acid radical precipitant and a first dispersant to obtain an iron-containing precursor;

[0034] S2, chemically reacting a manganese source, a second acid radical precipitant and a second dispersant to obtain a manganese-containing precursor;

[0035] S3, mixing and grinding an iron-containing precursor, a manganese-containing precursor, a lithium source, a phosphorus source and a carbon source to obtain a precursor mixture;

[0036] S4, sintering the precursor mixture in a nitrogen atmosphere to obtain a lithium manganese iron phosphate positive electrode material;

[0037] Among them, the general structural formula of lithium manganese iron phosphate positive electrode material is LiMn x Fe (1-x) PO4, 0.3 <X<0.45。

[0038] The present application provides a method for preparing a lithium iron manganese phosphate positive electrode material. By separately preparing an iron-containing precursor, a high-purity iron-containing precursor with an accurate element ratio can be obtained, and the morphology, crystal form, particle size and other characteristics of the iron-containing precursor are controlled by adjusting the synthesis conditions, the ratio of reactants and the precipitation process, thereby improving the conductivity of the lithium iron manganese phosphate positive electrode material; and by separately preparing a manganese-containing precursor with an accurate element ratio, manganese ions can be uniformly dispersed in a solution, which is beneficial to the subsequent preparation of a uniformly dispersed lithium iron manganese phosphate positive electrode material, thereby improving the electrochemical performance and stability of the lithium iron manganese phosphate positive electrode material, and by adjusting the reaction conditions, dispersant and precipitation process, the crystal form and crystal structure of the manganese-containing precursor are controlled, thereby improving the lithium iron manganese phosphate. The voltage of the voltage platform of the positive electrode material; and then sintering to form a lithium iron manganese phosphate positive electrode material by adjusting the ratio of iron in the iron-containing precursor and manganese in the manganese-containing precursor; compared with the solid phase method preparation in the prior art, due to the separate preparation of the iron-containing precursor and the manganese-containing precursor and the accurate control of the iron-manganese ratio, the evenly mixed manganese iron can form a more stable crystal structure, thereby increasing the number of active lithium ions, thereby increasing the conductivity of the lithium iron manganese phosphate positive electrode material, and then increasing the discharge specific capacity of the lithium battery made of the lithium iron manganese phosphate positive electrode material. Experimental verification shows that the first discharge specific capacity of the lithium battery made of the lithium iron manganese phosphate positive electrode material prepared in the present application at a rate of 0.1C can reach 165.9mAh / g.

[0039] In some embodiments, in step S1, the iron source and the first acid radical precipitant undergo a chemical reaction, and the first dispersant is used to evenly disperse the iron-containing precursor generated by the reaction and form a spherical iron-containing precursor. The reaction temperature of step S1 is 40°C to 70°C, the reaction time is 30min to 90min, the pH value is 4.0 to 6.8, and the stirring rate is 200r / min to 500r / min. Under the reaction conditions of this embodiment, an iron-containing precursor having a morphology, crystal form and particle size that meet the requirements can be formed, thereby improving the conductivity of the lithium manganese iron phosphate positive electrode material.

[0040] In some embodiments, the molar ratio of the first acid radical precipitant of step S1 to the iron in the iron source is (1.0-1.5): 1; the molar ratio of the first acid radical precipitant to iron can completely replace the iron in the iron source within the scope of this embodiment to form an iron-containing precursor precipitate; the amount of the first dispersant added in step S1 is 0.5%-3.0% of the total weight of the iron source, the first acid radical precipitant and the first dispersant; the mass percentage of the first dispersant of this embodiment can effectively disperse the iron-containing precursor without increasing the cost, thereby forming an iron-containing precursor whose morphology, crystal form and particle size meet the requirements. For example, the first dispersant is polyethylene glycol, which has good water solubility (can effectively disperse particles in a water-based system), low toxicity, biocompatibility, and surface activity (having hydrophobic and hydrophilic parts, which can reduce interfacial tension and stabilize the suspension).

[0041] In some embodiments, in step S2, the manganese source and the second acid radical precipitant react chemically, and the second dispersant is used to allow the manganese-containing precursor generated by the reaction to be evenly dispersed and form a spherical manganese-containing precursor. The reaction temperature of step S2 is 45°C to 80°C, the reaction time is 30min to 120min, the pH value is 5.0 to 6.5, and the stirring rate is 200r / min to 500r / min; under the reaction conditions of this embodiment, a manganese-containing precursor whose morphology, crystal form and crystal structure meet the requirements can be formed, thereby improving the conductivity of the lithium manganese iron phosphate positive electrode material.

[0042] In some embodiments, the molar ratio of the second acid radical precipitant in step S2 to the manganese in the manganese source is (1.0-1.4):1; the molar ratio of the second acid radical precipitant to manganese can completely replace the manganese in the manganese source to form a manganese-containing precursor precipitate within the scope of this embodiment; the amount of the second dispersant added in step S2 is 0.5%-3.0% of the total weight of the manganese source, the second acid radical precipitant and the second dispersant; the mass percentage of the first dispersant in this embodiment can effectively disperse the iron-containing precursor without increasing the cost, thereby forming an iron-containing precursor that meets the requirements in morphology, crystal form and particle size. For example, the second dispersant is Berol 475, which is a dispersant produced by Nouryon, a non-ionic surfactant, usually composed of fatty alcohol ethoxylates, which has good emulsification, wetting and dispersing properties, can effectively reduce surface tension, and promote the uniform dispersion of solid particles of manganese-containing precursors in liquids.

[0043] In some embodiments, the amount of carbon source added in step S3 is 10% to 20% of the total weight of the iron-containing precursor, the manganese-containing precursor, the lithium source, the phosphorus source and the carbon source; the carbon source in the mass ratio range of this example can cover the lithium iron phosphate as much as possible, increase the conductivity of the lithium manganese iron phosphate and reduce the water absorption.

[0044] In some embodiments, the first acid precipitation agent is oxalic acid or other soluble oxalate (such as ammonium oxalate), which reacts with Fe 2+ +C2O4 2- +2H2O=FeC2O4·2H2O, oxalate ions react with ferrous ions and water of the iron source to form an iron-containing precursor of ferrous oxalate dihydrate; the second acid precipitant is ammonium carbonate or ammonium bicarbonate, and through the chemical reaction Mn 2+ +CO3 2- =MnCO3, carbonate ions and manganese ions generate a manganese-containing precursor of manganese carbonate.

[0045] In some embodiments, the sintering parameters of step S4 are: sintering temperature is 700°C to 820°C, and sintering time is 15h to 20h; the sintering parameters of this embodiment are used to improve the coating property of carbon-coated lithium iron phosphate, and improve the conductivity and water absorption of lithium manganese iron phosphate positive electrode material.

[0046] In some implementations, the iron source is one or more combinations of ferrous chloride, ferrous sulfate, ferrous phosphate, ferrous oxalate and ferrous acetate; and / or, the lithium source is one or more combinations of lithium carbonate, lithium hydroxide, lithium dihydrogen phosphate; and / or, the phosphorus source is one or more combinations of lithium dihydrogen phosphate, ammonium hydrogen phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate and phosphoric acid; and / or, the manganese source is one or more combinations of manganese dihydrogen phosphate, manganese tetraoxide, manganese dioxide, manganese carbonate; and / or, the carbon source is one or more combinations of citric acid, glucose, sucrose, lactose, maltose, phenolic resin, carbon nanotubes and epoxy resin. The multiple sources of the iron source of this embodiment can select one or more combinations according to demand to prepare lithium iron manganese phosphate positive electrode material; the multiple sources of the lithium source can select one or more combinations according to demand to prepare lithium iron manganese phosphate positive electrode material; the multiple sources of the phosphorus source can select one or more combinations according to demand to prepare lithium iron manganese phosphate positive electrode material; the multiple sources of the manganese source can select one or more combinations according to demand to prepare lithium iron manganese phosphate positive electrode material; the multiple sources of the above raw materials can also reduce production costs. Exemplarily, the lithium source is lithium carbonate (Li2CO3), the iron source is ferric chloride (FeCl2), the phosphorus source is ammonium dihydrogen phosphate (NH4H2PO4), and the carbon source is citric acid (C6H8O7). Among them, citric acid can not only act as a carbon source, but also dissolve the edges and corners on the surface of lithium iron manganese phosphate, making the morphology of lithium iron manganese phosphate particles more rounded.

[0047] In a second aspect, an embodiment of the present application provides an electrode comprising a lithium manganese iron phosphate positive electrode material obtained by the preparation method described in any one of the contents of the first aspect.

[0048] The embodiment of the present application uses a lithium iron manganese phosphate positive electrode material obtained by separately preparing an iron-containing precursor and a manganese-containing precursor and controlling the iron-manganese ratio to make an electrode, thereby improving the conductivity of the lithium iron manganese phosphate material and further improving the discharge specific capacity of the lithium battery made of the lithium iron manganese phosphate positive electrode material.

[0049] In a third aspect, an embodiment of the present application provides a lithium battery, wherein the positive electrode of the lithium battery is made of the lithium iron manganese phosphate positive electrode material described in the second aspect.

[0050] The embodiment of the present application uses a lithium iron manganese phosphate positive electrode material obtained by separately preparing an iron-containing precursor and a manganese-containing precursor and controlling the iron-manganese ratio to make an electrode for a lithium battery, thereby improving the conductivity of the lithium iron manganese phosphate material and further improving the discharge specific capacity of the lithium battery.

[0051] In order to enable the above-mentioned implementation details and operations of the present application to be clearly understood by those skilled in the art, as well as to demonstrate the significant improvement in performance of a method for preparing a lithium iron manganese phosphate positive electrode material, an electrode, and a lithium battery in an embodiment of the present application, the above-mentioned technical solution is illustrated by way of multiple embodiments below.

[0052] Example 1

[0053] Preparation of iron-containing precursor: using iron source ferric chloride (FeCl2) and first acid radical precipitant ammonium oxalate as raw materials, polyethylene glycol as the first dispersant, through chemical reaction: Fe 2+ +C2O4 2- +2H2O=FeC2O4·2H2O, and an iron-containing precursor precipitate is obtained. The reaction temperature is 45°C, the reaction time is 70 min, the pH value is 4.8, the stirring rate is 300 r / min, the molar ratio of ammonium oxalate to iron in ferric chloride is 1.1:1, and the amount of polyethylene glycol added is 1.5% of the total weight of ferric chloride, ammonium oxalate and polyethylene glycol.

[0054] Preparation of manganese-containing precursor: Using manganese source Marif salt (manganese dihydrogen phosphate) and second precipitant ammonium carbonate as raw materials, Berol 475 as second dispersant, through chemical reaction: Mn 2+ +CO3 2- =MnCO3, and a manganese-containing precursor precipitate is obtained. The reaction temperature is 55°C, the reaction time is 50 min, the pH value is 5.6, the stirring rate is 280 r / min, the molar ratio of ammonium carbonate to manganese in dihydrogen manganese phosphate is 1.3:1, and the addition amount of Berol 475 is 2.3% of the total weight of dihydrogen manganese phosphate, ammonium carbonate and Berol 475.

[0055] The iron-containing precursor and manganese-containing precursor precipitation products obtained in the above steps are mixed with lithium carbonate, ammonium dihydrogen phosphate and citric acid and ground evenly, and then sintered at 700°C to 820°C for 15h to 20h under nitrogen protection to obtain lithium iron manganese phosphate material LiMn x Fe (1-x) PO4, where x is 0.30.

[0056] Example 2: The difference from Example 1 is that the reaction conditions for preparing the iron-containing precursor and the manganese-containing precursor, as well as the ratio of manganese to iron in the lithium manganese iron phosphate are adjusted.

[0057] Preparation of iron-containing precursor: using iron source ferric chloride (FeCl2) and first acid radical precipitant ammonium oxalate as raw materials, polyethylene glycol as the first dispersant, through chemical reaction: Fe 2+ +C2O4 2- +2H2O=FeC2O4·2H2O, and an iron-containing precursor precipitate is obtained. The reaction temperature is 48°C, the reaction time is 90 min, the pH value is 4.9, the stirring rate is 350 r / min, the molar ratio of ammonium oxalate to iron in ferric chloride is 1.15:1, and the amount of polyethylene glycol added is 1.8% of the total weight of ferric chloride, ammonium oxalate and polyethylene glycol.

[0058] Preparation of manganese-containing precursor: Using manganese source Marif salt (manganese dihydrogen phosphate) and second precipitant ammonium carbonate as raw materials, Berol 475 as second dispersant, through chemical reaction: Mn 2+ +CO3 2- =MnCO3, and a manganese-containing precursor precipitate is obtained. The reaction temperature is 56°C, the reaction time is 60 min, the pH value is 5.2, the stirring rate is 300 r / min, the molar ratio of ammonium carbonate to manganese in dihydrogen manganese phosphate is 1.12:1, and the addition amount of Berol 475 is 2.1% of the total weight of dihydrogen manganese phosphate, ammonium carbonate and Berol 475.

[0059] The iron-containing precursor and manganese-containing precursor precipitation products obtained in the above steps are mixed with lithium carbonate, ammonium dihydrogen phosphate and citric acid and ground evenly, and then sintered at 700°C to 820°C for 15h to 20h under nitrogen protection to obtain lithium iron manganese phosphate material LiMn x Fe (1-x) PO4, where x is 0.36.

[0060] Example 3: The difference from Example 1 is that the reaction conditions for preparing the iron-containing precursor and the manganese-containing precursor, as well as the ratio of manganese to iron in the lithium manganese iron phosphate are adjusted.

[0061] Preparation of iron-containing precursor: using iron source ferric chloride (FeCl2) and first acid radical precipitant ammonium oxalate as raw materials, polyethylene glycol as the first dispersant, through chemical reaction: Fe 2+ +C2O4 2- +2H2O=FeC2O4·2H2O, and an iron-containing precursor precipitate is obtained. The reaction temperature is 45°C, the reaction time is 82 min, the pH value is 4.9, the stirring rate is 250 r / min, the molar ratio of ammonium oxalate to iron in ferric chloride is 1.23:1, and the amount of polyethylene glycol added is 1.95% of the total weight of ferric chloride, ammonium oxalate and polyethylene glycol.

[0062] Preparation of manganese-containing precursor: Using manganese source Marif salt (manganese dihydrogen phosphate) and second precipitant ammonium carbonate as raw materials, Berol 475 as second dispersant, through chemical reaction: Mn 2+ +CO3 2- =MnCO3, to obtain a manganese-containing precursor precipitate. The reaction temperature is 70°C, the reaction time is 60 min, the pH value is 6.0, the stirring rate is 500 r / min, the molar ratio of ammonium carbonate to manganese in dihydrogen manganese phosphate is 1.0:1, and the addition amount of Berol 475 is 1.5% of the total weight of dihydrogen manganese phosphate, ammonium carbonate and Berol 475.

[0063] The iron-containing precursor and manganese-containing precursor precipitation products obtained in the above steps are mixed with lithium carbonate, ammonium dihydrogen phosphate and citric acid and ground evenly, and then sintered at 700°C to 820°C for 15h to 20h under nitrogen protection to obtain lithium iron manganese phosphate material LiMn x Fe (1-x) PO4, where x is 0.40.

[0064] Example 4: The difference from Example 1 is that the reaction conditions for preparing the iron-containing precursor and the manganese-containing precursor, as well as the ratio of manganese to iron in the lithium manganese iron phosphate are adjusted.

[0065] Preparation of iron-containing precursor: using iron source ferric chloride (FeCl2) and first acid radical precipitant ammonium oxalate as raw materials, polyethylene glycol as the first dispersant, through chemical reaction: Fe 2+ +C2O4 2- +2H2O=FeC2O4·2H2O, and an iron-containing precursor precipitate is obtained. The reaction temperature is 68°C, the reaction time is 120 min, the pH value is 5.7, the stirring rate is 380 r / min, the molar ratio of ammonium oxalate to iron in ferric chloride is 1.25:1, and the amount of polyethylene glycol added is 1.5% of the total weight of ferric chloride, ammonium oxalate and polyethylene glycol.

[0066] Preparation of manganese-containing precursor: Using manganese source Marif salt (manganese dihydrogen phosphate) and second precipitant ammonium carbonate as raw materials, Berol 475 as second dispersant, through chemical reaction: Mn 2+ +CO3 2- =MnCO3, and a manganese-containing precursor precipitate is obtained. The reaction temperature is 60°C, the reaction time is 60 min, the pH value is 6.2, the stirring rate is 400 r / min, the molar ratio of ammonium carbonate to manganese in dihydrogen manganese phosphate is 1.25:1, and the addition amount of Berol 475 is 2.8% of the total weight of dihydrogen manganese phosphate, ammonium carbonate and Berol 475.

[0067] The iron-containing precursor and manganese-containing precursor precipitation products obtained in the above steps are mixed with lithium carbonate, ammonium dihydrogen phosphate and citric acid and ground evenly, and then sintered at 700°C to 820°C for 15h to 20h under nitrogen protection to obtain lithium iron manganese phosphate material LiMn x Fe (1-x) PO4, where x is 0.45.

[0068] Example 5: The difference from Example 1 is that the reaction conditions for preparing the iron-containing precursor and the manganese-containing precursor, as well as the ratio of manganese to iron in the lithium manganese iron phosphate are adjusted.

[0069] Preparation of iron-containing precursor: using iron source ferric chloride (FeCl2) and first acid radical precipitant ammonium oxalate as raw materials, polyethylene glycol as the first dispersant, through chemical reaction: Fe 2+ +C2O4 2- +2H2O=FeC2O4·2H2O, and an iron-containing precursor precipitate is obtained. The reaction temperature is 63°C, the reaction time is 80 min, the pH value is 5.4, the stirring rate is 370 r / min, the molar ratio of ammonium oxalate to iron in ferric chloride is 1.29:1, and the amount of polyethylene glycol added is 0.85% of the total weight of ferric chloride, ammonium oxalate and polyethylene glycol.

[0070] Preparation of manganese-containing precursor: Using manganese source Marif salt (manganese dihydrogen phosphate) and second precipitant ammonium carbonate as raw materials, Berol 475 as second dispersant, through chemical reaction: Mn 2+ +CO3 2- =MnCO3, and a manganese-containing precursor precipitate is obtained. The reaction temperature is 63°C, the reaction time is 75 min, the pH value is 5.7, the stirring rate is 300 r / min, the molar ratio of ammonium carbonate to manganese in dihydrogen manganese phosphate is 1.15:1, and the addition amount of Berol 475 is 1.7% of the total weight of dihydrogen manganese phosphate, ammonium carbonate and Berol 475.

[0071] The iron-containing precursor and manganese-containing precursor precipitation products obtained in the above steps are mixed with lithium carbonate, ammonium dihydrogen phosphate and citric acid and ground evenly, and then sintered at 700°C to 820°C for 15h to 20h under nitrogen protection to obtain lithium iron manganese phosphate material LiMn x Fe (1-x) PO4, where x is 0.20.

[0072] Example 5: The difference from Example 1 is that the ratio of manganese to iron in lithium manganese iron phosphate is adjusted to 0.65

[0073] Preparation of iron-containing precursor: using iron source ferric chloride (FeCl2) and first acid radical precipitant ammonium oxalate as raw materials, polyethylene glycol as the first dispersant, through chemical reaction: Fe 2+ +C2O4 2- +2H2O=FeC2O4·2H2O, and an iron-containing precursor precipitate is obtained. The reaction temperature is 45°C, the reaction time is 70 min, the pH value is 4.8, the stirring rate is 300 r / min, the molar ratio of ammonium oxalate to iron in ferric chloride is 1.1:1, and the amount of polyethylene glycol added is 1.5% of the total weight of ferric chloride, ammonium oxalate and polyethylene glycol.

[0074] Preparation of manganese-containing precursor: Using manganese source Marif salt (manganese dihydrogen phosphate) and second precipitant ammonium carbonate as raw materials, Berol 475 as second dispersant, through chemical reaction: Mn 2+ +CO3 2- =MnCO3, and a manganese-containing precursor precipitate is obtained. The reaction temperature is 55°C, the reaction time is 50 min, the pH value is 5.6, the stirring rate is 280 r / min, the molar ratio of ammonium carbonate to manganese in dihydrogen manganese phosphate is 1.3:1, and the addition amount of Berol 475 is 2.3% of the total weight of dihydrogen manganese phosphate, ammonium carbonate and Berol 475.

[0075] The iron-containing precursor and manganese-containing precursor precipitation products obtained in the above steps are mixed with lithium carbonate, ammonium dihydrogen phosphate and citric acid and ground evenly, and then sintered at 700°C to 820°C for 15h to 20h under nitrogen protection to obtain lithium iron manganese phosphate material LiMn x Fe (1-x) PO4, where x is 0.65.

[0076] Comparative Example 1

[0077] Lithium carbonate, ferrous oxalate, manganese acetate and ammonium hydrogen phosphate are respectively used as lithium source, iron source, manganese source and phosphorus source, and sucrose is used as carbon source. The amount of sucrose is 15wt% of the total weight of lithium carbonate, ferrous oxalate, ammonium hydrogen phosphate, manganese acetate and sucrose. The above five raw materials are put into a ball mill according to the stoichiometric ratio, and the ball mill is carried out at a speed of 450r / min for 4.2h in a ball milling medium and alcohol environment. The ball-milled slurry is placed in a blast oven for drying to obtain a lithium iron phosphate precursor.

[0078] The precursor was pre-sintered at 680°C in a nitrogen atmosphere for 18 h and then calcined at 750°C for 13 h to obtain LiFe 0.5 Mn 0.5 PO4 material.

[0079] Performance / data testing:

[0080] The lithium manganese iron phosphate positive electrode materials prepared in Examples 1 to 6 and Comparative Example 1 were subjected to a 0.1C rate discharge specific capacity test and a 1C rate cycle 100 times efficiency test. The comparative test data are shown in Table 1.

[0081] Table 1 Performance test data of lithium manganese iron phosphate positive electrode materials in various embodiments and comparative examples

[0082] Manganese ratio in ferromanganese 0.1C first discharge specific capacity / mAh / g Cycle efficiency / % Example 1: 0.30 152.4 91.5 Example 2: 0.36 165.9 95.6 Example 3: 0.40 147.3 87.3 Example 4: 0.45 138.1 89.1 Example 5: 0.2 115.9 82.6 Example 6: 0.65 121.3 79.3 Comparative Example 1: 0.5 136.7 90.5

[0083] It can be seen from Table 1 that compared with Comparative Example 1 in which lithium iron manganese phosphate material is prepared by the traditional solid phase method, the electrode is made by preparing the lithium iron manganese phosphate positive electrode material obtained by separately preparing the iron-containing precursor and the manganese-containing precursor and controlling the iron-manganese ratio, thereby improving the electrical conductivity of the lithium iron manganese phosphate material and further improving the discharge specific capacity of the lithium battery, which solves the problem that the discharge specific capacity of the lithium iron manganese phosphate material obtained by the preparation method cannot meet the demand to a certain extent.

[0084] It should be understood that the size of the serial numbers of the steps in the above embodiments does not mean the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0085] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described or recorded in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0086] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.

Claims

1. A method for preparing a lithium manganese iron phosphate positive electrode material, characterized in that: include: S1, chemically reacting an iron source, a first acid radical precipitant and a first dispersant to obtain an iron-containing precursor; S2, chemically reacting a manganese source, a second acid radical precipitant and a second dispersant to obtain a manganese-containing precursor; S3, mixing and grinding the iron-containing precursor, the manganese-containing precursor, the lithium source, the phosphorus source and the carbon source to obtain a precursor mixture; S4, sintering the precursor mixture in a nitrogen atmosphere to obtain a lithium manganese iron phosphate positive electrode material; The general structural formula of the lithium manganese iron phosphate positive electrode material is LiMn x Fe (1-x) PO4, 0.3 <X<0.45。 2. The preparation method according to claim 1, characterized in that The reaction temperature of step S1 is 40° C. to 70° C., the reaction time is 30 min to 90 min, the pH value is 4.0 to 6.8, and the stirring rate is 200 r / min to 500 r / min.

3. The preparation method according to claim 1, characterized in that: The molar ratio of the first acid radical precipitant to the iron in the iron source in step S1 is (1.0-1.5):1; The amount of the first dispersant added in step S1 is 0.5% to 3.0% of the total weight of the iron source, the first acid radical precipitant and the first dispersant.

4. The preparation method according to claim 1, characterized in that: The reaction temperature of step S2 is 45° C. to 80° C., the reaction time is 30 min to 120 min, the pH value is 5.0 to 6.5, and the stirring rate is 200 r / min to 500 r / min.

5. The preparation method according to claim 1, characterized in that: The molar ratio of the second acid radical precipitant to the manganese in the manganese source in step S2 is (1.0-1.4):1; The amount of the second dispersant added in step S2 is 0.5% to 3.0% of the total weight of the manganese source, the second acid radical precipitant and the second dispersant.

6. The preparation method according to claim 1, characterized in that: The amount of the carbon source added in step S3 is 10% to 20% of the total weight of the iron-containing precursor, the manganese-containing precursor, the lithium source, the phosphorus source and the carbon source.

7. The preparation method according to claim 1, characterized in that: The sintering parameters of step S4 are as follows: the sintering temperature is 700° C. to 820° C., and the sintering time is 15 h to 20 h.

8. The preparation method according to claim 1, characterized in that: The iron source is one or more of ferrous chloride, ferrous sulfate, ferric phosphate, ferric oxide, ferrous oxalate and ferrous acetate; And / or, the lithium source is one or more combinations of lithium carbonate, lithium hydroxide, and lithium dihydrogen phosphate; And / or, the phosphorus source is one or more combinations of lithium dihydrogen phosphate, ammonium hydrogen phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate and phosphoric acid; And / or, the manganese source is one or more combinations of manganese dihydrogen phosphate, manganese tetraoxide, manganese dioxide, and manganese carbonate; And / or, the carbon source is one or more combinations of citric acid, glucose, sucrose, lactose, maltose, phenolic resin, carbon nanotubes and epoxy resin.

9. An electrode, characterized in that: The invention comprises a lithium manganese iron phosphate positive electrode material obtained by the preparation method according to any one of claims 1 to 8.

10. A lithium battery, characterized in that: The positive electrode of the lithium battery is made of the lithium iron manganese phosphate positive electrode material described in claim 9.

Citation Information

Patent Citations

  • Preparation method of lithium manganese iron phosphate positive electrode material

    CN114380280A

  • Method for preparing lithium manganese iron phosphate, cathode material, and lithium-ion battery

    US20230322557A1

  • Lithium manganese iron phosphate positive electrode material and preparation method therefor

    WO2024138863A1

Cited By

  • Manganese monohydrogen phosphate trihydrate production method, Mn-containing mother liquor recycling method and positive electrode material

    CN119911888A

  • Positive electrode active material and preparation method thereof, positive electrode plate and lithium ion battery

    CN122619779A