Preparation method of silicon carbide aerogel
Through the hybrid treatment and annealing technology of carbon skeleton precursor, carbon source and silicon source, SiC-SiO2 heterogeneous interface is formed, solving the brittleness and single function of silicon carbide aerogel, and achieving improved mechanical performance and versatility. Suitable for applications in complex environments.
Patent Information
- Application Number
- CN202410957746.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
The brittleness of silicon carbide aerogel leads to structural collapse and cannot adapt to extreme conditions in complex environments, such as strong electromagnetic interference, high temperatures and flame impacts. At the same time, its single function limits its application in deep space and deep exploration.
By mixing the carbon skeleton precursor, carbon source and silicon source, freeze-drying, sintering and two annealing treatments, SiC-SiO2 heterogeneous interface is formed, the framework structure and porosity are optimized, and the mechanical properties and versatility are improved.
It has achieved the improvement of the mechanical properties of silicon carbide aerogel, and has heat insulation, fire resistance and wide-band wave absorption capabilities, which are suitable for multifunctional applications in complex environments.
Smart Images

Figure CN118908215A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aerogel preparation, and in particular to a method for preparing silicon carbide aerogel. Background Art
[0002] Silicon carbide aerogel has great application potential in the fields of thermal insulation and wave absorption, and has received more and more widespread attention. However, the brittleness of the silicon carbide skeleton, especially when the local load is too large, may cause serious structural collapse, which seriously hinders its practical application. At the same time, with the exploration and development of deep space and deep earth space, service materials face a complex environment coupled with multiple extreme conditions, including strong electromagnetic interference, high temperature interference, flame impact, etc. However, most of the silicon carbide aerogels prepared so far have only a single function and cannot be used in complex environments. Summary of the invention
[0003] The main purpose of the present invention is to provide a method for preparing silicon carbide aerogel, aiming to make the prepared silicon carbide aerogel multifunctional so as to be suitable for complex environments.
[0004] To achieve the above object, the method for preparing silicon carbide aerogel proposed in the present invention comprises the following steps:
[0005] Mixing a carbon skeleton precursor, a carbon source, a silicon source and a solvent to obtain a precursor suspension;
[0006] Freezing and drying the precursor suspension to obtain a green body;
[0007] Sintering the green body to obtain an aerogel material;
[0008] The aerogel material is subjected to primary annealing and secondary annealing to obtain silicon carbide aerogel.
[0009] In one embodiment, in the step of mixing the carbon skeleton precursor, the carbon source, the silicon source and the solvent to obtain a precursor suspension:
[0010] The carbon skeleton precursor includes at least one of carbon fiber, polyacrylonitrile fiber, aramid fiber and phenolic fiber; and / or,
[0011] The carbon source comprises at least one of cellulose, chitosan and graphite powder; and / or,
[0012] The silicon source comprises at least one of silicon monoxide powder, silicon dioxide powder, silicon powder, methyltrimethoxysilane and tetraethyl orthosilicate; and / or,
[0013] The solvent includes at least one of water and ethanol.
[0014] In one embodiment, in the step of mixing the carbon skeleton precursor, the carbon source, the silicon source and the solvent to obtain a precursor suspension, the mass ratio of the carbon skeleton precursor, the carbon source, the silicon source and the solvent is (2-4):(1-2):(4-6):100.
[0015] In one embodiment, in the step of mixing the carbon skeleton precursor, the carbon source, the silicon source and the solvent to obtain a precursor suspension, the carbon skeleton precursor, the carbon source, the silicon source and the solvent are mixed by mechanical stirring.
[0016] In one embodiment, the rotation speed of the mechanical stirring is 100 to 200 r / min; and / or,
[0017] The mechanical stirring time is 0.5 to 2 hours.
[0018] In one embodiment, in the step of freezing and drying the precursor suspension to obtain a green body:
[0019] The freezing temperature is -40 to -30°C; and / or,
[0020] The freezing time is 16 to 28 hours.
[0021] In one embodiment, in the step of freezing and drying the precursor suspension to obtain a green body, the drying is vacuum drying, wherein:
[0022] The vacuum drying pressure is 1-20 Pa; and / or,
[0023] The vacuum drying time is 18 to 36 hours.
[0024] In one embodiment, in the step of sintering the green body to obtain the aerogel material, the sintering method comprises heating to a sintering temperature and then maintaining the temperature, wherein:
[0025] The heating rate is 5-10°C / min; and / or,
[0026] The sintering temperature is 1300-1500° C.; and / or,
[0027] The insulation time is 2 to 3 hours.
[0028] In one embodiment, in the step of subjecting the aerogel material to primary annealing and secondary annealing to obtain silicon carbide aerogel, the primary annealing method comprises heating to the primary annealing temperature and then maintaining the temperature, wherein:
[0029] The heating rate is 2-5°C / min; and / or,
[0030] The primary annealing temperature is 700-800° C.; and / or,
[0031] The insulation time is 0.5 to 2 hours.
[0032] In one embodiment, in the step of subjecting the aerogel material to primary annealing and secondary annealing to obtain silicon carbide aerogel, the secondary annealing method comprises heating to a secondary annealing temperature and then maintaining the temperature, wherein:
[0033] The heating rate is 8-10°C / min; and / or,
[0034] The secondary annealing temperature is 1000-1100° C.; and / or,
[0035] The insulation time is 0.5 to 1.5 hours.
[0036] In the technical solution provided by the present invention, the aerogel material obtained by sintering is first annealed to etch and remove the unreacted part of the skeleton, optimize the skeleton structure, and improve the porosity. At the same time, the structure is cross-linked and strengthened to a certain extent, which can ensure the stability of the crystal structure during the secondary annealing process; and then a secondary annealing is performed to actively oxidize the surface of the silicon carbide nanostructure to form SiC-SiO2 (silicon carbide-silicon dioxide) and crystalline SiO2-amorphous SiO2 heterogeneous interfaces. These heterogeneous interfaces can inhibit phonon heat conduction and electromagnetic wave propagation, and also prevent further oxidation and sintering of SiC. Through two annealings, grain sintering during the annealing process can be avoided, and dual regulation of the pore structure and the interface structure can be achieved; thereby, the mechanical properties of the prepared silicon carbide aerogel are not only enhanced, but also the integration of multiple functions such as heat insulation, fire prevention and wave absorption is achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0038] Figure 1 A partial schematic diagram of an embodiment of a method for preparing silicon carbide aerogel provided by the present invention;
[0039] Figure 2 This is a physical picture of the silicon carbide aerogel prepared in Example 1;
[0040] Figure 3 This is a scanning electron microscope (SEM) image of the silicon carbide aerogel prepared in Example 1;
[0041] Figure 4 This is an X-ray photoelectron spectroscopy (XPS) graph of the silicon carbide aerogel prepared in Comparative Example 1;
[0042] Figure 5 is an X-ray diffraction (XRD) pattern of the silicon carbide aerogel prepared in Example 1;
[0043] Figure 6 2D wave absorption performance diagram of silicon carbide aerogel prepared in Example 2;
[0044] Figure 7 This is a thermogravimetric curve of the silicon carbide aerogel prepared in Example 2 under air;
[0045] Figure 8 This is an infrared thermal image of the silicon carbide aerogel prepared in Example 2 under a high temperature flame;
[0046] Fig. 9 1 is a stress-strain diagram of the silicon carbide aerogels prepared in Example 2 and Comparative Example 1;
[0047] Fig.10 The thermal conductivity curve of silicon carbide aerogel prepared in Example 3 and Comparative Example 1;
[0048] Fig.11 This is a scanning electron microscope (SEM) image of the silicon carbide aerogel prepared in Comparative Example 1.
[0049] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0050] To make the purpose, technical scheme and advantages of the embodiment of the present invention clearer, the technical scheme in the embodiment of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiment, it is carried out according to the normal conditions or the conditions recommended by the manufacturer. If the reagents or instruments used do not specify the manufacturer, they are all conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, taking "A and / or B" as an example, including scheme A, or scheme B, or schemes that A and B meet at the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of technical solutions is contradictory or cannot be achieved, it should be considered that the combination of such technical solutions does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention.
[0051] Silicon carbide aerogel has great application potential in the fields of thermal insulation and wave absorption, and has received more and more widespread attention. However, the brittleness of the silicon carbide skeleton, especially when the local load is too large, may cause serious structural collapse, which seriously hinders its practical application. At the same time, with the exploration and development of deep space and deep earth space, service materials face a complex environment coupled with multiple extreme conditions, including strong electromagnetic interference, high temperature interference, flame impact, etc. However, most of the silicon carbide aerogels prepared so far have only a single function and cannot be used in complex environments.
[0052] In view of this, the present invention proposes a method for preparing silicon carbide aerogel, which can not only enhance and improve the mechanical properties of the prepared silicon carbide aerogel, but also integrate multiple functions such as heat insulation, fire prevention and wave absorption.
[0053] In the embodiments of the present invention, please refer to Figure 1 , the preparation method of the silicon carbide aerogel comprises the following steps:
[0054] S10, mixing a carbon skeleton precursor, a carbon source, a silicon source and a solvent to obtain a precursor suspension;
[0055] S20, freezing and drying the precursor suspension to obtain a green body;
[0056] S30, sintering the green body to obtain an aerogel material;
[0057] S40, performing primary annealing and secondary annealing on the aerogel material to obtain silicon carbide aerogel.
[0058] In the technical solution provided by the present invention, the aerogel material obtained by sintering is first annealed to etch and remove the unreacted part of the skeleton, optimize the skeleton structure, and improve the porosity. At the same time, the structure is cross-linked and strengthened to a certain extent, which can ensure the stability of the crystal structure during the secondary annealing process; and then a secondary annealing is performed to actively oxidize the surface of the silicon carbide nanostructure to form SiC-SiO2 and crystalline SiO2-amorphous SiO2 heterogeneous interfaces. These heterogeneous interfaces can inhibit phonon heat conduction and electromagnetic wave propagation, and also prevent further oxidation and sintering of SiC. Through two annealings, grain sintering during the annealing process can be avoided, and dual regulation of the pore structure and the interface structure can be achieved; thereby, the mechanical properties of the prepared silicon carbide aerogel are not only enhanced, but also the integration of multiple functions such as heat insulation, fire prevention and wave absorption is achieved.
[0059] In an embodiment of the present invention, in step S10, the carbon skeleton precursor includes at least one of carbon fiber, polyacrylonitrile fiber, aramid fiber and phenolic fiber. Using at least one of the above carbon skeleton precursors is conducive to improving the performance of the prepared silicon carbide aerogel. The carbon skeleton precursor can be any one of carbon fiber, polyacrylonitrile fiber, aramid fiber and phenolic fiber or any combination of multiple thereof.
[0060] In an embodiment of the present invention, in step S10, the carbon source includes at least one of cellulose, chitosan and graphite powder. Using at least one of the above carbon sources is conducive to improving the performance of the prepared silicon carbide aerogel. The carbon source can be any one of cellulose, chitosan and graphite powder or any combination of multiple thereof.
[0061] In an embodiment of the present invention, in step S10, the silicon source includes at least one of silicon monoxide powder, silicon dioxide powder, silicon powder, methyltrimethoxysilane and tetraethyl orthosilicate. Using at least one of the above silicon sources is conducive to improving the performance of the prepared silicon carbide aerogel. The silicon source can be any one of silicon monoxide powder, silicon dioxide powder, silicon powder, methyltrimethoxysilane and tetraethyl orthosilicate, or any combination of multiple thereof.
[0062] In an embodiment of the present invention, in step S10, the solvent includes at least one of water and ethanol. Using at least one of the above solvents is conducive to improving the performance of the prepared silicon carbide aerogel. The solvent can be water, ethanol, or a mixed solvent consisting of water and ethanol.
[0063] In an embodiment of the present invention, in step S10, the mass ratio of the carbon skeleton precursor, the carbon source, the silicon source and the solvent is (2-4): (1-2): (4-6): 100. The mass ratio of the carbon skeleton precursor, the carbon source, the silicon source and the solvent is within this range, which is beneficial to improving the mechanical properties of the prepared silicon carbide aerogel. The mass ratio of the carbon skeleton precursor, the carbon source, the silicon source and the solvent can be 2:1:4:100, 4:1:4:100, 2:2:4:100, 4:2:4:100, 2:1:6:100, 4:1:6:100, 2:2:6:100, 4:2:6:100 or 3:2:6:100.
[0064] In an embodiment of the present invention, in step S10, the carbon skeleton precursor, the carbon source, the silicon source and the solvent are mixed by mechanical stirring. Mechanical stirring is used to mix the raw materials uniformly, which can improve the uniformity of the precursor suspension, and is easy to operate and low in cost.
[0065] Further, in an embodiment of the present invention, the rotation speed of the mechanical stirring is 100 to 200 r / min. The rotation speed of the mechanical stirring is within this range, which is conducive to improving the uniformity of the precursor suspension. The rotation speed of the mechanical stirring can be 100 r / min, 120 r / min, 140 r / min, 160 r / min, 180 r / min or 200 r / min.
[0066] In an embodiment of the present invention, the mechanical stirring time is 0.5 to 2 hours. The mechanical stirring time within this range is beneficial to improving the uniformity of the precursor suspension. The mechanical stirring time can be 0.5 hours, 1 hour, 1.5 hours or 2 hours.
[0067] In an embodiment of the present invention, in step S20, the freezing temperature is -40 to -30°C. The freezing temperature within this range is conducive to forming a green body with a suitable structure to improve the performance of the prepared silicon carbide aerogel. The freezing temperature can be -40°C, -35°C or -30°C.
[0068] In an embodiment of the present invention, in step S20, the freezing time is 16 to 28 hours. The freezing time within this range is conducive to forming a green body with a suitable structure to improve the performance of the prepared silicon carbide aerogel. The freezing time can be 16 hours, 22 hours or 28 hours.
[0069] In an embodiment of the present invention, in step S20, the drying is vacuum drying, wherein the pressure of the vacuum drying is 1 to 20 Pa. The vacuum drying pressure within this range is conducive to forming a green body with a suitable structure to improve the performance of the obtained silicon carbide aerogel. The vacuum drying pressure can be 1Pa, 5Pa, 10Pa, 15Pa or 20Pa.
[0070] In an embodiment of the present invention, in step S20, the drying is vacuum drying, wherein the vacuum drying time is 18 to 36 hours. The vacuum drying time within this range is conducive to forming a green body with a suitable structure to improve the performance of the obtained silicon carbide aerogel. The vacuum drying time can be 18 hours, 24 hours, 30 hours or 36 hours.
[0071] In an embodiment of the present invention, in step S30, the sintering method includes heating to the sintering temperature and then keeping the temperature, wherein the heating rate is 5 to 10°C / min. During sintering, the heating rate is within this range, which is conducive to improving the performance of the obtained silicon carbide aerogel. During sintering, the heating rate can be 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min.
[0072] In an embodiment of the present invention, in step S30, the sintering method includes heating to a sintering temperature and then keeping the temperature, wherein the sintering temperature is 1300-1500°C. The sintering temperature within this range is conducive to improving the performance of the obtained silicon carbide aerogel. The sintering temperature can be 1300°C, 1350°C, 1400°C, 1450°C or 1500°C.
[0073] In an embodiment of the present invention, in step S30, the sintering method includes heating to a sintering temperature and then keeping the temperature, wherein the holding time is 2 to 3 hours. During sintering, the holding time at the sintering temperature is within this range, which is beneficial to improving the performance of the obtained silicon carbide aerogel. The holding time can be 2 hours, 2.5 hours or 3 hours.
[0074] In an embodiment of the present invention, in step S40, the method of the primary annealing includes heating to the primary annealing temperature and then keeping the temperature, wherein the heating rate is 2 to 5°C / min. In the primary annealing, the heating rate is within this range, which is conducive to etching and removing the unreacted part of the aerogel material skeleton, optimizing the skeleton structure, and improving the porosity. At the same time, the structure is cross-linked and strengthened to a certain extent, which can ensure the stability of the crystal structure during the secondary annealing process, and thus is conducive to improving the performance of the prepared silicon carbide aerogel. In the primary annealing, the heating rate can be 5°C / min, 3°C / min, 4°C / min or 5°C / min.
[0075] In an embodiment of the present invention, in step S40, the method of the primary annealing includes heating to the primary annealing temperature and then keeping the temperature, wherein the primary annealing temperature is 700-800°C. The primary annealing temperature within this range is conducive to etching and removing the unreacted part of the aerogel material skeleton, optimizing the skeleton structure, and improving the porosity. At the same time, the structure is cross-linked and strengthened to a certain extent, which can ensure the stability of the crystal structure during the secondary annealing process, and thus is conducive to improving the performance of the prepared silicon carbide aerogel. The primary annealing temperature can be 700°C, 720°C, 740°C, 760°C, 780°C or 800°C.
[0076] In an embodiment of the present invention, in step S40, the method of the primary annealing includes heating to the primary annealing temperature and then keeping the temperature, wherein the holding time is 0.5 to 2 hours. In the primary annealing, the holding time at the primary annealing temperature is within this range, which is conducive to etching and removing the unreacted part of the aerogel material skeleton, optimizing the skeleton structure, and improving the porosity. At the same time, the structure is cross-linked and strengthened to a certain extent, which can ensure the stability of the crystal structure during the secondary annealing process, and thus is conducive to improving the performance of the prepared silicon carbide aerogel. The holding time can be 0.5h, 1h, 1.5h or 2h.
[0077] In an embodiment of the present invention, in step S40, the secondary annealing method includes heating to the secondary annealing temperature and then keeping the temperature, wherein the heating rate is 8 to 10°C / min. In the secondary annealing, the heating rate is within this range, which is conducive to forming a heterogeneous interface of SiC-SiO2 and crystalline SiO2-amorphous SiO2, and preventing further oxidation and sintering of SiC, thereby helping to improve the performance of the obtained silicon carbide aerogel. In the secondary annealing, the heating rate can be 8°C / min, 9°C / min or 10°C / min.
[0078] In an embodiment of the present invention, in step S40, the secondary annealing method includes heating to a secondary annealing temperature and then keeping the temperature, wherein the secondary annealing temperature is 1000-1100°C. The secondary annealing temperature within this range is conducive to forming a heterogeneous interface of SiC-SiO2 and crystalline SiO2-amorphous SiO2, and preventing further oxidation and sintering of SiC, thereby helping to improve the performance of the obtained silicon carbide aerogel. The secondary annealing temperature can be 1000°C, 1050°C or 1100°C.
[0079] In an embodiment of the present invention, in step S40, the secondary annealing method includes heating to the secondary annealing temperature and then keeping the temperature, wherein the holding time is 0.5 to 1.5 hours. In the secondary annealing, the holding time at the secondary annealing temperature is within this range, which is conducive to forming the heterogeneous interface of SiC-SiO2 and crystalline SiO2-amorphous SiO2, and preventing further oxidation and sintering of SiC, thereby helping to improve the performance of the obtained silicon carbide aerogel. The holding time can be 0.5 hours, 1 hour or 1.5 hours.
[0080] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.
[0081] Example 1
[0082] Take 2g of carbon fiber, 2g of cellulose, 6g of silicon monoxide powder, 50mL of ethanol and 50mL of water in a beaker, mix and stir evenly to form a precursor suspension; pour the precursor suspension into a polytetrafluoroethylene mold, freeze it at -30°C for 24h, then take out the frozen sample, and vacuum dry it at a pressure of 1Pa for 24h to obtain a green body; place the green body in a sintering furnace for sintering, heat it to 1400°C at a heating rate of 10°C / min, and keep it warm for 2h to obtain an aerogel material; anneal the obtained aerogel material once, heat it to 800°C at a heating rate of 2°C / min, keep it warm for 1h, and take it out after cooling; anneal it twice, heat it to 1000°C at a heating rate of 10°C / min, and keep it warm for 1h to obtain silicon carbide aerogel.
[0083] See also Figure 2 The size of the silicon carbide aerogel prepared in Example 1 is 7×7 cm 2 .
[0084] The silicon carbide aerogel obtained in Example 1 was observed by scanning electron microscopy. Figure 3 shown.
[0085] See also Figure 3 It can be seen that the prepared silicon carbide aerogel has a multi-level skeleton structure, including a micron-scale hollow tube structure (5-10 μm) and a nanowire structure (10-50 nm), and the element mapping diagram shows that these skeleton structures are composed of Si, O, and C elements.
[0086] The silicon carbide aerogel prepared in Example 1 was subjected to X-ray photoelectron spectroscopy test, and the results were as follows: Figure 4 shown.
[0087] See also Figure 4 , it can be seen that there are Si-C bonds and Si-O bonds in the prepared silicon carbide aerogel, corresponding to SiC and SiO2.
[0088] The silicon carbide aerogel prepared in Example 1 was subjected to an X-ray diffraction test, and the results are as follows: Figure 5 shown.
[0089] See also Figure 5 , it can be seen that the prepared silicon carbide aerogel contains SiO2 crystals and SiC crystals.
[0090] The 2D wave absorbing performance of the silicon carbide aerogel prepared in Example 1 was tested. The results are as follows: Figure 6 shown.
[0091] See also Figure 6 It can be seen that the effective absorption bandwidth of the prepared silicon carbide aerogel reaches 6.7 GHz.
[0092] The thermogravimetric analysis curve of the silicon carbide aerogel prepared in Example 1 was tested, and the results were as follows: Figure 7 shown.
[0093] See also Figure 7 It can be seen that the high temperature resistance of the prepared silicon carbide aerogel reaches above 1280°C.
[0094] The above physical characterizations all indicate that there is a SiO2-SiC heterointerface structure inside the aerogel. The heterointerface effectively suppresses the thermal motion of phonons and reduces the thermal conductivity of the material. At the same time, the heterointerface regulates the dielectric properties of silicon carbide aerogel and optimizes the impedance matching, so that its effective absorption bandwidth reaches 6.7 GHz. In addition, the SiO2 layer in the heterointerface can also act as a barrier, effectively preventing further oxidation failure of the material at high temperature, thereby improving its high temperature resistance to above 1280°C.
[0095] Example 2
[0096] Take 3g of carbon fiber, 2g of cellulose, 6g of silicon monoxide powder, 50mL of ethanol and 50mL of water in a beaker, mix and stir evenly to form a precursor suspension; pour the precursor suspension into a polytetrafluoroethylene mold, freeze it at -30°C for 24h, then take out the frozen sample, and vacuum dry it at a pressure of 1Pa for 24h to obtain a green body; place the green body in a sintering furnace for sintering, heat it to 1400°C at a heating rate of 10°C / min, and keep it warm for 2h to obtain an aerogel material; anneal the obtained aerogel material once, heat it to 800°C at a heating rate of 2°C / min, keep it warm for 1h, and take it out after cooling; anneal it twice, heat it to 1000°C at a heating rate of 10°C / min, and keep it warm for 1h to obtain silicon carbide aerogel.
[0097] The high temperature thermal insulation capability of the silicon carbide aerogel prepared in Example 2 was tested by simulating a high temperature environment with a butane spray gun. The results are as follows: Figure 8 shown.
[0098] See also Figure 8 It can be seen that the temperature of the heated surface of the prepared silicon carbide aerogel is as high as 1150°C. After heating for 20 minutes, the temperature of the back-fired surface remains at around 80°C, and the temperature difference between the two surfaces reaches more than 1000°C, indicating its excellent high-temperature thermal insulation performance.
[0099] The compressive properties of the silicon carbide aerogel prepared in Example 2 were tested by uniaxial compression. The results are as follows: Fig. 9 shown.
[0100] See also Fig. 9 It can be seen that the maximum compressive stress of the prepared silicon carbide aerogel reaches 1.83MPa, which is significantly improved by more than 10 times compared with the traditional silicon carbide aerogel (hundreds of kilopascals). This mechanical enhancement effect is due to the introduction of a multi-level skeleton, which enables effective stress transmission and dissipation, reducing structural damage caused by stress concentration.
[0101] Example 3
[0102] Take 4g of carbon fiber, 2g of cellulose, 6g of silicon monoxide powder, 50mL of ethanol and 50mL of water in a beaker, mix and stir evenly to form a precursor suspension; pour the precursor suspension into a polytetrafluoroethylene mold, freeze it at -30°C for 24h, then take out the frozen sample, and vacuum dry it at a pressure of 1Pa for 24h to obtain a green body; place the green body in a sintering furnace for sintering, heat it to 1400°C at a heating rate of 10°C / min, and keep it warm for 2h to obtain an aerogel material; anneal the obtained aerogel material once, heat it to 800°C at a heating rate of 2°C / min, keep it warm for 1h, and take it out after cooling; anneal it twice, heat it to 1000°C at a heating rate of 10°C / min, and keep it warm for 1h to obtain silicon carbide aerogel.
[0103] The thermal conductivity of the silicon carbide aerogel prepared in Example 3 was measured using a laser thermal conductivity meter. The results are as follows: Fig.10 shown.
[0104] See also Fig.10 It can be seen that with the increase of temperature, the thermal conductivity of the prepared silicon carbide aerogel increases, which is due to the enhanced thermal radiation, but even at a high temperature of 600°C, its thermal conductivity is only 0.053W / m·K, indicating its excellent high-temperature thermal insulation performance.
[0105] Example 4
[0106] Take 4g of carbon fiber, 2g of cellulose, 6g of silicon monoxide powder, 50mL of ethanol and 50mL of water in a beaker, mix and stir evenly to form a precursor suspension; pour the precursor suspension into a polytetrafluoroethylene mold, freeze it at -30°C for 24h, then take out the frozen sample, and vacuum dry it at a pressure of 1Pa for 24h to obtain a green body; place the green body in a sintering furnace for sintering, heat it to 1400°C at a heating rate of 10°C / min, and keep it warm for 2h to obtain an aerogel material; anneal the obtained aerogel material once, heat it to 700°C at a heating rate of 2°C / min, keep it warm for 0.5h, and take it out after cooling; anneal it twice, heat it to 1000°C at a heating rate of 8°C / min, and keep it warm for 0.5h to obtain silicon carbide aerogel.
[0107] Example 5
[0108] Take 4g of carbon fiber, 2g of cellulose, 6g of silicon monoxide powder, 50mL of ethanol and 50mL of water in a beaker, mix and stir evenly to form a precursor suspension; pour the precursor suspension into a polytetrafluoroethylene mold, freeze it at -30°C for 24h, then take out the frozen sample, and vacuum dry it at a pressure of 1Pa for 24h to obtain a green body; place the green body in a sintering furnace for sintering, heat it to 1400°C at a heating rate of 10°C / min, and keep it warm for 2h to obtain an aerogel material; anneal the obtained aerogel material once, heat it to 800°C at a heating rate of 5°C / min, keep it warm for 2h, and take it out after cooling; anneal it twice, heat it to 1100°C at a heating rate of 10°C / min, and keep it warm for 1.5h to obtain silicon carbide aerogel.
[0109] Comparative Example 1
[0110] Take 4g of carbon fiber, 2g of cellulose, 6g of silicon monoxide powder, 50mL of ethanol and 50mL of water in a beaker, mix and stir evenly to form a precursor suspension; pour the precursor suspension into a polytetrafluoroethylene mold, freeze it at -30°C for 24h, then take out the frozen sample, and vacuum dry it at a pressure of 1Pa for 24h to obtain a green body; place the green body in a sintering furnace, heat it to 1400°C at a heating rate of 10°C / min, and keep it warm for 2h to obtain an aerogel material; anneal the obtained aerogel material, heat it to 1000°C at a heating rate of 10°C / min, and keep it warm for 1h to obtain silicon carbide aerogel.
[0111] The silicon carbide aerogel prepared in Comparative Example 1 was observed by scanning electron microscopy. Fig.11 shown.
[0112] See also Fig.11 It can be seen that the surface grains of the prepared silicon carbide aerogel are coarsened.
[0113] The compressive properties of the silicon carbide aerogel prepared in Comparative Example 1 were tested by uniaxial compression. The results are as follows: Fig. 9 shown.
[0114] See also Fig. 9 It can be seen that the compressive strength of the prepared silicon carbide aerogel is only 0.03MPa, and the structural brittleness is greatly increased.
[0115] The thermal conductivity of the silicon carbide aerogel prepared in Comparative Example 1 was measured using a laser thermal conductivity meter. The results are as follows: Fig.10 shown.
[0116] See also Fig.10It can be seen that the thermal conductivity of the prepared silicon carbide aerogel at a high temperature of 600°C reaches 0.12 W / m·K, while the thermal conductivity of the silicon carbide aerogel prepared in Example 3 at 600°C is only 0.053 W / m·K.
[0117] The performance parameters of the silicon carbide aerogels prepared in Examples 1 to 5 and Comparative Example 1 were tested and summarized. The performance parameters included porosity (%), density (g / cm 3 ), maximum compressive stress (MPa), absorption frequency bandwidth (GHz) and thermal conductivity at room temperature (W / m·K). The results are shown in Table 1.
[0118] Table 1 Performance parameters of silicon carbide aerogels prepared in Examples 1 to 5 and Comparative Example 1
[0119]
[0120] It can be seen from Table 1 that, compared with Comparative Example 1, the maximum compressive stress of the silicon carbide aerogels prepared in Examples 1 to 5 is increased, the absorption frequency width is increased, and the thermal conductivity is reduced.
[0121] The above results show that the silicon carbide aerogel prepared by the preparation method of the present invention not only has enhanced and improved mechanical properties, but also realizes the integration of multiple functions of heat insulation, fire prevention and wave absorption; in terms of mechanical properties, thanks to the introduction of the multi-level skeleton structure, the silicon carbide aerogel has excellent compressive resistance, and the maximum compressive strength can reach 2.63Mpa; in terms of thermal insulation performance, due to the optimization and regulation of the pore structure and the interface structure in the two annealing processes, the silicon carbide aerogel exhibits an ultra-low thermal conductivity, the thermal conductivity at room temperature can reach 0.021W / m·K, and the thermal conductivity at 600°C can reach 0.053W / m·K); in terms of fire resistance, the silicon carbide aerogel can withstand the impact of 1200°C flames, showing excellent fire resistance; in terms of electromagnetic wave absorption performance, the silicon carbide aerogel has an ultra-wide band electromagnetic wave absorption capability, and the absorption frequency width can reach 6.7GHz.
[0122] The above description is only an exemplary embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for preparing silicon carbide aerogel, characterized in that: The following steps are involved: Mixing a carbon skeleton precursor, a carbon source, a silicon source and a solvent to obtain a precursor suspension; Freezing and drying the precursor suspension to obtain a green body; Sintering the green body to obtain an aerogel material; The aerogel material is subjected to primary annealing and secondary annealing to obtain silicon carbide aerogel.
2. The method for preparing silicon carbide aerogel according to claim 1, characterized in that: In the step of mixing the carbon skeleton precursor, the carbon source, the silicon source and the solvent to obtain a precursor suspension: The carbon skeleton precursor includes at least one of carbon fiber, polyacrylonitrile fiber, aramid fiber and phenolic fiber; and / or, The carbon source comprises at least one of cellulose, chitosan and graphite powder; and / or, The silicon source comprises at least one of silicon monoxide powder, silicon dioxide powder, silicon powder, methyltrimethoxysilane and tetraethyl orthosilicate; and / or, The solvent includes at least one of water and ethanol.
3. The method for preparing silicon carbide aerogel according to claim 1, characterized in that: In the step of mixing the carbon skeleton precursor, the carbon source, the silicon source and the solvent to obtain a precursor suspension, the mass ratio of the carbon skeleton precursor, the carbon source, the silicon source and the solvent is (2-4):(1-2):(4-6):
100.
4. The method for preparing silicon carbide aerogel according to claim 1, characterized in that: In the step of mixing the carbon skeleton precursor, the carbon source, the silicon source and the solvent to obtain a precursor suspension, the carbon skeleton precursor, the carbon source, the silicon source and the solvent are mixed by mechanical stirring.
5. The method for preparing silicon carbide aerogel according to claim 4, characterized in that: The rotation speed of the mechanical stirring is 100-200 r / min; and / or, The mechanical stirring time is 0.5 to 2 hours.
6. The method for preparing silicon carbide aerogel according to claim 1, characterized in that: In the step of freezing and drying the precursor suspension to obtain a green body: The freezing temperature is -40 to -30°C; and / or, The freezing time is 16 to 28 hours.
7. The method for preparing silicon carbide aerogel according to claim 1, characterized in that: In the step of freezing and drying the precursor suspension to obtain a green body, the drying is vacuum drying, wherein: The vacuum drying pressure is 1-20 Pa; and / or, The vacuum drying time is 18 to 36 hours.
8. The method for preparing silicon carbide aerogel according to claim 1, characterized in that: In the step of sintering the green body to obtain the aerogel material, the sintering method comprises heating to a sintering temperature and then maintaining the temperature, wherein: The heating rate is 5-10°C / min; and / or, The sintering temperature is 1300-1500° C.; and / or, The insulation time is 2 to 3 hours.
9. The method for preparing silicon carbide aerogel according to claim 1, characterized in that: In the step of subjecting the aerogel material to primary annealing and secondary annealing to obtain silicon carbide aerogel, the primary annealing method comprises heating to the primary annealing temperature and then maintaining the temperature, wherein: The heating rate is 2-5°C / min; and / or, The primary annealing temperature is 700-800° C.; and / or, The insulation time is 0.5 to 2 hours.
10. The method for preparing silicon carbide aerogel according to claim 1, characterized in that: In the step of subjecting the aerogel material to primary annealing and secondary annealing to obtain silicon carbide aerogel, the secondary annealing method comprises heating to a secondary annealing temperature and then maintaining the temperature, wherein: The heating rate is 8-10°C / min; and / or, The secondary annealing temperature is 1000-1100° C.; and / or, The insulation time is 0.5 to 1.5 hours.
Citation Information
Patent Citations
Method for improving mechanical property and heat-insulating property of silicon carbide nanowire aerogel through oxidation treatment
CN114773092A
Wave-absorbing and heat-insulating integrated micron hollow tube SiC aerogel as well as preparation method and application thereof
CN118324139A