Method for constructing copper nano-cluster electrocatalyst based on amyloid fiber and application of copper nano-cluster electrocatalyst in chlorophenol wastewater

By constructing copper nanocluster electrocatalysts based on amyloid fibers, the problem of traditional electrocatalyst size is solved, and the efficient purification of chlorophenol wastewater is achieved, and the copper clusters are uniformly distributed and efficient catalytic effect is achieved. The low-cost Cu catalyst is comparable to that of precious metals. effect.

CN118908351AActive Publication Date: 2024-11-08CHANGZHOU UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410974496.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

In traditional electrocatalytic reduction technology, excessive size of the electrocatalyst leads to uneven reactions and low efficiency, and too small size leads to low active area and uncontrollable dispersion, making it difficult to effectively degrade chlorophenol wastewater.

Method used

The copper nanocluster electrocatalyst is constructed based on amyloid fibers, and the amyloid fibers are self-assembled on the titanium oxide substrate by lysozyme, and the TiSO-AFs-Cu cathode electrocatalyst is prepared by adding copper ions and reducing agents. The material is used to build the electrical Chemical reactors realize efficient purification of chlorophenol wastewater.

Benefits of technology

The efficient purification of chlorophenol wastewater is achieved, the copper clusters are uniformly distributed to maximize the effective surface area, avoiding mass transfer limitation, and the low-cost Cu catalyst achieves an effect comparable to precious metals, stable solid loading and high electrochemical active area .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908351A_ABST
    Figure CN118908351A_ABST
Patent Text Reader

Abstract

The invention discloses a method for constructing a copper nano-cluster electrocatalyst based on amyloid fiber and application of the copper nano-cluster electrocatalyst in chlorophenol wastewater, and the method comprises the following steps: dissolving lysozyme powder in water, and adjusting the pH value of the solution to 2 to prepare a lysozyme solution; the preparation method comprises the following steps: taking titanium oxide TiSO as a substrate, immersing into a lysozyme solution, heating and stirring to obtain an amyloid fiber AFs solution and a TiSO-AFs electrode; the TiSO-AFs electrode is taken out, an amyloid fiber solution, a copper metal ion solution and a reducing agent are added, so that copper ions are immobilized on the surface of the electrode and converted into a copper simple substance, the TiSO-AFs electrode is washed with deionized water and dried after standing, an electrochemical reactor is built through the material, and efficient purification of chlorophenol wastewater is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of synthesis of sewage treatment materials, and specifically relates to a method for constructing a copper nanocluster electrocatalyst based on amyloid fibers and an application of the method in chlorophenol wastewater. Background Art

[0002] There are three main pollutants in industrial wastewater: pathogenic pollutants, metal pollutants and organic pollutants. Among them, water pollution accidents caused by organic pollutants account for half of the total water pollution accidents. Compared with other pollutants, they are the most harmful to the water environment. These organic pollutants will cause serious pollution to the water environment, making the composition of industrial wastewater more complex, with higher concentration and salinity, greater pH changes, and more difficult to degrade. Some of them also have "three-cause" effects (i.e. carcinogenic, teratogenic, mutagenic) and bioaccumulation, posing a serious threat to human health and the ecological environment. Therefore, it is urgent to solve the problem of organic pollution.

[0003] Chlorophenols are a common organic pollutant produced in industries such as petroleum coking, papermaking and dyeing, and plastic manufacturing. They are widely used as organic solvents in wood preservatives, insecticides and herbicides, rust inhibitors, and paints and coatings. They are mainly distributed in soil and groundwater. The unique structure of chlorophenols makes them difficult to degrade, semi-volatile, highly toxic, and can remain in nature for a long time.

[0004] Therefore, effective treatment and pollution control of phenolic wastewater has become a key issue that needs to be addressed urgently.

[0005] At present, the treatment methods for chlorophenol wastewater at home and abroad mainly include physical and chemical methods (such as adsorption, extraction, membrane treatment), chemical oxidation methods (such as ozone oxidation, Fenton method, photocatalysis, ultrasonic degradation) and biological methods. However, these methods have their corresponding disadvantages. Physical and chemical methods are only applicable to specific pollutant concentrations and are prone to secondary pollution; biological treatment takes a long time, the equipment occupies a large area, and is toxic to microorganisms, and the treatment efficiency is low; chemical oxidation methods have high requirements for wastewater and reaction environment, and are also prone to secondary pollution. In contrast, electrocatalytic reduction technology is considered to be one of the most effective methods for degrading chlorophenol wastewater because of its green and efficient nature, no secondary pollutants, short treatment time, small footprint, applicability in a wide concentration range, and mild operating conditions.

[0006] However, in the actual application of traditional electrocatalytic reduction technology, some difficult-to-solve problems arise due to the size of the electrocatalyst. If the size is too large, uneven reaction and low efficiency may occur, while if the size is too small, migration-aggregation behavior may occur, resulting in low active area and uncontrollable dispersion. Summary of the invention

[0007] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0008] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.

[0009] Therefore, the purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for constructing a copper nanocluster electrocatalyst based on amyloid fibers.

[0010] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for constructing a copper nanocluster electrocatalyst based on amyloid fibers, comprising:

[0011] Dissolving lysozyme powder in water and adjusting the pH of the solution to 2 to prepare a lysozyme solution;

[0012] Titanium suboxide TiSO was used as a substrate, immersed in a lysozyme solution, heated and stirred, to obtain an amyloid fiber AFs solution and a TiSO-AFs electrode;

[0013] The TiSO-AFs electrode was taken out, and an amyloid fiber solution, a copper metal ion solution and a reducing agent were added to fix the copper ions on the electrode surface and convert them into copper element. After standing, the electrode was washed with deionized water and dried to obtain a TiSO-AFs-Cu electrode.

[0014] As a preferred embodiment of the method of the present invention, the mass fraction of the lysozyme solution is 1.8-2.2 wt %.

[0015] As a preferred embodiment of the method of the present invention, the heating and stirring comprises the following steps: the heating temperature is 90° C., the stirring speed is 180 to 200 rpm, and the stirring time is 5 to 12 hours.

[0016] As a preferred embodiment of the method of the present invention, the copper metal ion solution comprises a CuSO4 solution with a concentration of 0.1M.

[0017] As a preferred embodiment of the method of the present invention, the reducing agent comprises ascorbic acid solution with a concentration of 0.01M.

[0018] As a preferred embodiment of the method of the present invention, the volume ratio of the amyloid fiber solution, the copper metal ion solution and the reducing agent is 5:1:100.

[0019] Another object of the present invention is to overcome the deficiencies in the prior art and provide a copper nanocluster electrocatalyst.

[0020] Another object of the present invention is to overcome the deficiencies in the prior art and provide a copper nanocluster electrocatalyst for use in treating chlorophenol wastewater.

[0021] As a preferred solution of the application of the present invention, the reactor is separated into a cathode cell and an anode cell by a proton exchange membrane;

[0022] Titanium suboxide was used as the anode and TiSO-AFs-Cu electrode was used as the cathode;

[0023] During the whole reduction process, the constant potential was controlled at 5 V;

[0024] Wherein, the electrolyte is 0.1M Na2SO4 solution;

[0025] The cathode chamber contains 10 mg / L para-chlorophenol contaminated solution, the anode chamber contains 0.1M Na2SO4 electrolyte, and the action time is 60 minutes.

[0026] As a preferred solution of the application of the present invention, wherein: the proton exchange membrane is a nafion membrane with a size of 2cm×2cm; the volume of the cathode battery and the positive battery is 200mL each;

[0027] The electrode geometry of the cathode and anode is 2.5 cm×4 cm.

[0028] Beneficial effects of the present invention:

[0029] (1) The present invention provides a method for preparing a copper nano-electrocatalyst constructed of amyloid fibers that can achieve efficient purification of chlorophenol wastewater. Titanium dioxide TiSO is used as a substrate, lysozyme is used to self-assemble and synthesize amyloid fibers on the surface of the substrate, copper ion solution and a reducing agent are added to induce in situ preparation of TiSO-AFs-Cu cathode electrocatalyst, and an electrochemical reactor is constructed using the material to achieve efficient purification of chlorophenol wastewater.

[0030] (2) The surface of the amyloid fiber in the present invention is rich in amino acids, which can make the copper clusters evenly distributed when immobilized, maximize the effective surface area, and ensure the atomic utilization efficiency of the copper clusters; using the amyloid fiber as a template, small-sized copper clusters are constructed on the surface of the substrate electrode as cathode catalysts for electrocatalytic reduction, and based on the size effect, a high-efficiency catalytic effect that is not available in macroscopic bulk electrodes is obtained; the mesh substrate electrode realized by the present invention can avoid the disadvantage of limited mass transfer during the electrochemical reduction process; and the efficient operation of the system is achieved from both macroscopic and microscopic aspects.

[0031] (3) In traditional electrocatalytic reduction systems, precious metal catalysts are often used. This product uses Cu, which is abundant in material and low in cost, as the catalytic cathode of the system, which can achieve a catalytic effect comparable to that of precious metals such as palladium. In view of the shortcomings of traditional catalysts, such as difficult solid-liquid separation and uncontrollable distribution, amyloid fibers are used as templates to achieve stable immobilization of the catalyst on the substrate electrode. At the same time, AFs with a relatively high aspect ratio can be cross-linked into a three-dimensional network structure on the surface of the substrate electrode, ensuring a high solid loading amount and high electrochemical active area of ​​the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:

[0033] Figure 1 This is an AFM characterization image of the electrode material of the present invention;

[0034] Figure 2 This is a cycle removal effect diagram in an embodiment of the present invention;

[0035] Figure 3 This is a comparison chart of the effects of adding tert-butyl alcohol in the examples of the present invention. DETAILED DESCRIPTION

[0036] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0037] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0038] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0039] Example 1

[0040] (1) Take 2 g of lysozyme powder and dissolve it in 95 g of water. Then slowly add 1 M HCl solution and measure the pH value of the solution until the pH reaches 2.

[0041] (2) Insert the TiSO electrode into the prepared lysozyme solution, then place it in an oil bath, stir continuously for 8 h at 90°C to allow it to react fully;

[0042] (3) Take out the constructed TiSO-AFs electrode and put it into a new container. First, add 5 mL of the amyloid fiber solution prepared in step (2) into it. Then put it into a shaker and slowly add 1 mL of 0.1 M CuSO4 solution into it while shaking at a low speed.

[0043] (4) Adjust the shaking speed to medium (580 r / min) and shake continuously for 24 h;

[0044] While shaking on a shaker at a low speed (100 r / min), slowly add 100 mL of 0.01 M ascorbic acid solution to the solution, then set the temperature to 60 °C and adjust the shaking speed to medium (580 r / min) for 24 h.

[0045] The AFM characterization of the prepared electrode material can be found in Figure 1 .

[0046] Example 2

[0047] (1) Take 4 g of lysozyme powder and dissolve it in 190 g of water. Then slowly add 1 M HCl solution and measure the pH value of the solution until the pH reaches 2.

[0048] (2) Insert the TiSO electrode into the prepared lysozyme solution, then place it in an oil bath, stir continuously for 8 h at 90°C to allow it to react fully;

[0049] (3) Take out the constructed TiSO-AFs electrode and put it into a new container. First, add 5 mL of the amyloid fiber solution prepared in step (2) into it. Then put it into a shaker and slowly add 1 mL of 0.1 M CuSO4 solution into it while shaking at a low speed.

[0050] (4) Adjust the shaking speed to medium (580 r / min) and shake continuously for 24 h;

[0051] While shaking on a shaker at a low speed (100 r / min), 100 mL of 0.01 M ascorbic acid solution was slowly added to the solution, and then the temperature was set to 60° C., the shaking speed of the shaker was adjusted to a medium speed (580 r / min), and the solution was shaken for 24 h.

[0052] Example 3

[0053] (1) Take 2 g of lysozyme powder and dissolve it in 95 g of water. Then slowly add 1 M HCl solution and measure the pH value of the solution until the pH reaches 2.

[0054] (2) Insert the TiSO electrode into the prepared lysozyme solution, then place it in an oil bath, stir continuously for 12 h at 90 °C to allow it to react fully;

[0055] (3) Take out the constructed TiSO-AFs electrode and put it into a new container. First, add 5 mL of the amyloid fiber solution prepared in step (2) into it. Then put it into a shaker and slowly add 1 mL of 0.1 M CuSO4 solution into it while shaking at a low speed.

[0056] (4) Adjust the shaking speed to medium (580 r / min) and shake continuously for 24 h;

[0057] While shaking on a shaker at a low speed (100 r / min), 100 mL of 0.01 M ascorbic acid solution was slowly added to the solution, and then the temperature was set to 60° C., the shaking speed of the shaker was adjusted to a medium speed (580 r / min), and the solution was shaken for 24 h.

[0058] Application Example 1

[0059] The reactor was separated into a cathode cell (200 mL) and an anode cell (200 mL) by a proton exchange membrane (2 cm × 2 cm);

[0060] A titanium oxide with a length of 4 cm and a width of 2.5 cm was used as an anode; a TiSO-AFs-Cu electrode with a length of 4 cm and a width of 2.5 cm (prepared in Example 1) was used as a cathode;

[0061] During the whole reduction experiment, the constant potential on the cathode was controlled by the current technology of the switching power supply, the voltage was 5 V, and 0.1 M Na2SO4 was used as the background electrolyte;

[0062] Reaction voltage conditions: constant 5V voltage;

[0063] Reaction solution volume requirements: 200 mL in the cathode chamber, 10 mg / L 4-CP contaminated solution, 200 mL in the anode chamber, 0.1 M Na2SO4 electrolyte;

[0064] Reaction time requirement: 60min;

[0065] The polluted wastewater is added to the cathode chamber of the reactor before the reaction, and the removal rate of pollutants is 99.5%.

[0066] Application Example 2

[0067] The reactor was separated into a cathode cell (200 mL) and an anode cell (200 mL) by a proton exchange membrane (2 cm × 2 cm);

[0068] A titanium oxide with a length of 4 cm and a width of 2.5 cm was used as an anode; a TiSO-AFs-Cu electrode with a length of 4 cm and a width of 2.5 cm (prepared in Example 2) was used as a cathode;

[0069] During the whole reduction experiment, the constant potential on the cathode was controlled by the current technology of the switching power supply, the voltage was 10 V, and 0.1 M Na2SO4 was the background electrolyte;

[0070] 200 mL of cathode chamber, 10 mg / L 4-CP contaminated solution; 200 mL of anode chamber, 0.1 M Na2SO4 electrolyte;

[0071] Reaction time requirement: 60min;

[0072] The polluted wastewater was added to the cathode chamber of the reactor before the reaction, and the removal rate of pollutants was 99.6%.

[0073] Application Example 3

[0074] The reactor was separated into a cathode cell (200 mL) and an anode cell (200 mL) by a proton exchange membrane (2 cm × 2 cm);

[0075] A titanium oxide with a length of 4 cm and a width of 2.5 cm was used as an anode; a TiSO-AFs-Cu electrode with a length of 4 cm and a width of 2.5 cm (prepared in Example 3) was used as a cathode;

[0076] During the whole reduction experiment, the constant potential on the cathode was controlled by the current technology of the switching power supply, with a constant voltage of 5V;

[0077] Reaction solution volume requirements: 200 mL in the cathode chamber, 10 mg / L 4-CP contaminated solution;

[0078] Anode chamber 200mL, 0.05M Na2SO4 electrolyte; reaction time requirement: 60min;

[0079] The polluted wastewater was added to the cathode chamber of the reactor before the reaction, and the removal rate of pollutants was 98.2%.

[0080] Application Example 4

[0081] The same conditions as in Application Example 1 were set, with a reaction period of 60 min, and a continuous cycle reaction was performed;

[0082] React for 10 cycles and record the experimental results. Figure 2 ;

[0083] The experimental results show that the removal effect of each cycle is consistent, and the pollutant removal rate of 60 minutes is close to 100%, indicating that the material prepared in this experiment is stable.

[0084] Comparative Example 1

[0085] (1) Take 2 g of lysozyme powder and dissolve it in 70 g of water. Then slowly add 1 M HCl solution and measure the pH value of the solution until the pH reaches 2.

[0086] (2) Insert the TiSO electrode into the prepared lysozyme solution, then place it in an oil bath, stir continuously for 8 h at 90°C to allow it to react fully;

[0087] (3) Take out the constructed TiSO-AFs electrode and put it into a new container. First, add 5 mL of the amyloid fiber solution prepared in step (2) into it. Then put it into a shaker and slowly add 1 mL of 0.1 M CuSO4 solution into it while shaking at a low speed.

[0088] (4) Adjust the shaking speed to medium (580 r / min) and shake continuously for 24 h;

[0089] While shaking on a shaker at a low speed (100 r / min), 100 mL of 0.01 M ascorbic acid solution was slowly added to the solution, and then the temperature was set to 60° C., the shaking speed of the shaker was adjusted to a medium speed (580 r / min), and the solution was shaken for 24 h.

[0090] Comparative Example 2

[0091] (1) Take 2 g of lysozyme powder and dissolve it in 95 g of water. Then slowly add 1 M HCl solution and measure the pH value of the solution simultaneously until the pH reaches 2.

[0092] (2) Insert the TiSO electrode into the prepared lysozyme solution, then place it in an oil bath and stir it continuously for 8 h at 60 °C to allow it to react fully.

[0093] (3) Take out the constructed TiSO-AFs electrode and put it into a new container. First, add 5 mL of the amyloid fiber solution prepared in step (2) into it. Then put it into a shaker and slowly add 1 mL of 0.1 M CuSO4 solution into it while shaking at a low speed.

[0094] (4) Adjust the shaking speed of the shaker to medium and shake continuously for 24 h. While the shaker is shaking at a low speed, slowly add 100 mL of 0.01 M ascorbic acid solution to the solution. Then set the temperature to 60°C and adjust the shaking speed of the shaker to medium for 24 h.

[0095] Comparative Example 3

[0096] (1) Take 2 g of lysozyme powder and dissolve it in 95 g of water. Then slowly add 1 M HCl solution and measure the pH value of the solution simultaneously until the pH reaches 2.

[0097] (2) Insert the TiSO electrode into the prepared lysozyme solution, then place it in an oil bath and stir it continuously for 8 hours at 90°C to allow it to react fully.

[0098] (3) Take out the constructed TiSO-AFs electrode and put it into a new container. First, add 5 mL of the amyloid fiber solution prepared in step (2) into it. Then put it into a shaker and slowly add 1 mL of 0.1 M CuSO4 solution into it while shaking at a low speed.

[0099] (4) Adjust the shaking speed of the shaker to medium and shake continuously for 24 h. While the shaker is shaking at a low speed, slowly add 1 mL of 0.056 M sodium borohydride solution to the solution. Then set the temperature to 60°C and adjust the shaking speed of the shaker to medium for 24 h.

[0100] Comparative Example 4

[0101] (1) Take 2 g of camel milk, dissolve it in 95 g of water, then slowly add 1 M HCl solution, and measure the pH value of the solution simultaneously until the pH is 2;

[0102] (2) Insert the TiSO electrode into the prepared lysozyme solution, then place it in an oil bath, stir continuously for 8 h at 90°C to allow it to react fully;

[0103] (3) Take out the constructed TiSO-AFs electrode and put it into a new container. First, add 5 mL of the amyloid fiber solution prepared in step (2) into it. Then put it into a shaker and slowly add 1 mL of 0.1 M CuSO4 solution into it while shaking at a low speed.

[0104] (4) Adjust the shaking speed to medium and shake continuously for 24 hours;

[0105] While the shaker was shaking at a low speed, 100 mL of 0.01 M ascorbic acid solution was slowly added to the solution, and then the temperature was set to 60° C., the shaking speed of the shaker was adjusted to medium, and the mixture was shaken for 24 h.

[0106] Comparative Example 5

[0107] (1) Take 2 g of lysozyme powder and dissolve it in 95 g of water. Then slowly add 1 M HCl solution and measure the pH value of the solution until the pH reaches 2.

[0108] (2) Insert the TiSO electrode into the prepared lysozyme solution, then place it in an oil bath, stir it continuously for 8 hours at 100°C to allow it to react fully;

[0109] (3) Take out the constructed TiSO-AFs electrode and put it into a new container. First, add 5 mL of the amyloid fiber solution prepared in step (2) into it. Then put it into a shaker and slowly add 1 mL of 0.1 M CuSO4 solution into it while shaking at a low speed.

[0110] (4) Adjust the shaking speed to medium and shake continuously for 24 hours;

[0111] While the shaker was shaking at a low speed, 100 mL of 0.01 M ascorbic acid solution was slowly added to the solution, and then the temperature was set to 60° C., the shaking speed of the shaker was adjusted to medium, and the mixture was shaken for 24 h.

[0112] The 10 mg / L 4-CP contaminated liquid was treated according to the treatment method of Application Example 1. The measurement results are shown in Table 1.

[0113] Table 1

[0114]

[0115] As can be seen from Table 1, the mass fraction of the lysozyme solution in Comparative Example 1 was changed from 2% to 2.8%, and the pollutant removal rate was 99.4% in 60 minutes.

[0116] In comparative example 2, the temperature of the oil bath was changed from 90°C to 60°C, and the pollutant removal rate was 99.1% in 60 minutes;

[0117] Comparative Example 3: When reducing the electrode, the reducing agent added was changed from 100 mL of 0.01 M ascorbic acid to 1 mL of 0.056 M sodium borohydride solution. The pollutant removal rate was 78.2% in 60 minutes.

[0118] Comparative Example 4: Lysozyme was replaced with camel milk, and the pollutant removal rate after 60 min of reaction was only 0.3%;

[0119] In Comparative Example 5, the temperature of the oil bath was changed from 90° C. to 100° C., and the pollutant removal effect in 60 minutes was 31.9%.

[0120] Comparative Example 6

[0121] (1) Take 2 g of lysozyme powder and dissolve it in 95 g of water. Then slowly add 1 M HCl solution and measure the pH value of the solution until the pH reaches 2.

[0122] (2) Insert the TiSO electrode into the prepared lysozyme solution, then place it in an oil bath, stir continuously for 8 h at 90°C to allow it to react fully;

[0123] (3) Take out the constructed TiSO-AFs electrode and put it into a new container. First, add 5 mL of the amyloid fiber solution prepared in step (2) into it. Then put it into a shaker and slowly add 1 mL of 0.1 M CuSO4 solution into it while shaking at a low speed.

[0124] (4) Adjust the shaking speed to medium and shake continuously for 24 hours;

[0125] While the shaker was shaking at a low speed, 100 mL of 0.01 M ascorbic acid solution was slowly added to the solution, and then the temperature was set to 60° C., the shaking speed of the shaker was adjusted to medium, and the mixture was shaken for 24 h.

[0126] Three identical TiSO-AFs-Cu electrodes were prepared according to the above steps (1), (2), (3), and (4), and were placed in the reactor for reaction. 1 mL of 10 mM, 0.1 mL of 10 mM, and 0 mL of 10 Mm tert-butyl alcohol solution were added to the reacting pollutant solution in turn, and the reaction was carried out for 60 min respectively. Figure 3 The removal effects were 18.9%, 62.5% and 99.4% respectively. Tert-butyl alcohol is a free radical quencher. The experimental results show that the electrode treats 4-cp by generating free radicals.

[0127] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.

Claims

1. A method for constructing copper nanocluster electrocatalysts based on amyloid fibers, characterized in that: include, Dissolving lysozyme powder in water and adjusting the pH of the solution to 2 to prepare a lysozyme solution; Titanium suboxide TiSO was used as a substrate, immersed in a lysozyme solution, heated and stirred, to obtain an amyloid fiber AFs solution and a TiSO-AFs electrode; The TiSO-AFs electrode was taken out, and amyloid fiber AFs solution, copper metal ion solution and reducing agent were added to fix the copper ions on the electrode surface and convert them into copper element. After standing, it was washed with deionized water and dried to obtain a TiSO-AFs-Cu electrode.

2. The method according to claim 1, characterized in that: The mass fraction of the lysozyme solution is 1.8-2.2 wt %.

3. The method according to claim 1 or 2, characterized in that: The heating and stirring, wherein the heating temperature is 90° C., the stirring speed is 180-200 rpm, and the stirring time is 5-12 hours.

4. The method according to claim 1, characterized in that: The copper metal ion solution includes a CuSO4 solution with a concentration of 0.1M.

5. The method according to claim 1, characterized in that: The reducing agent includes ascorbic acid solution, and the concentration is 0.01M.

6. The method according to any one of claims 1, 2, 4 or 5, characterized in that: The volume ratio of the amyloid fiber solution, the copper metal ion solution and the reducing agent is 5:1:

100.

7. The copper nanocluster electrocatalyst prepared by the method according to any one of claims 1 to 6.

8. Use of the copper nanocluster electrocatalyst as claimed in claim 7 in treating chlorophenol wastewater.

9. The use according to claim 8, characterized in that: include, The reactor is separated into a cathode cell and an anode cell by a proton exchange membrane; Titanium suboxide was used as the anode and TiSO-AFs-Cu electrode was used as the cathode; During the whole reduction process, the constant potential was controlled at 5 V; Wherein, the electrolyte is 0.1M Na2SO4 solution; The cathode chamber contains 10 mg / L para-chlorophenol contaminated solution, the anode chamber contains 0.1M Na2SO4 electrolyte, and the action time is 60 minutes.

10. The use according to claim 9, characterized in that: The proton exchange membrane is a nafion membrane with a size of 2cm×2cm; the capacity of the cathode battery and the positive battery is 200mL each; The electrode geometry of the cathode and anode is 2.5 cm×4 cm.

Citation Information

Patent Citations

  • Ti<n>O<2n-1> doped electrode, and preparation method thereof and use thereof

    CN108911052A

  • Preparation method and application of Fe and Cu double-monatomic anchored Ti4O7 electrode

    CN115650375A

  • Electrical energy devices

    US20030036001A1

  • Membrane electrode assembly with improved cohesion

    US20210126262A1