Cascade separation and extraction co-production method for valuable elements in red mud
Through high-concentration sulfuric acid high-temperature acid leaching and step-by-step treatment steps, iron, aluminum, titanium and sodium elements in red mud were successfully recovered, forming a variety of high-value-added products, solving the problems of red mud treatment and resource utilization, and simplifying the process flow And reduce costs.
Patent Information
- Application Number
- CN202410973374.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art is difficult to effectively treat and refine the use of iron, aluminum and titanium elements in red mud, and the process flow is complex and the cost is high, resulting in serious environmental problems caused by the accumulation of red mud.
High-temperature acid leaching is carried out by high-concentration sulfuric acid. Through a series of step-by-step treatment steps, including stir leaching, cooling crystallization, precipitation reaction and hydrothermal synthesis, the sodium hexamodefluorate, titanium-doped iron phosphate and calcium sulfate whiskers are successfully recovered. These products can achieve efficient utilization of iron, aluminum, titanium and sodium in red mud.
The high-value utilization of iron, aluminum, titanium and sodium elements in red mud has been achieved, which reduces raw material costs, increases product added value, and simplifies the process flow, solving the problems of red mud accumulation and resource utilization.
Smart Images

Figure BDA0004953866080000041 
Figure BDA0004953866080000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of industrial solid waste resource utilization, and in particular to a method for the stepwise separation, extraction and co-production of valuable elements in red mud. Background Art
[0002] Red mud is a difficult-to-handle byproduct of alumina production. It is red due to its high alkalinity and rich iron content, and has become a major problem in solid waste treatment. In 2020, my country's bauxite production accounted for 24% of the world's total, and its bauxite imports accounted for 80% of the world's total; red mud production accounted for 55% of the world's total, about 100 million tons. The cumulative stockpile of red mud in the world has exceeded 5 billion tons. At present, the amount of red mud added each year continues to increase at a rate of about 200 million tons, and the environmental problems caused by its accumulation are gradually becoming a serious threat to the sustainable development of the aluminum industry. This challenge is faced by the global aluminum industry in common, and effective measures are urgently needed to address it.
[0003] In recent years, there have been many studies on the recovery of valuable metals such as iron and aluminum in red mud. Patent CN109250737B discloses a method for extracting aluminum from Bayer red mud. The Bayer red mud is mixed with alkali solution and limestone for dissolution reaction. After the reaction is completed, a red mud dissolution slurry is obtained. The red mud dissolution slurry is diluted to Na 2 The concentration of O is 400-450g / L, and then separated by sedimentation to obtain dealuminated red mud and sodium aluminate solution. Patent CN106111051B discloses a method for extracting iron and aluminum from red mud to prepare an adsorbent, which specifically includes: 1. Acid leaching of red mud: leaching iron and aluminum from red mud with dilute hydrochloric acid; 2. Separation and purification of iron and aluminum: adding sodium hydroxide to the leachate to generate a precipitate and perform solid-liquid separation, adding dilute hydrochloric acid to the precipitate to prepare a ferric chloride solution, evaporating and concentrating it, cooling and crystallizing it to obtain ferric chloride hexahydrate, adding dilute hydrochloric acid to the supernatant to prepare an aluminum chloride solution, evaporating and concentrating it, cooling and crystallizing it to obtain aluminum chloride hexahydrate; 3. Preparation of adsorbent: using ferric chloride and aluminum chloride obtained from red mud as the main raw materials, adjusting the pH by coprecipitation at room temperature to obtain a precipitate, and then washing, drying, and grinding to obtain an adsorbent. Patent CN103031443A discloses a method for removing sodium from red mud and recovering aluminum and iron. The specific steps are: mixing red mud with sulfuric acid, then roasting or stirring and leaching, and then immersing, washing and filtering the roasting or leaching product. The Na in the solid residue is 2 The O content can be reduced to below 1%, and the aluminum and iron in the solution are recovered by neutralization precipitation, resin adsorption and other methods. The above patented methods generally only separate and extract a certain element in red mud, and the products obtained are relatively single. The resource utilization of other elements in red mud is not high, the separation of iron and titanium is relatively difficult, and the new solid and liquid wastes need to be processed, and the process technology products are difficult to promote and apply.
[0004] The preparation methods of titanium-doped iron phosphate include hydrothermal method, solid phase method and coprecipitation method. Patent CN111498825A discloses a preparation method of titanium-doped lithium iron phosphate. Titanium tetrachloride is introduced into phosphoric acid solution, and then the reaction slurry is placed in a sealed reactor, and the water is evaporated under reduced pressure until the water is completely evaporated; after the evaporated powder is poured out, it is mixed with lithium carbonate through air flow crushing, and then mixed, slurried, ground, sprayed and calcined to obtain a primary calcined material; the primary calcined material is added to polyethylene glycol solution, stirred and slurried to obtain a slurry, and then ferrous sulfate solution, phosphoric acid solution and ammonia solution are added to the slurry together, and the reaction material is filtered, washed and dried to obtain an iron-titanium mixture; the iron-titanium mixture is mixed with lithium carbonate and carbon source, slurried, and then ground, sprayed and calcined. The obtained material is subjected to air flow crushing, screening, and iron removal to obtain titanium-doped lithium iron phosphate. Existing titanium-doped iron phosphate is mainly synthesized using iron phosphate, titanium source and other additives, and its structural performance cannot be compared with the heterogeneous isomorphism of natural minerals themselves. Therefore, it is of great advantage to prepare titanium-doped iron phosphate using red mud containing iron and titanium.
[0005] Calcium sulfate whiskers are fibrous single crystals of calcium sulfate synthesized from raw gypsum by a specific process and formula. It has a uniform cross-section, a complete appearance and a highly perfect internal structure. It is a non-metallic material with many special properties. It is applied to polymer materials, which can not only strengthen and toughen, but also play the role of thickening, heat resistance, wear resistance, oil resistance, etc. Patent CN116876070A discloses a method for preparing calcium sulfate whiskers, wherein the citric acid residue is first ground and dissolved, then acidified and magnetized, and then crystal seeds are added, and then stabilized by a hydrothermal reaction, and then stabilized by adding a stabilizer, filtered and rinsed, dried and dehydrated, and calcined to obtain calcium sulfate whiskers. Patent CN202110991996.7 discloses a calcium sulfate whisker and a method for preparing the same, wherein calcium ions are extracted from lactic acid fermentation broth or lactic acid fermentation treatment broth by using a suitable extraction system, and the extract phase is subjected to a regulated sulfuric acid acid hydrolysis process to obtain high-purity and high-quality calcium sulfate whiskers in one step. The existing preparation methods of calcium sulfate whiskers generally have the problems of long process flow, need to add additional seed crystals, and high raw material cost. Summary of the invention
[0006] The purpose of the present invention is to provide a method for the stepwise separation and extraction of valuable elements in red mud. The method uses red mud as a raw material and uses high-concentration sulfuric acid for high-temperature acid leaching, so that iron, aluminum, titanium and sodium elements can be fully leached, and sodium hexametafluoride, titanium-doped ferric phosphate, sodium hydroxide and calcium sulfate whiskers and other products can be recovered and prepared.
[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0008] The red mud valuable elements cascade separation and extraction co-production method comprises the following steps:
[0009] A. After the red mud is dried, ground and sieved, it is stirred and leached with a high-concentration strong acid under high temperature conditions to obtain an acid leaching solution containing iron, aluminum and sodium and a filter residue, which is used as a building material;
[0010] B. Cooling and crystallizing the acid leaching solution, filtering, and obtaining a crystalline product sodium salt and a filtrate a;
[0011] C. Add lime milk to the filtrate a, stir evenly, let stand, and then filter to obtain slurry c. 1 and filtrate b;
[0012] D. Add sodium fluoride to the filtrate b. After the reaction is complete, separate the solid and liquid to obtain sodium hexafluoroaluminate and the filtrate d;
[0013] E. Detect the iron ion content in the filtrate d, add a phosphorus-containing solution to the filtrate d according to the reaction ratio, adjust the pH to 1-2, perform a homogeneous precipitation reaction, filter, take the precipitate and dry it to obtain titanium-doped iron phosphate powder and filtrate e;
[0014] F. Add the sodium salt of the crystal product obtained in step B to the lime milk at a calcium-sulfur ratio of 0.95-1.10 for reaction. After the reaction is completed, filter to obtain slurry c 2 and sodium hydroxide solution;
[0015] G. Slowly add lime milk to the filtrate e at a calcium-sulfur ratio of 0.75-1.0. After the reaction is complete, slurry c is obtained. 3 ;
[0016] H. Make the slurry c 1 、c 2 and c 3 The calcium sulfate whiskers are obtained by mixing, slurry preparation, hydrothermal synthesis, aging, drying and calcination.
[0017] In the step A, the high concentration strong acid is 6-14 mol / L sulfuric acid, and the solid-liquid ratio of the feed is 1:2-1:8.
[0018] In the step A, the high temperature condition is 60-120° C. and the reaction time is 1-4 h.
[0019] In the step B, the temperature of cooling crystallization is -20°C to 15°C.
[0020] In the steps C, F and G, the added lime milk has a calcium hydroxide content of ≥20%, a pH of ≥11 and a solid content of ≤50%.
[0021] In the step D, the reaction conditions are:
[0022] The reaction temperature is 10-70°C, and the reaction time is 10-90min. The amount of sodium fluoride added is 3-9:1 in terms of the molar ratio of F ions to Al ions.
[0023] In the step E, the phosphorus-containing solution is one of phosphoric acid, monoammonium hydrogen phosphate, and diammonium hydrogen phosphate, or a mixture of more than one of them.
[0024] In the step E, the conditions for the homogeneous precipitation reaction are: the molar ratio of iron ions to phosphate ions in the phosphorus-containing solution is 1:0.8-2, the reaction temperature is 50-100° C., and the reaction time is 2-8 hours.
[0025] In the step H, the calcium-sulfur ratio after mixing and slurrying is less than 1.05;
[0026] The hydrothermal synthesis reaction conditions are: temperature 95-120°C, pH 5-8, reaction time 3-4h;
[0027] Aging conditions are: adjusting pH to 5-7, reaction time to 0.5-8h;
[0028] The drying temperature is 110-130℃;
[0029] The calcination temperature is 350-600°C.
[0030] During the hydrothermal synthesis reaction and aging, ammonia water or sodium hydroxide is used for pH adjustment.
[0031] In the step E, the method for detecting the iron ion content in the filtrate d can adopt various methods of the prior art, such as:
[0032] (1) Use a pipette to transfer 2 mL of filtrate b into a 250 mL conical flask, add 5 mL of hydrochloric acid, and heat to near boiling. While hot, add stannous chloride solution dropwise while shaking the conical flask until the color of the solution changes from brown to light yellow.
[0033] (2) Add 4-5 drops of sodium tungstate indicator solution, and add titanium trichloride solution drop by drop while shaking until the solution turns light blue. Immediately cool with running water, add 50ml of water, and titrate with potassium dichromate standard titration solution until the blue color just fades (usually 1-2 drops, do not record the reading). Dilute to 100mL with water, add 10mL of sulfuric acid-phosphoric acid mixed solution, 3-4 drops of sodium diphenylamine sulfonate indicator solution, and titrate with potassium dichromate standard titration solution until a stable purple-red color (does not disappear in 30 seconds) is the end point.
[0034] (3) Calculation of results:
[0035] The iron content is expressed as the mass fraction w of iron (Fe), and the value is expressed in %, calculated according to the formula:
[0036]
[0037] Where:
[0038] V—The volume of potassium dichromate standard titration solution consumed by titrating the leaching solution, in mL
[0039] V 0 —The volume of potassium dichromate standard titration solution consumed in titrating the blank sample, in mL
[0040] V 1 —Total volume of the leachate, in mL
[0041] V 2 —Sampling volume, in mL
[0042] c—The exact value of the concentration of potassium dichromate standard titration solution, in mol / L
[0043] m—Original sample sampling mass, in g
[0044] 19.75%—Fe content of the sample.
[0045] The present invention has the following advantages:
[0046] The method of the invention uses red mud as raw material and uses high-concentration sulfuric acid for high-temperature acid leaching, so that the iron, aluminum, titanium and sodium elements can be fully leached and recycled.
[0047] The present invention first cools and crystallizes the red mud acid leaching solution to obtain a crystal product, sodium sulfate; lime milk is added to the crystallization residual solution to obtain a slurry of calcium sulfate whiskers. 1 ; Sodium fluoride is added to the residual liquid to recover the aluminum element as a high value-added sodium hexametafluoride product; a phosphorus source is added to the filtrate to produce a titanium-doped iron phosphate product. The high-value utilization of iron, aluminum, titanium and sodium elements in red mud is achieved in the entire process steps.
[0048] The slurry of the present invention 1 , sodium sulfate and sulfuric acid produced in the process of preparing titanium-doped ferric phosphate are used to prepare calcium sulfate whiskers without adding seed crystals, which reduces the cost of raw materials and increases the added value of the product. DETAILED DESCRIPTION
[0049] In order to facilitate a better understanding of the present invention, the following examples are used to illustrate the present invention. These examples belong to the protection scope of the present invention, but do not limit the protection scope of the present invention.
[0050] Example 1
[0051] The method for cascade separation and extraction of valuable elements from red mud comprises the following steps:
[0052] A. After the red mud is dried, ground and sieved, it is stirred and leached with 6 mol / L sulfuric acid at 90°C, with a solid-liquid ratio of 1:5 and a reaction time of 1h to obtain an acid leaching solution containing iron, aluminum and sodium and a filter residue, which is used as a building material;
[0053] B. Cooling the acid leaching solution for crystallization at a temperature of -20°C, filtering to obtain a crystalline product sodium salt and a filtrate a;
[0054] C. Add lime milk to the filtrate a, stir evenly, let stand, and then filter to obtain slurry c. 1 and filtrate b;
[0055] D. Add sodium fluoride to the filtrate b. After the reaction is complete, separate the solid and liquid to obtain sodium hexafluoroaluminate and the filtrate d;
[0056] The reaction conditions for adding sodium fluoride are:
[0057] The reaction temperature was 10°C, and the reaction time was 10 min. The amount of sodium fluoride added was 3:1 in terms of the molar ratio of F ions to Al ions.
[0058] E. Detect the iron ion content in the filtrate d, add a phosphorus-containing solution to the filtrate d according to the reaction ratio, adjust the pH to 1, perform a homogeneous precipitation reaction, filter, take the precipitate and dry it to obtain titanium-doped iron phosphate powder and filtrate e;
[0059] The phosphorus-containing solution is one of phosphoric acid, monoammonium hydrogen phosphate, diammonium phosphate, or a mixture of more than one of them;
[0060] The conditions for the homogeneous precipitation reaction were as follows: the molar ratio of iron ions to phosphate ions in the phosphorus-containing solution was 1:0.8, the reaction temperature was 50°C, and the reaction time was 2 h;
[0061] F. Add the sodium salt of the crystal product obtained in step B to the lime milk at a calcium-sulfur ratio of 0.95 for reaction. After the reaction is completed, filter to obtain slurry c 2 and sodium hydroxide solution;
[0062] G. Slowly add lime milk to the filtrate e at a calcium-sulfur ratio of 0.75. After the reaction is complete, slurry c is obtained. 3 ;
[0063] H. Make the slurry c 1 、c 2 and c 3 The calcium sulfate whiskers are obtained by mixing and slurrying, hydrothermal synthesis, aging, drying and calcining;
[0064] The calcium-sulfur ratio after mixing and slurry preparation is 0.97;
[0065] The hydrothermal synthesis reaction conditions were: temperature 95 °C, pH 5, reaction time 3 h;
[0066] Aging conditions are: pH 5, reaction time 0.5h;
[0067] The drying temperature is 110°C;
[0068] The calcination temperature is 350°C.
[0069] During the hydrothermal synthesis reaction and aging, ammonia water or sodium hydroxide is used for pH adjustment.
[0070] In the steps C, F and G, the added lime milk has a calcium hydroxide content of ≥20%, a pH of ≥11 and a solid content of ≤50%.
[0071] Example 2
[0072] The method for cascade separation and extraction of valuable elements from red mud comprises the following steps:
[0073] A. After the red mud is dried, ground and sieved, it is stirred and leached with 14 mol / L sulfuric acid at 120°C, with a solid-liquid ratio of 1:2 and a reaction time of 4 hours. The acid leaching solution and filter residue containing iron and aluminum sodium are obtained, and the filter residue is used as building materials;
[0074] B. Cooling the acid leaching solution for crystallization at a temperature of 15° C., filtering to obtain a crystalline product sodium salt and a filtrate a;
[0075] C. Add lime milk to the filtrate a, stir evenly, let stand, and then filter to obtain slurry c. 1 and filtrate b;
[0076] D. Add sodium fluoride to the filtrate b. After the reaction is complete, separate the solid and liquid to obtain sodium hexafluoroaluminate and the filtrate d;
[0077] The reaction conditions for adding sodium fluoride are:
[0078] The reaction temperature was 70°C and the reaction time was 90 min. The amount of sodium fluoride added was 9:1 in terms of the molar ratio of F ions to Al ions.
[0079] E. Detect the iron ion content in the filtrate d, add a phosphorus-containing solution to the filtrate d according to the reaction ratio, adjust the pH to 2, perform a homogeneous precipitation reaction, filter, take the precipitate and dry it to obtain titanium-doped iron phosphate powder and filtrate e;
[0080] The phosphorus-containing solution is one of phosphoric acid, monoammonium hydrogen phosphate, diammonium phosphate, or a mixture of more than one of them;
[0081] The conditions for the homogeneous precipitation reaction were: the molar ratio of iron ions to phosphate ions in the phosphorus-containing solution was 1:2, the reaction temperature was 100°C, and the reaction time was 8 h;
[0082] F. Add the sodium salt of the crystal product obtained in step B to the lime milk at a calcium-sulfur ratio of 1.10 for reaction. After the reaction is completed, filter to obtain slurry c 2 and sodium hydroxide solution;
[0083] G. Slowly add lime milk to the filtrate e at a calcium-sulfur ratio of 1.0. After the reaction is complete, slurry c is obtained. 3 ;
[0084] H. Make the slurry c 1 、c 2 and c 3 The calcium sulfate whiskers are obtained by mixing and slurrying, hydrothermal synthesis, aging, drying and calcining;
[0085] The calcium-sulfur ratio after mixing and slurry preparation is 0.95;
[0086] The hydrothermal synthesis reaction conditions were: temperature 120 °C, pH 8, reaction time 4 h;
[0087] Aging conditions: pH 7, reaction time 8h;
[0088] The drying temperature is 130°C;
[0089] The calcination temperature is 600°C.
[0090] During the hydrothermal synthesis reaction and aging, ammonia water or sodium hydroxide is used for pH adjustment.
[0091] In the steps C, F and G, the added lime milk has a calcium hydroxide content of ≥20%, a pH of ≥11 and a solid content of ≤50%.
[0092] Example 3
[0093] The method for cascade separation and extraction of valuable elements from red mud comprises the following steps:
[0094] A. After the red mud is dried, ground and sieved, it is stirred and leached with 10 mol / L sulfuric acid at 110°C, with a solid-liquid ratio of 1:3 and a reaction time of 2 hours to obtain an acid leaching solution containing iron, aluminum and sodium and a filter residue, which is used as a building material;
[0095] B. Cooling and crystallizing the acid leaching solution at a temperature of 0°C, filtering to obtain a crystalline product sodium salt and a filtrate a;
[0096] C. Add lime milk to the filtrate a, stir evenly, let stand, and then filter to obtain slurry c. 1 and filtrate b;
[0097] D. Add sodium fluoride to the filtrate b. After the reaction is complete, separate the solid and liquid to obtain sodium hexafluoroaluminate and the filtrate d;
[0098] The reaction conditions for adding sodium fluoride are:
[0099] The reaction temperature was 40°C and the reaction time was 50 min. The amount of sodium fluoride added was 6:1 in terms of the molar ratio of F ions to Al ions.
[0100] E. Detect the iron ion content in the filtrate d, add a phosphorus-containing solution to the filtrate d according to the reaction ratio, adjust the pH to 1.5, perform a homogeneous precipitation reaction, filter, take the precipitate and dry it to obtain titanium-doped iron phosphate powder and filtrate e;
[0101] The phosphorus-containing solution is one of phosphoric acid, monoammonium hydrogen phosphate, diammonium phosphate, or a mixture of more than one of them;
[0102] The conditions for the homogeneous precipitation reaction were: the molar ratio of iron ions to phosphate ions in the phosphorus-containing solution was 1:1, the reaction temperature was 70°C, and the reaction time was 4 h;
[0103] F. Add the sodium salt of the crystal product obtained in step B to the lime milk at a calcium-sulfur ratio of 1.00 for reaction. After the reaction is completed, filter to obtain slurry c 2 and sodium hydroxide solution;
[0104] G. Slowly add lime milk to the filtrate e at a calcium-sulfur ratio of 0.85. After the reaction is complete, slurry c is obtained. 3 ;
[0105] H. Make the slurry c 1 、c 2 and c 3 The calcium sulfate whiskers are obtained by mixing and slurrying, hydrothermal synthesis, aging, drying and calcining;
[0106] The calcium-sulfur ratio after mixing and slurry preparation is 1.00;
[0107] The hydrothermal synthesis reaction conditions were: temperature 110 °C, pH 6, reaction time 3.5 h;
[0108] Aging conditions: pH 6, reaction time 4h;
[0109] The drying temperature is 120°C;
[0110] The calcination temperature is 500°C.
[0111] During the hydrothermal synthesis reaction and aging, ammonia water or sodium hydroxide is used for pH adjustment.
[0112] In the steps C, F and G, the added lime milk has a calcium hydroxide content of ≥20%, a pH of ≥11 and a solid content of ≤50%.
[0113] Example 4
[0114] The method for cascade separation and extraction of valuable elements from red mud comprises the following steps:
[0115] A. After the red mud is dried, ground and sieved, it is stirred and leached with 6 mol / L sulfuric acid at 100°C, with a solid-liquid ratio of 1:5 and a reaction time of 2 hours to obtain an acid leaching solution containing iron, aluminum and sodium and a filter residue, which is used as a building material;
[0116] B. Cooling the acid leaching solution for crystallization at a temperature of -5°C, filtering to obtain a crystalline product sodium salt and a filtrate a;
[0117] C. Add lime milk to the filtrate a, stir evenly, let stand, and then filter to obtain slurry c. 1 and filtrate b;
[0118] D. Add sodium fluoride to the filtrate b. After the reaction is complete, separate the solid and liquid to obtain sodium hexafluoroaluminate and the filtrate d;
[0119] The reaction conditions for adding sodium fluoride are:
[0120] The reaction temperature was 25°C, and the reaction time was 60 min. The amount of sodium fluoride added was 3:1 in terms of the molar ratio of F ions to Al ions.
[0121] E. Detect the iron ion content in the filtrate d, add a phosphorus-containing solution to the filtrate d according to the reaction ratio, adjust the pH to 1, perform a homogeneous precipitation reaction, filter, take the precipitate and dry it to obtain titanium-doped iron phosphate powder and filtrate e;
[0122] The phosphorus-containing solution is one of phosphoric acid, monoammonium hydrogen phosphate, diammonium phosphate, or a mixture of more than one of them;
[0123] The conditions for the homogeneous precipitation reaction were as follows: the molar ratio of iron ions to phosphate ions in the phosphorus-containing solution was 1:0.8, the reaction temperature was 50°C, and the reaction time was 2 h;
[0124] F. Add the sodium salt of the crystal product obtained in step B to the lime milk at a calcium-sulfur ratio of 0.95 for reaction. After the reaction is completed, filter to obtain slurry c 2 and sodium hydroxide solution;
[0125] G. Slowly add lime milk to the filtrate e at a calcium-sulfur ratio of 0.8. After the reaction is complete, slurry c is obtained. 3 ;
[0126] H. Make the slurry c 1 、c 2 and c 3 The calcium sulfate whiskers are obtained by mixing and slurrying, hydrothermal synthesis, aging, drying and calcining;
[0127] The calcium-sulfur ratio after mixing and slurry preparation is 0.9;
[0128] The hydrothermal synthesis reaction conditions were: temperature 100 °C, pH 5, reaction time 3 h;
[0129] Aging conditions are: pH 5, reaction time 2h;
[0130] The drying temperature is 110°C;
[0131] The calcination temperature is 400°C.
[0132] During the hydrothermal synthesis reaction and aging, ammonia water or sodium hydroxide is used for pH adjustment.
[0133] In the steps C, F and G, the added lime milk has a calcium hydroxide content of ≥20%, a pH of ≥11 and a solid content of ≤50%.
[0134] Example 5
[0135] The method for cascade separation and extraction of valuable elements from red mud comprises the following steps:
[0136] A. After the red mud is dried, ground and sieved, it is stirred and leached with 6 mol / L sulfuric acid at 100°C, with a solid-liquid ratio of 1:5 and a reaction time of 2 hours to obtain an acid leaching solution containing iron, aluminum and sodium and a filter residue, which is used as a building material;
[0137] B. Cooling the acid leaching solution for crystallization at a temperature of 5° C. and filtering to obtain a crystalline product sodium salt and a filtrate a;
[0138] C. Add lime milk to the filtrate a, stir evenly, let stand, and then filter to obtain slurry c. 1 and filtrate b;
[0139] D. Add sodium fluoride to the filtrate b. After the reaction is complete, separate the solid and liquid to obtain sodium hexafluoroaluminate and the filtrate d;
[0140] The reaction conditions for adding sodium fluoride are:
[0141] The reaction temperature was 50°C and the reaction time was 60 min. The amount of sodium fluoride added was 6:1 in terms of the molar ratio of F ions to Al ions.
[0142] E. Detect the iron ion content in the filtrate d, add a phosphorus-containing solution to the filtrate d according to the reaction ratio, adjust the pH to 1.5, perform a homogeneous precipitation reaction, filter, take the precipitate and dry it to obtain titanium-doped iron phosphate powder and filtrate e;
[0143] The phosphorus-containing solution is one of phosphoric acid, monoammonium hydrogen phosphate, diammonium phosphate, or a mixture of more than one of them;
[0144] The conditions for the homogeneous precipitation reaction were: the molar ratio of iron ions to phosphate ions in the phosphorus-containing solution was 1:1, the reaction temperature was 70°C, and the reaction time was 4 h;
[0145] F. Add the sodium salt of the crystal product obtained in step B to the lime milk at a calcium-sulfur ratio of 0.95 for reaction. After the reaction is completed, filter to obtain slurry c 2 and sodium hydroxide solution;
[0146] G. Slowly add lime milk to the filtrate e at a calcium-sulfur ratio of 0.8. After the reaction is complete, slurry c is obtained. 3 ;
[0147] H. Make the slurry c 1 、c 2 and c 3 The calcium sulfate whiskers are obtained by mixing and slurrying, hydrothermal synthesis, aging, drying and calcining;
[0148] The calcium-sulfur ratio after mixing and slurry preparation is 0.9;
[0149] The hydrothermal synthesis reaction conditions were: temperature 100 °C, pH 5, reaction time 3 h;
[0150] Aging conditions are: pH 5, reaction time 2h;
[0151] The drying temperature is 120°C;
[0152] The calcination temperature is 450°C.
[0153] During the hydrothermal synthesis reaction and aging, ammonia water or sodium hydroxide is used for pH adjustment.
[0154] In the steps C, F and G, the added lime milk has a calcium hydroxide content of ≥20%, a pH of ≥11 and a solid content of ≤50%.
[0155] Example 6
[0156] The method for cascade separation and extraction of valuable elements from red mud comprises the following steps:
[0157] A. After the red mud is dried, ground and sieved, it is stirred and leached with 6 mol / L sulfuric acid at 100°C, with a solid-liquid ratio of 1:5 and a reaction time of 2 hours to obtain an acid leaching solution containing iron, aluminum and sodium and a filter residue, which is used as a building material;
[0158] B. Cooling and crystallizing the acid leaching solution at a temperature of 0°C, filtering to obtain a crystalline product sodium salt and a filtrate a;
[0159] C. Add lime milk to the filtrate a, stir evenly, let stand, and then filter to obtain slurry c. 1 and filtrate b;
[0160] D. Add sodium fluoride to the filtrate b. After the reaction is complete, separate the solid and liquid to obtain sodium hexafluoroaluminate and the filtrate d;
[0161] The reaction conditions for adding sodium fluoride are:
[0162] The reaction temperature was 50°C and the reaction time was 60 min. The amount of sodium fluoride added was 6:1 in terms of the molar ratio of F ions to Al ions.
[0163] E. Detect the iron ion content in the filtrate d, add a phosphorus-containing solution to the filtrate d according to the reaction ratio, adjust the pH to 1.8, perform a homogeneous precipitation reaction, filter, take the precipitate and dry it to obtain titanium-doped iron phosphate powder and filtrate e;
[0164] The phosphorus-containing solution is one of phosphoric acid, monoammonium hydrogen phosphate, diammonium phosphate, or a mixture of more than one of them;
[0165] The conditions for the homogeneous precipitation reaction were: the molar ratio of iron ions to phosphate ions in the phosphorus-containing solution was 1:1.1, the reaction temperature was 90°C, and the reaction time was 4 h;
[0166] F. Add the sodium salt of the crystal product obtained in step B to the lime milk at a calcium-sulfur ratio of 1.10 for reaction. After the reaction is completed, filter to obtain slurry c 2 and sodium hydroxide solution;
[0167] G. Slowly add lime milk to the filtrate e at a calcium-sulfur ratio of 0.75-1.0. After the reaction is complete, slurry c is obtained. 3 ;
[0168] H. Make the slurry c 1 、c 2 and c 3 The calcium sulfate whiskers are obtained by mixing and slurrying, hydrothermal synthesis, aging, drying and calcining;
[0169] The calcium-sulfur ratio after mixing and slurry preparation is 1.0;
[0170] The hydrothermal synthesis reaction conditions were: temperature 100 °C, pH 5, reaction time 3 h;
[0171] Aging conditions are: pH 5, reaction time 2h;
[0172] The drying temperature is 125°C;
[0173] The calcination temperature is 450°C.
[0174] During the hydrothermal synthesis reaction and aging, ammonia water or sodium hydroxide is used for pH adjustment.
[0175] In the steps C, F and G, the added lime milk has a calcium hydroxide content of ≥20%, a pH of ≥11 and a solid content of ≤50%.
[0176] Comparative Example 1
[0177] The main difference between this comparative example and Example 4 is that the red mud is leached by acid leaching under low temperature conditions.
[0178] This comparative example processing method comprises the following steps:
[0179] (1) After the red mud is dried, ground and sieved, it is stirred and leached with 6 mol / L sulfuric acid at 25°C, with a solid-liquid ratio of 1:5 and a reaction time of 2 h to obtain an acid leaching solution containing iron, aluminum and sodium;
[0180] The iron leaching rate of this embodiment is 32.1%. The results show that only under the condition of high temperature acid leaching, the recovery rate of valuable metal ions is high and is conducive to the subsequent steps.
[0181] Comparative Example 2
[0182] The main difference between this comparative example and Example 5 is that the molar ratio of calcium to sulfur in step H is 0.5.
[0183] At this time, the recovery rate of calcium sulfate whiskers is only 41.8%. In the present invention, the optimal calcium-sulfur molar ratio range of the hydrothermal synthesis of calcium sulfate whiskers is (0.90-1.05):1.
[0184] In the comparative example, when the calcium-sulfur molar ratio becomes low, the yield of calcium sulfate decreases, which indicates that the reaction does not reach the theoretical complete conversion. On the contrary, when the calcium-sulfur molar ratio is higher than the optimal range, that is, when the amount of sulfuric acid added increases, the yield of calcium sulfate also decreases. The main reason is that too much sulfuric acid causes sodium ions in the solution to combine with sulfate ions to form sodium sulfate and precipitate, thereby causing the loss of calcium sulfate yield.
[0185] Table 1 Comparison of experimental data between examples and comparative examples
[0186]
[0187] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for the stepwise separation and extraction of valuable elements from red mud, characterized in that: The following steps are involved: A. After the red mud is dried, ground and sieved, it is stirred and leached with a high-concentration strong acid under high temperature conditions to obtain an acid leaching solution containing iron, aluminum and sodium and a filter residue; B. Cooling and crystallizing the acid leaching solution, filtering, and obtaining a crystalline product sodium salt and a filtrate a; C. Add lime milk to the filtrate a, stir evenly, let stand, and then filter to obtain slurry c1 and filtrate b; D. Add sodium fluoride to the filtrate b. After the reaction is complete, separate the solid and liquid to obtain sodium hexafluoroaluminate and the filtrate d; E. Detect the iron ion content in the filtrate d, add a phosphorus-containing solution to the filtrate d according to the reaction ratio, adjust the pH to 1-2, perform a homogeneous precipitation reaction, filter, take the precipitate and dry it to obtain titanium-doped iron phosphate powder and filtrate e; F. Add the sodium salt of the crystallized product obtained in step B to lime milk at a calcium-sulfur ratio of 0.95-1.10 for reaction. After the reaction is completed, filter to obtain slurry c2 and sodium hydroxide solution; G. Slowly add lime milk to the filtrate e at a calcium-sulfur ratio of 0.75-1.0, and after the reaction is complete, obtain slurry c3; H. Slurries c1, c2 and c3 are mixed, hydrothermally synthesized, aged, dried and calcined to obtain calcium sulfate whiskers.
2. The method for cascade separation and extraction of valuable elements from red mud according to claim 1, characterized in that: In the step A, the high concentration strong acid is 6-14 mol / L sulfuric acid, and the solid-liquid ratio of the feed is 1:2-1:
8.
3. The method for cascade separation and extraction of valuable elements from red mud according to claim 2, characterized in that: In the step A, the high temperature condition is 60-120° C. and the reaction time is 1-4 h.
4. The method for cascade separation and extraction of valuable elements from red mud according to claim 1, characterized in that: In the step B, the temperature of cooling crystallization is -20°C to 15°C.
5. The method for cascade separation and extraction of valuable elements from red mud according to claim 1, characterized in that: In the steps C, F and G, the added lime milk has a calcium hydroxide content of ≥20%, a pH of ≥11 and a solid content of ≤50%.
6. The method for cascade separation and extraction of valuable elements from red mud according to claim 5, characterized in that: In the step D, the reaction conditions are: The reaction temperature is 10-70°C, and the reaction time is 10-90min. The amount of sodium fluoride added is 3-9:1 in terms of the molar ratio of F ions to Al ions.
7. The method for cascade separation and extraction of valuable elements from red mud according to claim 1, characterized in that: In the step E, the phosphorus-containing solution is one of phosphoric acid, monoammonium hydrogen phosphate, and diammonium hydrogen phosphate, or a mixture of more than one of them.
8. The method for cascade separation and extraction of valuable elements from red mud according to claim 7, characterized in that: In the step E, the conditions for the homogeneous precipitation reaction are: the molar ratio of iron ions to phosphate ions in the phosphorus-containing solution is 1:0.8-2, the reaction temperature is 50-100° C., and the reaction time is 2-8 hours.
9. The method for cascade separation and extraction of valuable elements from red mud according to claim 1, characterized in that: In the step H, the calcium-sulfur ratio after mixing and slurrying is less than 1.05; The hydrothermal synthesis reaction conditions are: temperature 95-120°C, pH 5-8, reaction time 3-4h; Aging conditions are: adjusting pH to 5-7, reaction time to 0.5-8h; The drying temperature is 110-130℃; The calcination temperature is 350-600°C.
10. The method for cascade separation and extraction of valuable elements from red mud according to claim 9, characterized in that: During the hydrothermal synthesis reaction and aging, ammonia water or sodium hydroxide is used for pH adjustment.