Preparation method of high-performance iron oxide for soft magnetic ferrite
Through the mixing and multi-stage leaching separation technology of industrial hydrochloric acid and raw ore powder, combined with atomization and baking method, the problems of purity and environmental pollution in iron oxide preparation are solved, and efficient and environmentally friendly iron oxide preparation is achieved, and soft magnetic materials are improved. The supply capacity of the industry.
Patent Information
- Application Number
- CN202411176424.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing iron oxide preparation technology has problems such as low purity, high cost, and environmental pollution, which affects the development of my country's soft magnetic material industry.
Using industrial hydrochloric acid and raw ore powder to mix, single-stage or two-stage leaching and solid-liquid separation device are used to obtain a high-purity ferric chloride solution, and flash baked by atomizer to form high-purity iron oxide, and at the same time recovered and reuse hydrochloric acid to achieve zero discharge of wastewater and reuse of solid waste.
It improves the preparation efficiency and purity of iron oxide, realizes zero wastewater discharge and reuse of solid waste, avoids environmental pollution, and reduces resource waste.
Smart Images

Figure CN118908289A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of iron oxide preparation, and in particular relates to a method for preparing high-performance iron oxide for soft ferrite. Background Art
[0002] Magnetite (Fe3O4) is the earliest iron-based magnetic material discovered. People have used the physical properties of magnetite to develop permanent magnetic materials and mechanical equipment such as generators and motors, which has promoted the continuous progress of human science and technology. Later, the physical properties of iron oxide (Fe2O3) that it exhibits weak magnetism in its normal state were used to develop ferrite soft magnetic materials. Since the emergence of soft ferrite composite materials in the 1950s, a special iron oxide (Fe2O3) preparation technology has been developed, which has matured after several iterations. The purity, fineness, specific surface area and other properties of iron oxide have been continuously improved, and the performance of magnetic powder and devices has also been improved accordingly. The technical equipment level of the magnetic material industry has made great progress.
[0003] At present, the production capacity of iron oxide raw materials for soft magnetic ferrites in my country mainly comes from steel enterprises. This is mainly because iron plants rely on the "Rusner method" acid regeneration technology to achieve hydrochloric acid recycling to avoid environmental protection policy supervision on the discharge of cold rolling pickling liquid. The by-products produced are limited by the difficulty and high cost of purification, and the blast furnace gas used in the roasting furnace has many impurities. Therefore, the purity of the iron oxide produced is not high and the quality is unstable. High-performance iron oxide red (purity ≥ 99.5%) still needs to be imported from abroad. Special varieties are expensive and limited in sale, which seriously affects the stability of the supply market of medium and high-end magnetic materials in my country. It has become a prominent shortcoming that restricts the quality upgrade of my country's soft magnetic materials industry. Summary of the invention
[0004] The present invention provides a method for preparing high-performance iron oxide for soft ferrite, which is used to improve the preparation efficiency and purity of iron oxide, achieve zero wastewater discharge, and convert all solid waste into silicon micropowder for reuse, thereby avoiding environmental pollution.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows: A method for preparing high-performance iron oxide for soft ferrite comprises the following steps: Step 1. Add the raw ore powder into the stirring tank, then add industrial hydrochloric acid from the hydrochloric acid tank into the stirring tank, and perform stirring operation; Step 2. Pumping the uniformly stirred mixture into a multi-stage leaching and separation device, and controlling the multi-stage leaching and separation device to filter the silicon powder in the mixture; Step 3. The ferric chloride solution obtained by filtration is supplied to an atomizer, which atomizes the ferric chloride solution and supplies the solution to a roaster; Step 4. flash roasting the atomized ferric chloride solution in a roaster to obtain high-purity iron oxide; Step 5. The gas obtained by flash roasting enters the absorption tower, and the purified gas is discharged to the outside. The purified liquid passes through a condenser to obtain regenerated acid, and then enters the hydrochloric acid kettle and / or a multi-stage leaching separation device.
[0006] Furthermore, in step 2, industrial hydrochloric acid is added from a hydrochloric acid kettle into the multi-stage leaching and separation device according to a predetermined amount.
[0007] Furthermore, in step 2, the silicon micropowder obtained by filtration is sold or mixed with ore, or the silicon micropowder is processed to obtain white carbon black.
[0008] Furthermore, the multi-stage leaching separation device includes a separation cabinet with a plurality of primary separation filter discs arranged side by side. The axes of these primary separation filter discs overlap and are connected in sequence to form a guide channel between these primary separation filter discs. Each of the primary separation filter discs has a filter cavity connected to the guide channel, and one of these primary separation filter discs is driven to drive the other primary separation filter discs to rotate synchronously.
[0009] Furthermore, the separation cabinet includes a cabinet body divided into a first chamber and a second chamber by a partition plate, one circumferential side of each primary separation filter disc is located in the first chamber, and the other circumferential side of the primary separation filter disc is located in the second chamber, a notch is opened at the upper part of the partition plate and at the upper end of each primary separation filter disc, and a discharge port is opened at the lower end of the second chamber and at each primary separation filter disc, and a mixture of raw ore powder and industrial hydrochloric acid enters the first chamber through a liquid inlet pipe system, and the liquid level of the mixture is lower than the lowest end of the notch.
[0010] Furthermore, the primary separation filter disc includes a disc-shaped ceramic filter plate rotatably mounted on both sides of the mounting ring, and an inner base tube is detachably connected to the inner edge of each disc-shaped ceramic filter plate, the inner base tubes of two adjacent primary separation filter discs close to each other are connected to each other, and the guide channel is formed between the inner base tubes connected to each other, and the filter chamber is formed in the space enclosed by the mounting ring and the two disc-shaped ceramic filter plates.
[0011] Furthermore, a connecting spring is sleeved on the outside of each of the inner base tubes, and both ends of the connecting tube are movably sleeved on the outside of the inner base tubes of two adjacent primary separation filter plates close to each other, and the two ends of the connecting tube are respectively connected to the corresponding connecting springs; a guide bar is constructed on the outer wall of each inner base tube, and each guide bar extends along the axial direction of the inner base tube, and a guide groove is opened on the inner wall of the connecting tube, and the guide groove extends along the axial direction of the connecting tube, and the guide bar is movably assembled in the guide groove.
[0012] Furthermore, the assembly ring is fixedly installed with the separation cabinet, and the assembly ring is connected with the acid liquid replenishment piping system; the acid liquid replenishment piping system includes an acid replenishment main pipe connected with multiple first acid replenishment branch pipes and multiple second acid replenishment branch pipes, each of the first acid replenishment branch pipes is connected with a corresponding portion of the first chamber, each of the second acid replenishment branch pipes is connected with an acid replenishment joint on the corresponding assembly ring, a first acid replenishment valve and a second acid replenishment valve are respectively installed on each of the first acid replenishment branch pipes and each of the second acid replenishment branch pipes, and multiple spiral guide blades are constructed in each inner base pipe, and these spiral guide blades are evenly arranged along the circumference of the inner base pipe.
[0013] Furthermore, a secondary membrane filtration mechanism is installed at one end of the outer side of the separation cabinet, and a guide pipe is connected to the outlet end of the secondary membrane filtration mechanism. The guide pipe passes through one end of the guide channel through each primary separation filter plate and out of the other end of the guide channel, and the outlet end of the guide pipe is connected to the separation cabinet through a fixed seat.
[0014] Further, the secondary membrane filtration mechanism includes a filter cartridge connected to one end of the guide channel through an adapter cartridge, a filter membrane tube is coaxially arranged in the filter cartridge, an end cap is detachably mounted on the end of the filter cartridge away from the adapter cartridge, a plurality of extrusion ports are provided on the end cap, a spiral guide blade extending along its axis is constructed on the inner wall of the filter cartridge, an end face of the spiral guide blade away from the filter cartridge is close to or in contact with the outer peripheral surface of the filter membrane tube, a plurality of conducting holes are provided on the portion of the spiral guide blade close to the adapter cartridge, a connecting seat is constructed at the end of the filter membrane tube, and the connecting seat is rotatably connected to the end cap; a plurality of drainage ports are evenly arranged on the adapter cartridge along its circumference, a transfer sleeve is rotatably connected to the outside of the adapter cartridge, the transfer sleeve is detachably connected to the separation cabinet, a drainage joint is constructed on the transfer sleeve, and a drainage valve is installed on the drainage joint.
[0015] Due to the adoption of the above structure, the technical progress achieved by the present invention compared with the prior art is that: the present invention mixes industrial hydrochloric acid and raw ore powder, and then performs single-stage or two-stage leaching in a multi-stage leaching and separation device. Generally, two-stage leaching is performed according to the purity requirement, and solid-liquid separation is performed, and impurities such as silicon micropowder in the solution are fully separated by a two-stage separation method to obtain a ferric chloride solution; then, the ferric chloride solution is atomized by an atomizer, so that the atomized ferric chloride solution is flash-roasted in a roaster, and the ferric chloride is pyrolyzed to form ferric oxide, and the obtained hydrochloric acid is collected and utilized again, and the obtained hydrochloric acid is collected in a hydrochloric acid kettle or directly supplied to the multi-stage leaching and separation device; the separated silicon micropowder can be recovered for other uses. In summary, the present invention fully removes impurities in ferric chloride by means of two-stage leaching and two-stage separation, obtains a highly pure ferric chloride solution, and then rapidly pyrolyzes the atomized ferric chloride solution by flash roasting to form high-purity iron oxide, thereby improving the efficiency of preparation, and reusing the hydrochloric acid obtained by pyrolysis to improve the utilization rate and avoid the waste of resources. Therefore, the present invention can effectively improve the preparation efficiency and purity of iron oxide, can achieve zero discharge of wastewater, and the purpose of reusing solid waste after all being converted into silicon micropowder, thereby avoiding the occurrence of environmental pollution. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention.
[0017] In the attached picture: Figure 1 is a process flow chart of an embodiment of the present invention; Figure 2 is a process structure block diagram of an embodiment of the present invention; Figure 3 It is a schematic structural diagram of a multi-stage leaching and separation device according to an embodiment of the present invention; Figure 4 It is a structural schematic diagram of the multi-stage leaching and separation device from another angle according to an embodiment of the present invention; Figure 5 It is a structural cross-sectional view of a multi-stage leaching and separation device according to an embodiment of the present invention; Figure 6 for Figure 5 A magnified view of the structure of the middle A part; Figure 7 It is a schematic diagram of the partial structure of a multi-stage leaching and separation device according to an embodiment of the present invention; Figure 8 A schematic diagram of the structure of a primary separation filter disc in a multi-stage leaching and separation device according to an embodiment of the present invention; Fig. 9It is a structural exploded diagram of a primary separation filter disc in a multi-stage leaching separation device according to an embodiment of the present invention; Fig.10 It is an axial structural cross-sectional view of a primary separation filter disc in a multi-stage leaching separation device according to an embodiment of the present invention; Fig.11 It is a structural exploded diagram of another primary separation filter disc in the multi-stage leaching separation device according to an embodiment of the present invention; Fig.12 This is a structural schematic diagram of the connection between the secondary membrane filtration mechanism and the flow guide pipe according to an embodiment of the present invention; Fig.13 An exploded view of the structure of the connection between the secondary membrane filtration mechanism and the flow guide pipe according to an embodiment of the present invention; Fig.14 It is a partial structural cross-sectional view of the connection between the filter cartridge and the end cover in the secondary membrane filtration mechanism of an embodiment of the present invention.
[0018] Labeled parts: 100-cabinet, 101-partition plate, 102-first chamber, 103-second chamber, 104-discharge port, 105-fixed seat, 106-notch, 200-multi-stage leaching separation device, 201-primary separation filter disc, 2011-assembly ring, 2012-adapter groove, 2013-disc-shaped ceramic filter plate, 2014-inner base tube, 2015-first connecting edge, 2016-spiral guide blade, 2017-guide strip, 2018-second connecting edge, 202-filtration chamber, 203-acid supplement joint, 204-guiding channel, 205-connecting spring, 206-connecting pipe, 207-guide groove, 300-secondary membrane filtration mechanism, 301-guiding pipe, 302-filter cartridge, 303-transmission wheel, 304-liquid outlet channel, 305-filter membrane tube, 306-connecting seat, 307-end cover, 308-extrusion port, 309-extrusion cavity, 310-spiral guide blade, 311-conducting hole, 312-transition tube, 313-adapter tube, 314-drainage port, 315-guide strip, 400-adapter mechanism, 401-adapter sleeve, 402-drainage cavity, 403-drainage joint, 404-drainage valve, 500-liquid inlet pipe system, 501-liquid inlet main pipe, 502-liquid inlet branch pipe, 503-liquid inlet valve, 600-acid replenishment pipe system, 601-acid replenishment main pipe, 602-first acid replenishment branch pipe, 603-second acid replenishment branch pipe, 604-first acid replenishment valve, 605-second acid replenishment valve. DETAILED DESCRIPTION
[0019] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0020] The present invention discloses a method for preparing high-performance iron oxide for soft ferrite. Figure 1 ,2 As shown, the following steps are included: Step 1. Add the raw ore powder into the stirring tank, then add industrial hydrochloric acid from the hydrochloric acid tank into the stirring tank, and perform stirring operation; Step 2. Pumping the uniformly stirred mixture into the multi-stage leaching and separation device 200, and controlling the multi-stage leaching and separation device 200 to filter the silicon powder in the mixture; Step 3. The ferric chloride solution obtained by filtration is supplied to an atomizer, which atomizes the ferric chloride solution and supplies the solution to a roaster; Step 4. flash roasting the atomized ferric chloride solution in a roaster to obtain high-purity iron oxide; Step 5. The gas obtained by flash roasting enters the absorption tower, and the purified gas is discharged to the outside. The purified liquid passes through the condenser to obtain regenerated acid, and then enters the hydrochloric acid kettle and / or the multi-stage leaching separation device 200.
[0021] The working principle and advantages of the present invention are: the present invention mixes industrial hydrochloric acid and raw ore powder, and then performs single-stage or two-stage leaching in a multi-stage leaching and separation device 200. Generally, two-stage leaching is performed according to the purity requirements, and solid-liquid separation is performed, and impurities such as silicon micropowder in the solution are fully separated by a secondary separation method to obtain a ferric chloride solution; then, the ferric chloride solution is atomized by an atomizer, so that the atomized ferric chloride solution is flash-roasted in a roaster, and the ferric chloride is pyrolyzed to form ferric oxide, and the obtained hydrochloric acid is collected and reused again, and the obtained hydrochloric acid is collected in a hydrochloric acid kettle or directly supplied to a multi-stage leaching and separation device 200; the separated silicon micropowder can be recycled for other uses. In summary, the present invention fully removes impurities in ferric chloride by means of two-stage leaching and two-stage separation, obtains a ferric chloride solution with extremely high purity, and then quickly pyrolyzes the atomized ferric chloride solution by flash roasting to form high-purity ferric oxide, thereby improving the efficiency of preparation, and reusing the hydrochloric acid obtained by pyrolysis, improving the utilization rate, and avoiding the occurrence of resource waste. Therefore, the present invention can effectively improve the preparation efficiency and purity of iron oxide, achieve zero wastewater discharge, and convert all solid waste into silicon micropowder for reuse, thereby avoiding environmental pollution.
[0022] As a preferred embodiment of the present invention, in step 2, industrial hydrochloric acid is added from the hydrochloric acid kettle into the multi-stage leaching and separation device 200 according to a predetermined amount. In this way, industrial hydrochloric acid is added into the multi-stage leaching and separation device 200 to perform the first and / or second stage acid supplementation on the mixture formed by mixing industrial hydrochloric acid and raw ore powder, thereby promoting a full and thorough reaction, thereby improving the yield of ferric chloride preparation, and avoiding the presence of iron ions in the separated solid waste (microsilica powder).
[0023] As a preferred embodiment of the present invention, in step 2, the filtered silicon powder is sold or mixed with ore. The silicon powder can also be solid-liquid converted, that is, the silicon powder is used as a raw material to react to obtain silicon tetrachloride, and then the silicon tetrachloride is reacted in the gas phase to obtain white carbon black.
[0024] As a preferred embodiment of the present invention, Figure 3-5As shown, the multi-stage leaching separation device 200 includes a separation cabinet and a plurality of primary separation filter discs 201. Among them, these primary separation filter discs 201 are arranged side by side in the separation cabinet, and the axes of these primary separation filter discs 201 overlap and are connected together in sequence. In this embodiment, a guide channel 204 is formed between these primary separation filter discs 201, each primary separation filter disc 201 has a filter cavity 202, and each filter cavity 202 is connected to the guide channel 204, and one of the primary separation filter discs 201 is driven to rotate, thereby driving the other primary separation filter discs 201 to rotate synchronously. The separation cabinet of this embodiment includes a cabinet body 100, and a partition plate 101 is arranged in the middle of the cabinet body 100, and the partition plate 101 divides the inner cavity of the cabinet body 100 into a first chamber 102 and a second chamber 103. One circumferential side of each primary separation filter disc 201 is located in the first chamber 102, and the other circumferential side of the primary separation filter disc 201 is located in the second chamber 103. When the primary separation filter disc 201 is driven to rotate, the part of the primary separation filter disc 201 located in the first chamber 102 and the second chamber 103 rotates back and forth, that is, the part of the primary separation filter disc 201 located in the first chamber 102 rotates and gradually enters the second chamber 103, and at the same time, the part located in the second chamber 103 gradually enters the first chamber 102. In this embodiment, a notch 106 is opened at the upper part of the partition plate 101 and at the upper end of each primary separation filter disc 201, and a discharge port 104 is opened at the lower end of the second chamber 103 and at each primary separation filter disc 201. The mixture of raw ore powder and industrial hydrochloric acid enters the first chamber 102 through the liquid inlet pipe system 500, and the liquid level of the mixture is lower than the lower end of the notch 106.The working principle and advantages of this embodiment are as follows: this embodiment continuously supplies the mixed material to the first chamber 102 through the liquid inlet pipe system 500, and generates negative pressure in the guide channel 204 by sucking the guide channel 204. In this way, the filter chamber 202 of each primary separation filter disc 201 also generates negative pressure, so that the primary separation filter disc 201 located below the liquid surface of the first chamber 102 sucks the mixed material, so that the ferric chloride solution passes through each primary separation filter disc 201 and enters each filter chamber 202, and then converges from these filter chambers 202 into the guide channel 204, and is finally extracted, and the impurities in the mixed material are filtered to the axial outer end surface of the primary separation filter disc 201. As the primary separation filter disc 201 The part of the primary separation filter disc 201 that adsorbs impurities enters the second chamber 103 through the notch 106. After that, the part rotates in the second chamber 103 until it rotates to the position where the second chamber 103 and the first chamber 102 are connected to each other. The part of the partition plate 101 at this position plays the role of isolating the first chamber 102 and the second chamber 103 on the one hand, and plays the role of scraping the outer wall of the two axial end faces of the primary separation filter disc 201 on the other hand, that is, as the primary separation filter disc 201 rotates, the lower part of the partition plate 101 scrapes off the impurities adsorbed on the axial end face of the primary separation filter disc 201, and these impurities fall into the bottom of the second chamber 103 and are discharged through the corresponding discharge port 104. Since the liquid level of the mixed material in this embodiment is lower than the lowest end of the notch 106, the mixed material in the first chamber 102 is prevented from entering the second chamber 103 through the notch 106. Moreover, since the primary separation filter disc 201 of this embodiment is in a state of continuous rotation, the ferric chloride solution is continuously extracted, impurities are filtered out and continuously scraped off, thereby making the entire process continuous and improving production efficiency. The specific structure of the liquid inlet pipe system 500 of this embodiment is that the liquid inlet pipe system 500 includes a liquid inlet main pipe 501, which is connected to the outlet end of the stirring tank, and a plurality of liquid inlet branch pipes 502 are connected side by side to the liquid inlet main pipe 501, and these liquid inlet branch pipes 502 are respectively connected to the positions corresponding to the first chamber 102, and a liquid inlet valve 503 is installed on each liquid inlet branch pipe 502. Since the present embodiment adopts multiple liquid inlet branches 502, the mixed material can enter various parts of the first chamber 102 evenly, thereby ensuring that each primary separation filter disc 201 has the same filtering capacity, avoiding changes in the filtering capacity of individual primary separation filter discs 201 and affecting the suction of the mixed material by other primary separation filter discs 201; and if the filtering capacities of these primary separation filter discs 201 are consistent, the filtering effect and filtering efficiency are optimal.
[0025] As a preferred embodiment of the present invention, Figure 5 , 8As shown in Figure 11, the primary separation filter disc 201 includes an assembly ring 2011, two disc-shaped ceramic filter plates 2013 and two inner base tubes 2014. Among them, the inner edges of the two axial ends of the assembly ring 2011 are respectively configured with transfer grooves 2012, and the outer edge of each disc-shaped ceramic filter plate 2013 is rotationally assembled in the transfer groove 2012, so that the disc-shaped ceramic filter plate 2013 is rotationally connected with the assembly ring 2011, and the two inner base tubes 2014 are symmetrically arranged at the center of the assembly ring 2011, and the axes of the assembly ring 2011, the disc-shaped ceramic filter plate 2013 and the inner base tubes 2014 coincide. A first connecting edge 2015 is configured at one end of the two inner base tubes 2014 that are close to each other, and the inner edge of the disc-shaped ceramic filter plate 2013 is detachably connected with the first connecting edge 2015 of the corresponding inner base tube 2014. In this embodiment, the inner base tubes 2014 of two adjacent primary separation filter discs 201 close to each other are connected to each other, and the guide channel 204 is formed between the inner base tubes 2014 connected to each other, and the filter chamber 202 is formed in the space surrounded by the assembly ring 2011 and the two disc-shaped ceramic filter plates 2013. In this embodiment, the inner base tubes 2014 of two adjacent primary separation filter discs 201 close to each other are connected to each other in two ways. The first way is that the inner base tube 2014 is configured with a second connecting edge 2018 at one end away from the first connecting edge 2015, and the two second connecting edges 2018 in the two corresponding inner base tubes 2014 in the two adjacent primary separation filter discs 201 can be detachably connected together, thereby realizing the connection of the adjacent primary separation filter discs 201 and the continuous conduction of the guide channel 204. The second type is that a connecting spring 205 is sleeved on the outside of each inner base tube 2014, and a connecting tube 206 is arranged between two adjacent primary separation filter discs 201, and both ends of the connecting tube 206 are movably sleeved on the outside of the inner base tube 2014 of the two adjacent primary separation filter discs 201 close to each other, and the two ends of the connecting tube 206 are respectively connected to the corresponding connecting springs 205; in this embodiment, a guide strip 2017 is constructed on the outer wall of each inner base tube 2014, and the guide strip 2017 extends along the axial direction of the inner base tube 2014, and a guide groove 207 is opened on the inner wall of the connecting tube 206, and the guide groove 207 extends along the axial direction of the connecting tube 206, and the guide strip 2017 is movably assembled in the guide groove 207. The separation cabinet of this embodiment includes a plurality of sub-cabinets 100, which are independent entities and can be increased or decreased according to needs. The sub-cabinets 100 are arranged side by side, and each sub-cabinet 100 has a first sub-chamber and a second sub-chamber. The first sub-chambers of the sub-cabinets 100 constitute a first chamber 102, and the second sub-chambers of the sub-cabinets 100 constitute a second chamber 103. The above-mentioned multiple liquid inlet branch pipes 502 are connected one by one with the multiple first sub-chambers.The ends of the two inner base tubes 2014 of each primary separation filter disc 201 that are away from each other extend out of the two opposite sides of the sub-cabinet 100, and the two inner base tubes 2014 that are close to each other on the adjacent sub-cabinets 100 are connected through the connecting pipe 206. It can be seen that the present embodiment can adjust the distance between the sub-cabinets 100, that is, adjust the depth of the inner base tube 2014 extending into the connecting pipe 206, so as to achieve the installation of a predetermined number of sub-cabinets 100 in a limited space, thereby ensuring the efficiency of leaching and separation. Moreover, when a single sub-cabinet 100 or a single primary separation filter disc 201 is damaged, the working efficiency is reduced, and other problems, the single sub-cabinet 100 or a single primary separation filter disc 201 can be stopped, and then repaired or replaced to avoid affecting the efficiency of the entire leaching and separation. Since the primary separation filter disc 201 is assembled in the present embodiment, it is convenient for later maintenance, care, replacement, transportation, etc. In this embodiment, an assembly pipe is constructed on the inner base pipe 2014 on the primary separation filter disc 201 located at one side of the separation cabinet. The assembly pipe coincides with the axis of the primary separation filter disc 201, and the assembly pipe extends out of the separation cabinet, and the assembly pipe is rotatably connected to the separation cabinet, and the inner cavity of the assembly pipe is connected to the guide channel 204. In this embodiment, a transmission wheel 303 is installed at the position where the assembly pipe is located outside the separation cabinet. The transmission wheel 303 is generally a driven sprocket, which is connected to the driving sprocket through a chain. The driving sprocket is assembled on the output shaft of the driving motor. In this way, the driving motor drives the driving sprocket to rotate, so that it drives the driven sprocket to rotate through the chain, and the driven sprocket drives each primary separation filter disc 201 to rotate synchronously through the assembly pipe, so as to achieve the purpose of continuous filtering and scraping.
[0026] As a preferred embodiment of the present invention, Figure 4 , 7As shown in Figure 10, the assembly ring 2011 is fixedly connected to the cabinet body 100 or the partition plate 101 of the separation cabinet, and the assembly ring 2011 is connected to the acid liquid supplement pipe system 600. Specifically, the acid liquid supplement pipe system 600 includes an acid supplement main pipe 601, a plurality of first acid supplement branch pipes 602 and a plurality of second acid supplement branch pipes 603. Among them, these first acid supplement branch pipes 602 and second acid supplement branch pipes 603 are all connected to the acid supplement main pipe 601, each first acid supplement branch pipe 602 is connected to the corresponding part of the first chamber 102, and each second acid supplement branch pipe 603 is connected to the corresponding acid supplement connector 203 on the assembly ring 2011, and the acid supplement connector 203 is connected to the filter chamber 202 through the assembly ring 2011. A first acid supplementation valve 604 and a second acid supplementation valve 605 are installed on each first acid supplementation branch pipe 602 and each second acid supplementation branch pipe 603, respectively. A plurality of spiral guide vanes 2016 are constructed in each inner base pipe 2014, and these spiral guide vanes 2016 are evenly arranged along the circumference of the inner base pipe 2014. Industrial hydrochloric acid is added into the first chamber 102 through the first acid supplementation branch pipe 602 of this embodiment, and the first-level acid supplementation is performed for the mixed material in the first chamber 102, so that most of the iron ions in the mixed material are dissolved in the solution. In this embodiment, the second acid supplementation branch pipe 603 is used to supplement acid solution for each filter chamber 202, so that the ferric chloride solution obtained by filtration is rich in acid, thereby ensuring that the undissolved iron ions in the ferric chloride solution react with the acid solution, and ensuring that the iron ions react fully. Furthermore, since a plurality of spiral guide blades 2016 are constructed in each inner base tube 2014, when the mixed liquid passes through the inner base tube 2014 and moves in the guide channel 204, the mixed liquid generates a swirl flow, thereby promoting full mixing of different components in the mixed liquid.
[0027] As a preferred embodiment of the present invention, in order to filter the impurities in the ferric chloride solution filtered out by the primary separation filter disc 201 again, improve the purity of the ferric chloride solution, and reduce the content of impurities therein, the measures taken are as follows: Figure 5 , 6As shown in Figures 12, 13, and 14, a secondary membrane filtration mechanism 300 is installed at one end of the outer side of the separation cabinet, and the outlet end of the secondary membrane filtration mechanism 300 is connected to a guide tube 301. The guide tube 301 passes through one end of the guide channel 204 through each primary separation filter disc 201 and out of the other end of the guide channel 204, and the outlet end of the guide tube 301 is connected to the separation cabinet through a fixed seat 105. The guide tube 301 has a liquid outlet channel 304, which is located in the guide channel 204, and the liquid outlet channel 304 is connected to the guide channel 204 through the secondary membrane filtration mechanism 300. The working principle and advantages of this embodiment are: this embodiment generates negative pressure in the liquid outlet channel 304 by sucking the flow guide tube 301, so that the ferric chloride solution in the first chamber 102 passes through the filter chamber 202, the flow guide channel 204, the secondary membrane filtration mechanism 300 and the liquid outlet channel 304 in sequence, and is finally supplied to the atomizer. It can be seen that the mixed material is subjected to primary filtration at the primary separation filter disc 201, the ferric chloride solution is extracted, and most of the impurities are filtered out. The ferric chloride solution is subjected to secondary filtration in the secondary membrane filtration mechanism 300, and the impurities in the ferric chloride are completely removed to obtain a high-purity ferric chloride solution, so as to facilitate the subsequent preparation of high-purity iron oxide.
[0028] As a preferred embodiment of the present invention, Figure 6 , 12-14, the secondary membrane filtration mechanism 300 includes a filter cartridge 302, a filter membrane tube 305, an end cap 307, a transfer cartridge 313, a connecting seat 306, a transition cartridge 312 and a transfer mechanism 400. The transfer cartridge 313, the transition cartridge 312 and the filter cartridge 302 are sequentially arranged outwardly along the axis of the flow guide tube 301, and the three are an integrally formed structure. The end of the transfer cartridge 313 away from the transition cartridge 312 is connected to the corresponding end of the flow guide channel 204, and a plurality of guide strips 315 are constructed on the inner wall of the transfer cartridge 313. The filter membrane tube 305 is arranged in the filter cartridge 302, and the axes of the two coincide. An extrusion cavity 309 is formed between the filter membrane tube 305 and the filter cartridge 302. The end cap 307 is detachably mounted on the end of the filter cartridge 302 away from the transfer cartridge 313, and a plurality of extrusion ports 308 are provided on the end cap 307. In this embodiment, a spiral material guide blade 310 is constructed on the inner wall of the filter cartridge 302. The spiral material guide blade 310 spirally extends along the axis of the filter cartridge 302, and the end surface of the spiral material guide blade 310 away from the filter cartridge 302 is close to or in contact with the outer peripheral surface of the filter membrane tube 305. A plurality of conducting holes 311 are opened at the part of the spiral material guide blade 310 close to the adapter tube 313. The connecting seat 306 of this embodiment is constructed at the end of the filter membrane tube 305 away from the guide tube 301, and the connecting seat 306 is rotatably connected to the center of the end cover 307. The adapter mechanism 400 of this embodiment includes an adapter sleeve 401 and a drainage joint 403, wherein the adapter sleeve 401 is rotatably assembled outside the adapter tube 313, a drainage cavity 402 is formed between the adapter sleeve 401 and the adapter tube 313, one axial end of the adapter sleeve 401 is detachably connected to the separation cabinet, and a plurality of drainage ports 314 are evenly provided on the adapter tube 313 along its circumference, and these drainage ports 314 connect the drainage cavity 402 with the guide channel 204. The drainage joint 403 of this embodiment is constructed on the adapter sleeve 401 and connected to the drainage cavity 402, and a drainage valve 404 is installed on the drainage joint 403. The working principle and advantages of this embodiment are: this embodiment can achieve primary filtration, that is, only complete the filtration of the primary separation filter disc 201. Specifically, the guide tube 301 is closed, and the drainage joint 403 is sucked to generate negative pressure in the drainage chamber 402. In this way, the ferric chloride solution enters the filter chamber 202 through the guide channel 204 and then enters the drainage chamber 402, and then is discharged from the drainage joint 403. This embodiment can also achieve secondary filtration, that is, close the drainage valve 404, suck the guide tube 301, and the ferric chloride solution passes through the filter chamber 202, the guide channel 204, the extrusion chamber 309, the filter membrane tube 305 and the liquid outlet channel 304 in sequence, and finally obtains a high-purity ferric chloride solution. As for the impurities filtered by the filter membrane tube 305, under the action of the rotating filter cylinder 302, the spiral guide blade 310 drives the impurities attached to the filter membrane tube 305 outward until the impurities are discharged from the extrusion port 308 on the end cover 307.In this embodiment, since a plurality of guide holes 311 are provided at the front section of the spiral guide blade 310, it is ensured that the ferric chloride solution quickly enters the extrusion cavity 309 from the guide channel 204, and the filtration membrane tube 305 is prevented from being sucked empty. It can be seen that in this embodiment, whether to perform secondary filtration on the ferric chloride solution can be selected according to the purity of the ferric chloride solution after primary filtration, so as to provide favorable support in the early stage for obtaining high-purity iron oxide later.
[0029] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein with equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the scope of protection of the claims of the present invention.
Claims
1. A method for preparing high-performance iron oxide for soft ferrite, characterized in that: The steps include: Step 1. Add the raw ore powder into the stirring tank, then add industrial hydrochloric acid from the hydrochloric acid tank into the stirring tank, and perform stirring operation; Step 2. Pumping the uniformly stirred mixture into a multi-stage leaching and separation device, and controlling the multi-stage leaching and separation device to filter the silicon powder in the mixture; Step 3. The ferric chloride solution obtained by filtration is supplied to an atomizer, which atomizes the ferric chloride solution and supplies the solution to a roaster; Step 4. flash roasting the atomized ferric chloride solution in a roaster to obtain high-purity iron oxide; Step 5. The gas obtained by flash roasting enters the absorption tower, and the purified gas is discharged to the outside. The purified liquid passes through a condenser to obtain regenerated acid, and then enters the hydrochloric acid kettle and / or a multi-stage leaching separation device.
2. The method for preparing high-performance iron oxide for soft ferrite according to claim 1, characterized in that: In step 2, industrial hydrochloric acid is added from a hydrochloric acid kettle into a multi-stage leaching and separation device according to a predetermined amount.
3. The method for preparing a high-performance iron oxide for soft ferrite according to claim 1, characterized in that: In step 2, the silica powder obtained by filtration is sold or mixed with ore, or the silica powder is processed to obtain white carbon black.
4. The method for preparing high-performance iron oxide for soft ferrite according to claim 1, characterized in that: The multi-stage leaching separation device includes a separation cabinet with a plurality of primary separation filter discs arranged side by side. The axes of the primary separation filter discs overlap and are connected in sequence to form a guide channel between the primary separation filter discs. Each of the primary separation filter discs has a filter cavity connected to the guide channel, and one of the primary separation filter discs is driven to drive the other primary separation filter discs to rotate synchronously.
5. The method for preparing high-performance iron oxide for soft ferrite according to claim 4, characterized in that: The separation cabinet includes a cabinet body divided into a first chamber and a second chamber by a partition plate, one circumferential side of each primary separation filter disc is located in the first chamber, and the other circumferential side of the primary separation filter disc is located in the second chamber, a notch is opened at the upper part of the partition plate and at the upper end of each primary separation filter disc, and a discharge port is opened at the lower end of the second chamber and at each primary separation filter disc, and a mixture of raw ore powder and industrial hydrochloric acid enters the first chamber through a liquid inlet pipe system, and the liquid level of the mixture is lower than the lower end of the notch.
6. The method for preparing high-performance iron oxide for soft ferrite according to claim 4, characterized in that: The primary separation filter disc comprises a disc-shaped ceramic filter plate rotatably mounted on both sides of the mounting ring, an inner base tube is detachably connected to the inner edge of each disc-shaped ceramic filter plate, the inner base tubes of two adjacent primary separation filter discs close to each other are connected to each other, and a guide channel is formed between the inner base tubes connected to each other, and the filter chamber is formed in the space enclosed by the mounting ring and the two disc-shaped ceramic filter plates.
7. The method for preparing high-performance iron oxide for soft ferrite according to claim 6, characterized in that: A connecting spring is sleeved on the outside of each of the inner base tubes, and the two ends of the connecting tube are movably sleeved on the outside of the inner base tubes of the two adjacent primary separation filter plates that are close to each other, and the two ends of the connecting tube are respectively connected to the corresponding connecting springs; a guide bar is constructed on the outer wall of each of the inner base tubes, and each of the guide bars extends along the axial direction of the inner base tube, and a guide groove is opened on the inner wall of the connecting tube, and the guide groove extends along the axial direction of the connecting tube, and the guide bar is movably assembled in the guide groove.
8. The method for preparing high-performance iron oxide for soft ferrite according to claim 6, characterized in that: The assembly ring is fixedly installed with the separation cabinet, and the assembly ring is connected with the acid liquid replenishment pipe system; the acid liquid replenishment pipe system includes an acid replenishment main pipe connected with multiple first acid replenishment branch pipes and multiple second acid replenishment branch pipes, each of the first acid replenishment branch pipes is connected with a corresponding portion of the first chamber, each of the second acid replenishment branch pipes is connected with an acid replenishment joint on the corresponding assembly ring, a first acid replenishment valve and a second acid replenishment valve are respectively installed on each of the first acid replenishment branch pipes and each of the second acid replenishment branch pipes, and multiple spiral guide blades are constructed in each inner base pipe, and these spiral guide blades are evenly arranged along the circumference of the inner base pipe.
9. The method for preparing high-performance iron oxide for soft ferrite according to claim 4, characterized in that: A secondary membrane filtration mechanism is installed at one end of the outer side of the separation cabinet, and a guide pipe is connected to the outlet end of the secondary membrane filtration mechanism. The guide pipe passes through one end of the guide channel through each primary separation filter disc and out of the other end of the guide channel, and the outlet end of the guide pipe is connected to the separation cabinet through a fixed seat.
10. The method for preparing high-performance iron oxide for soft ferrite according to claim 9, characterized in that: The secondary membrane filtration mechanism includes a filter cartridge connected to one end of a guide channel through an adapter cartridge, a filter membrane tube is coaxially arranged in the filter cartridge, an end cap is detachably mounted on the end of the filter cartridge away from the adapter cartridge, a plurality of extrusion ports are provided on the end cap, a spiral guide blade extending along the axis of the filter cartridge is constructed on the inner wall of the filter cartridge, an end face of the spiral guide blade away from the filter cartridge is close to or in contact with the outer peripheral surface of the filter membrane tube, a plurality of conducting holes are provided on the portion of the spiral guide blade close to the adapter cartridge, a connecting seat is constructed at the end of the filter membrane tube, and the connecting seat is rotatably connected to the end cap; a plurality of drainage ports are evenly arranged on the adapter cartridge along its circumference, a transfer sleeve is rotatably connected to the outside of the adapter cartridge, the transfer sleeve is detachably connected to a separation cabinet, a drainage joint is constructed on the transfer sleeve, and a drainage valve is installed on the drainage joint.
Citation Information
Cited By
Production method of high-efficiency and environment-friendly high-purity ferric oxide powder