High-performance temperable high-transmittance three-silver low-emissivity coated glass and preparation method thereof

By designing multi-layer film structures in low-radiation coated glass, including tin oxide, zinc oxide, zinc oxide, silver, titanium and other materials, and using magnetron sputtering technology to deposit the film layer, the light transmittance and The trade-off between sunshade performance achieves a balance between high light transmittance and good sunshade effect, and improves the stability and processing performance of glass.

CN118908592AInactive Publication Date: 2024-11-08XIANNING CSG ENERGY SAVING GLASS +1

Patent Information

Application Number
CN202411097474.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

While existing low-radiation coating glasses increase light transmittance, their sunshade performance often decreases, making it difficult to take into account high light transmittance and good sunshade effects.

Method used

High-performance tempered high-transparent three-silver low-radiation coating glass, the coating layer consists of eighteen layers of films, including tin oxide, zinc oxide, zinc oxide, silver, titanium, zinc oxide and other materials, and is subject to magnetron sputtering. The technology deposits the film layer to ensure the optimization of the film layer thickness and gas ratio, and form a stable silver-titanium alloy layer and zinc-tin oxide layer to improve transmittance and sunshade performance.

Benefits of technology

It achieves good sunshade effect while maintaining high light transmittance, with a light-heat ratio of more than 2.0, and is not easy to scratch during subsequent processing and transportation, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908592A_ABST
    Figure CN118908592A_ABST
Patent Text Reader

Abstract

The invention provides high-performance temperable high-transmittance three-silver low-emissivity coated glass and a preparation method thereof, and belongs to the technical field of fine and deep processing of glass. Comprising a glass substrate layer and a coating layer, the coating layer is sequentially compounded with eighteen film layers from the glass substrate layer to the outside, and the eighteen film layers comprise the first tin oxide layer, the second zinc tin oxide layer, the third zinc oxide layer, the fourth silver layer, the fifth titanium layer, the sixth zinc oxide layer, the seventh zinc tin oxide layer and the eighth zinc oxide layer. The ninth layer is a silver layer, the tenth layer is a titanium layer, the eleventh layer is a zinc oxide layer, the twelfth layer is a zinc tin oxide layer, the thirteenth layer is a zinc oxide layer, the fourteenth layer is a silver layer, the fifteenth layer is a titanium layer, the sixteenth layer is a zinc oxide layer, the seventeenth layer is a zinc tin oxide layer, and the eighteenth layer is a zirconium oxide layer. The glass provided by the invention has the advantages of high transmittance, good sun-shading performance, high film layer structure stability, tempering capability and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of glass deep processing, and in particular relates to high-performance temperable high-transmittance triple-silver low-emissivity coated glass and a preparation method thereof. Background Art

[0002] In the field of modern architecture, glass materials have become an indispensable component due to their beauty, light transmission and structural characteristics. As society's requirements for architectural aesthetics and functionality continue to increase, glass is no longer just a transparent partition of the structure, but has gradually become an intelligent material that meets multiple functional requirements. In particular, low-emissivity (LOW-E) coated glass has become a hot topic in the construction industry because of its significant effects in energy saving, heat insulation and improving indoor comfort.

[0003] Low-emissivity glass can effectively reflect indoor heat and reduce heat loss by coating one or more layers of metal or metal oxide films on the glass surface, while allowing natural light to enter and improving the lighting effect. However, there is often a trade-off between the performance of this type of glass and its light transmittance and sunshade performance. As the light transmittance increases, although the lighting effect is improved, the sunshade performance may decrease. Therefore, a new type of low-emissivity coated glass is provided, which can maintain high light transmittance while also having good sunshade performance, thereby achieving green energy saving of buildings and improving the comfort of residents. Summary of the invention

[0004] The purpose of the present invention is to provide a high-performance temperable high-transmittance triple-silver low-emissivity coated glass and a preparation method thereof in order to improve the transmittance while also achieving good sunshade effect in view of the above-mentioned problems existing in the prior art.

[0005] The object of the present invention can be achieved by the following technical scheme: high-performance temperable high-transmittance three-silver low-emissivity coated glass, characterized in that the coated glass comprises a glass substrate layer and a coating layer, and the coating layer is compounded with eighteen film layers in sequence from the glass substrate layer to the outside, wherein the first layer is a tin oxide layer, the second layer is a zinc oxide tin layer, the third layer is a zinc oxide layer, the fourth layer is a silver layer, the fifth layer is a titanium layer, the sixth layer is a zinc oxide layer, the seventh layer is a zinc oxide tin layer, the eighth layer is a zinc oxide layer, the ninth layer is a silver layer, the tenth layer is a titanium layer, the eleventh layer is a zinc oxide layer, the twelfth layer is a zinc oxide tin layer, the thirteenth layer is a zinc oxide layer, the fourteenth layer is a silver layer, the fifteenth layer is a titanium layer, the sixteenth layer is a zinc oxide layer, the seventeenth layer is a zinc oxide tin layer, and the eighteenth layer is a zirconium oxide layer.

[0006] Preferably, the coating thickness of the first layer is 15 to 25 nanometers, the coating thickness of the second layer is 10 to 25 nanometers, the coating thickness of the third layer is 5 to 15 nanometers, the coating thickness of the fourth layer is 10 to 20 nanometers, and the coating thickness of the fifth layer is 1 to 6 nanometers; the coating thickness of the sixth layer is 10 to 20 nanometers; the coating thickness of the seventh layer is 35 to 50 nanometers; the coating thickness of the eighth layer is 5 to 10 nanometers; the coating thickness of the ninth layer is 10 to 20 nanometers; the coating thickness of the tenth layer is 1 to 6 nanometers; the coating thickness of the eleventh layer is 5 to 15 nanometers; the coating thickness of the twelfth layer is 50 to 65 nanometers; the coating thickness of the thirteenth layer is 5 to 15 nanometers; the coating thickness of the fourteenth layer is 15 to 30 nanometers; the coating thickness of the fifteenth layer is 1 to 6 nanometers; the coating thickness of the sixteenth layer is 5 to 15 nanometers; the coating thickness of the seventeenth layer is 10 to 20 nanometers; and the coating thickness of the eighteenth layer is 5 to 10 nanometers.

[0007] The method for preparing the above-mentioned high-performance temperable high-transmittance triple-silver low-emissivity coated glass is characterized in that the method comprises the following steps:

[0008] 1) Select float glass as the glass substrate layer;

[0009] 2) Use a coating-specific washing machine to clean and dry the glass substrate layer. Before coating, the surface of the glass substrate layer must be dry, free of impurities and static electricity; use deionized water for cleaning, and the water resistance must be greater than 10μs / cm;

[0010] 3) Magnetron sputtering coating

[0011] A. Magnetron sputtering first layer

[0012] Target quantity: 1 to 2 AC rotating targets; target configuration is tin oxide (SnO x ); Process gas ratio: argon and nitrogen, the ratio of argon and nitrogen is 1:1.8; sputtering pressure is 3~5×10 -3 mbar;

[0013] B. Magnetron sputtering second layer

[0014] Target quantity: 2 to 3 AC rotating targets; target configuration is zinc tin oxide (ZnSnO x ); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 1:1.8; sputtering pressure is 3~5×10 -3 mbar;

[0015] C. Magnetron sputtering third layer

[0016] Target quantity: 1-2 AC rotating targets; target configuration is zinc oxide (SnO x); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 1:1.8; sputtering pressure is 3~5×10 -3 mbar;

[0017] D. Magnetron sputtering fourth layer

[0018] Target quantity: 1 DC plane target; target configuration is silver (Ag); process gas ratio: pure argon; sputtering gas pressure is 2-3×10 -3 mbar;

[0019] E. Magnetron sputtering fifth layer

[0020] Target quantity: 1 AC rotating target; target configuration is titanium (Ti); process gas ratio: pure argon; sputtering gas pressure is 2-3×10 -3 mbar;

[0021] F. Magnetron sputtering sixth layer

[0022] Target quantity: 1 to 2 AC rotating targets; target configuration is zinc oxide (SnO x ); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 1:1.8; sputtering pressure is 2~3×10 -3 mbar;

[0023] G. Magnetron sputtering seventh layer

[0024] Target quantity: 1 to 2 AC rotating targets; target configuration is zinc tin oxide (ZnSnO x ); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 1:1.8; sputtering pressure is 3~5×10 -3 mbar;

[0025] H. Magnetron sputtering eighth layer

[0026] Target quantity: 2 to 4 AC rotating targets; target configuration is zinc oxide (SnO x ); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 1:1.8; sputtering pressure is 3~5×10 -3 mbar;

[0027] I. Magnetron sputtering ninth layer

[0028] Target quantity: 1 DC plane target; target configuration is silver (Ag); process gas ratio: pure argon; sputtering gas pressure is 2-3×10 -3 mbar;

[0029] J. Magnetron sputtering tenth layer

[0030] Target quantity: 1 AC flat target; target configuration is titanium (Ti); process gas ratio: argon and oxygen, the ratio of argon and oxygen is 3:1; sputtering pressure is 2~3×10 -3 mbar;

[0031] K. Magnetron sputtering eleventh layer

[0032] Target quantity: 1 to 2 AC plane targets; target configuration is zinc oxide (SnO x ); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 1:1.8; sputtering pressure is 3~5×10 -3 mbar;

[0033] L. Magnetron sputtering twelfth layer

[0034] Target quantity: 2 to 4 AC rotating targets; the target material is zinc tin oxide (ZnSnO x ); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 1:1.8; sputtering pressure is 3~5×10 -3 mbar;

[0035] M, magnetron sputtering thirteenth layer

[0036] Target quantity: 1 to 2 AC plane targets; target configuration is zinc oxide (SnO x ); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 1:1.8; sputtering pressure is 3~5×10 -3 mbar

[0037] N. Magnetron sputtering 14th layer

[0038] Target quantity: 1 DC plane target; target configuration is silver (Ag); process gas ratio: pure argon; sputtering gas pressure is 2-3×10 -3 mbar;

[0039] O. Magnetron sputtering fifteenth layer

[0040] Target quantity: 1 AC flat target; target configuration is titanium (Ti); process gas ratio: argon and oxygen, the ratio of argon and oxygen is 3:1; sputtering pressure is 2~3×10 -3 mbar;

[0041] P, magnetron sputtering sixteenth layer

[0042] Target quantity: 1 to 2 AC plane targets; target configuration is zinc oxide (SnO x ); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 1:1.8; sputtering pressure is 3~5×10 -3 mbar

[0043] Q. Magnetron sputtering seventeenth layer

[0044] Target quantity: 2 to 4 AC rotating targets; the target material is zinc tin oxide (ZnSnO x ); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 1:1.8; sputtering pressure is 3~5×10 -3 mbar

[0045] R, magnetron sputtering eighteenth layer

[0046] Target quantity: 1 to 2 AC plane targets; the target material is zirconium oxide (ZrO x ); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 20:1; sputtering pressure is 3~5×10 -3 mbar

[0047] 4) The total film thickness is controlled at 198-383 nm, and the transmission speed of the sputtering chamber is generally controlled at 3.0-6.0 m / min.

[0048] Advantages of the present invention:

[0049] 1. The transmittance of this patented technology product 6mm ultra-white single piece is T∈[70,80], a*∈[0,-3], b*∈[-1,+5]; the glass surface color is a*∈[2,-1], b*∈[-3,-9]; the film surface color is a*∈[0,-2], b*∈[-5,-10];

[0050] 2. It can be processed by subsequent cutting, edging, tempering or bending, etc. It can be produced on a large scale and is not easy to be scratched or oxidized during long-term transportation and storage.

[0051] 3. Light-to-heat ratio performance>2.0; BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 It is a schematic diagram of the layered structure of the coated glass.

[0053] In the figure, G, glass substrate layer; 1, first layer; 2, second layer; 3, third layer; 4, fourth layer; 5, fifth layer; 6, sixth layer; 7, seventh layer; 8, eighth layer; 9, ninth layer; 10, tenth layer; 11, eleventh layer; 12, twelfth layer; 13, thirteenth layer; 14, fourteenth layer; 15, fifteenth layer; 16, sixteenth layer; 17, seventeenth layer; 18, eighteenth layer. DETAILED DESCRIPTION

[0054] The present invention will be described in detail below in conjunction with the accompanying drawings.

[0055] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0056] The structure of the low-emissivity coated glass in the embodiment of the present invention is as follows.

[0057] like Figure 1 As shown, the high-performance temperable high-transmittance triple-silver low-emissivity coated glass comprises a glass substrate layer and a coating layer, wherein the coating layer is compounded with eighteen film layers in sequence from the glass substrate layer to the outside, wherein the first layer 1 is a tin oxide layer, the second layer 2 is a zinc oxide tin layer, the third layer 3 is a zinc oxide layer, the fourth layer 4 is a silver layer, the fifth layer 5 is a titanium layer, the sixth layer 6 is a zinc oxide layer, the seventh layer 7 is a zinc oxide tin layer, the eighth layer 8 is a zinc oxide layer, the ninth layer 9 is a silver layer, the tenth layer 10 is a titanium layer, the eleventh layer is a zinc oxide layer, the twelfth layer is a zinc oxide tin layer, the thirteenth layer is a zinc oxide layer, the fourteenth layer is a silver layer, the fifteenth layer is a titanium layer, the sixteenth layer is a zinc oxide layer, the seventeenth layer is a zinc oxide tin layer, and the eighteenth layer is a zirconium oxide layer.

[0058] like Figure 1 As shown, the coating thickness of the first layer 1 is 15 to 25 nanometers, the coating thickness of the second layer 2 is 10 to 25 nanometers, the coating thickness of the third layer 3 is 5 to 15 nanometers, the coating thickness of the fourth layer 4 is 10 to 20 nanometers, the coating thickness of the fifth layer is 1 to 6 nanometers; the coating thickness of the sixth layer 6 is 10 to 20 nanometers; the coating thickness of the seventh layer 7 is 35 to 50 nanometers; the coating thickness of the eighth layer 8 is 5 to 10 nanometers; the coating thickness of the ninth layer 9 is 10 to 20 nanometers; the coating thickness of the tenth layer 10 is 10 to 20 nanometers. The coating thickness is 1 to 6 nanometers; the coating thickness of the eleventh layer 11 is 5 to 15 nanometers; the coating thickness of the twelfth layer 12 is 50 to 65 nanometers; the coating thickness of the thirteenth layer 13 is 5 to 15 nanometers; the coating thickness of the fourteenth layer 14 is 15 to 30 nanometers; the coating thickness of the fifteenth layer 15 is 1 to 6 nanometers; the coating thickness of the sixteenth layer 16 is 5 to 15 nanometers; the coating thickness of the seventeenth layer 17 is 10 to 20 nanometers; the coating thickness of the eighteenth layer 18 is 5 to 10 nanometers.

[0059] This coated glass uses a tin oxide layer as the bottom layer, which makes the film layer and the glass more firmly bonded, and can effectively prevent the film layer from falling off during subsequent processing; each low-emissivity functional layer (silver layer) is plated with a titanium layer on top, and in the subsequent tempering process, the two layers are combined with each other to form a silver-titanium alloy layer, further improving the transmittance of the glass. At the same time, since zinc tin oxide has high light absorption and transmission properties, this coated glass has both high transmittance and good sunshade performance; furthermore, in this coated glass, zinc oxide layers are set on both sides of the zinc tin oxide layer, so that it is more tightly bonded with the silver-titanium alloy layer formed after tempering, improving the structural stability of the film layer, and preventing the film layer from falling off.

[0060] The method for preparing the low-emissivity coated glass according to the embodiment of the present invention is as follows.

[0061] 1) Select float glass as the glass substrate layer;

[0062] 2) Use a coating-specific washing machine to clean and dry the glass substrate layer. Before coating, the surface of the glass substrate layer must be dry, free of impurities and static electricity; use deionized water for cleaning, and the water resistance must be greater than 10μs / cm;

[0063] 3) The above film layers are deposited by magnetron sputtering vacuum coating. Before production or experiment, ensure that the vacuum degree is less than 3.5×10 -3 bar, the targets of various coating materials operate normally. The specific coating processes, targets and parameters used are shown in Table 1.

[0064]

[0065]

[0066] 4) The total film thickness is controlled at 198-383 nm, and the transmission speed of the sputtering chamber is generally controlled at 3.0-6.0 m / min.

[0067] After testing, the color parameters of the coated glass in this embodiment before and after tempering are shown in Table 2 below:

[0068]

[0069] After testing, the performance parameters of the coated glass after tempering in this embodiment are shown in Table 3 below:

[0070]

[0071]

[0072] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner without departing from the spirit of the present invention or exceeding the scope defined by the appended claims.

Claims

1. High performance temperable high transmittance triple silver low emissivity coated glass, characterized by: The coated glass comprises a glass substrate layer (G) and a coating layer, wherein the coating layer is compounded with eighteen film layers in sequence from the glass substrate layer (G) outwards, wherein the first layer (1) is a tin oxide layer, the second layer (2) is a zinc tin oxide layer, the third layer (3) is a zinc oxide layer, the fourth layer (4) is a silver layer, the fifth layer (5) is a titanium layer, the sixth layer (6) is a zinc oxide layer, the seventh layer (7) is a zinc tin oxide layer, the eighth layer (8) is a zinc oxide layer, the ninth layer (9) is a silver layer, the tenth layer (10) is a titanium layer, the eleventh layer (11) is a zinc oxide layer, the twelfth layer (12) is a zinc tin oxide layer, the thirteenth layer (13) is a zinc oxide layer, the thirteenth layer (14) is a silver layer, the fifteenth layer (15) is a titanium layer, the sixteenth layer (16) is a zinc oxide layer, the seventeenth layer (17) is a zinc tin oxide layer, and the eighteenth layer (18) is a zirconium oxide layer.

2. The high-performance temperable high-transmittance triple-silver low-emissivity coated glass according to claim 1, characterized in that: The coating thickness of the first layer (1) is 15 to 25 nanometers, the coating thickness of the second layer (2) is 10 to 25 nanometers, the coating thickness of the third layer (3) is 5 to 15 nanometers, the coating thickness of the fourth layer (4) is 10 to 20 nanometers, the coating thickness of the fifth layer (5) is 1 to 6 nanometers; the coating thickness of the sixth layer (6) is 10 to 20 nanometers; the coating thickness of the seventh layer (7) is 35 to 50 nanometers; the coating thickness of the eighth layer (8) is 5 to 10 nanometers; the coating thickness of the ninth layer (9) is 10 to 20 nanometers; and the coating thickness of the tenth layer The coating thickness of the eleventh layer (11) is 5 to 15 nanometers; the coating thickness of the twelfth layer (12) is 50 to 65 nanometers; the coating thickness of the thirteenth layer (13) is 5 to 15 nanometers; the coating thickness of the thirteenth layer (14) is 15 to 30 nanometers; the coating thickness of the fifteenth layer (15) is 1 to 6 nanometers; the coating thickness of the sixteenth layer (16) is 5 to 15 nanometers; the coating thickness of the seventeenth layer (17) is 10 to 20 nanometers; and the coating thickness of the eighteenth layer (18) is 5 to 10 nanometers.

3. A method for preparing the high-performance temperable high-transmittance triple-silver low-emissivity coated glass according to claim 1, characterized in that: This method comprises the following steps: 1) Selecting a float glass substrate as the glass substrate layer (G); 2) Use a coating-specific washing machine to clean and dry the glass substrate layer (G). Before coating, the surface of the glass substrate layer (G) must be dry, free of impurities and static electricity; use deionized water for cleaning, and the water resistance must be greater than 10μs / cm; 3) Magnetron sputtering coating A. Magnetron sputtering first layer (1) Target quantity: 1 to 2 AC rotating targets; target configuration is tin oxide (SnO x ); Process gas ratio: argon and nitrogen, the ratio of argon and nitrogen is 1:1.8; sputtering pressure is 3~5×10 -3 mbar; B. Magnetron sputtering second layer (2) Target quantity: 2 to 3 AC rotating targets; target configuration is zinc tin oxide (ZnSnO x ); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 1:1.8; sputtering pressure is 3~5×10 -3 mbar; C. Magnetron sputtering third layer (3) Target quantity: 1-2 AC rotating targets; target configuration is zinc oxide (SnO x ); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 1:1.8; sputtering pressure is 3~5×10 -3 mbar; D. Magnetron sputtering fourth layer (4) Target quantity: 1 DC plane target; target configuration is silver (Ag); process gas ratio: pure argon; The sputtering pressure is 2~3×10 -3 mbar; E. Magnetron sputtering fifth layer (5) Target quantity: 1 AC rotating target; target configuration is titanium (Ti); process gas ratio: pure argon; The sputtering pressure is 2~3×10 -3 mbar; F. Magnetron sputtering sixth layer (6) Target quantity: 1 to 2 AC rotating targets; target configuration is zinc oxide (SnO x ); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 1:1.8; sputtering pressure is 2~3×10 -3 mbar; G. Magnetron sputtering seventh layer (7) Target quantity: 1 to 2 AC rotating targets; target configuration is zinc tin oxide (ZnSnO x ); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 1:1.8; sputtering pressure is 3~5×10 -3 mbar; H. Magnetron sputtering eighth layer (8) Target quantity: 2 to 4 AC rotating targets; target configuration is zinc oxide (SnO x ); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 1:1.8; sputtering pressure is 3~5×10 -3 mbar; I. Magnetron sputtering ninth layer (9) Target quantity: 1 DC plane target; target configuration is silver (Ag); process gas ratio: pure argon; The sputtering pressure is 2~3×10 -3 mbar; J. Magnetron sputtering tenth layer (10) Target quantity: 1 AC flat target; target configuration is titanium (Ti); process gas ratio: argon and oxygen, the ratio of argon and oxygen is 3:1; sputtering pressure is 2~3×10 -3 mbar; K. Magnetron sputtering eleventh layer (11) Target quantity: 1 to 2 AC plane targets; target configuration is zinc oxide (SnO x ); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 1:1.8; sputtering pressure is 3~5×10 -3 mbar; L. Magnetron sputtering twelfth layer (12) Target quantity: 2 to 4 AC rotating targets; the target material is zinc tin oxide (ZnSnO x ); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 1:1.8; sputtering pressure is 3~5×10 -3 mbar; M, magnetron sputtering thirteenth layer (13) Target quantity: 1 to 2 AC plane targets; target configuration is zinc oxide (SnO x ); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 1:1.8; sputtering pressure is 3~5×10 -3 mbar N. Magnetron sputtering thirteenth layer (14) Target quantity: 1 DC plane target; target configuration is silver (Ag); process gas ratio: pure argon; The sputtering pressure is 2~3×10 -3 mbar; O. Magnetron sputtering fifteenth layer (15) Target quantity: 1 AC flat target; target configuration is titanium (Ti); process gas ratio: argon and oxygen, the ratio of argon and oxygen is 3:1; sputtering pressure is 2~3×10 -3 mbar; P, magnetron sputtering sixteenth layer (16) Target quantity: 1 to 2 AC plane targets; target configuration is zinc oxide (SnO x ); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 1:1.8; sputtering pressure is 3~5×10 -3 mbar Q. Magnetron sputtering seventeenth layer (17) Target quantity: 2 to 4 AC rotating targets; the target material is zinc tin oxide (ZnSnO x ); Process gas ratio: argon and oxygen, the ratio of argon and oxygen is 1:1.8; sputtering pressure is 3~5×10 -3 mbar R, magnetron sputtering eighteenth layer (18) Target quantity: 1 to 2 AC plane targets; the target material is zirconium oxide (ZrO x ); Process gas ratio: argon and oxygen, the ratio of argon to oxygen is 20:1; The sputtering pressure is 3~5×10 -3 mbar 4) The total film thickness is controlled at 198-383 nm, and the transmission speed of the sputtering chamber is generally controlled at 3.0-6.0 m / min.

Citation Information

Patent Citations

  • Novel energy-saving toughened three-silver-layer low-radiation coated glass

    CN102350833A

  • Low radiation laminate

    JP2013133260A

  • Coated article with zinc oxide over IR reflecting layer and corresponding method

    US20050191501A1

  • Laminated glazing comprising a silver-based functional coating

    WO2024160764A1

Cited By

  • Tempering medium-low transmittance three-silver low-emissivity coated glass and preparation method thereof

    CN119874213A