Lightweight water-retaining material prepared from sludge incineration slag and preparation method of lightweight water-retaining material

Through alkali activation treatment and sintering, light-quality water-retaining ceramics are prepared from sludge incinerator slag, red mud, waste mud and other materials, solving the problem of low resource utilization efficiency of sludge incinerator slag, and achieving efficient resource utilization and environmental friendliness solid waste treatment.

CN118908604AActive Publication Date: 2024-11-08ZHANGZHOU ENVIRONMENT GRP CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410959386.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

There are still challenges in the efficient resource utilization of sludge incinerator slag. In traditional methods, the quality of sludge incinerator slag accounts for a low proportion, resulting in low disposal efficiency and landfill dominance, resulting in waste of land resources and environmental risks.

Method used

By alkali-activated treatment of sludge incinerator slag, red mud, waste mud and other materials, combined with pore-forming agent, light-quality water-retaining materials are prepared by sintering, which increases the mass proportion of sludge incinerator slag, and reduces the sintering temperature and increases Porosity and specific surface area form ceramic particles with high water absorption and mechanical strength.

Benefits of technology

It has achieved efficient resource utilization of sludge incinerator slag, reduced landfill demand, improved resource utilization, reduced solid waste emissions, high added value of products, and good water absorption and durability of ceramic granules.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908604A_ABST
    Figure CN118908604A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of sludge reutilization, and particularly discloses a lightweight water-retaining material prepared from sludge incineration slag and a preparation method of the lightweight water-retaining material. The preparation method of the light water-retaining material prepared from the sludge incineration slag comprises the following steps: respectively drying and grinding the sludge incineration slag, red mud, waste mud and a pore-forming agent, preparing an alkali activator with solutes of Na2SiO3 and NaOH, spraying the alkali activator onto the mixed powder, granulating to form particles, and drying the particles to obtain the light water-retaining material, namely the light water-retaining material prepared from the sludge incineration slag, the red mud, the waste mud and the pore-forming agent, the mass ratio of the sludge incineration slag reaches 40-60%, and the solute of the alkali activator is Na2SiO3 and NaOH. After drying, pre-calcining and roasting at a high temperature of 950-1100 DEG C, and cooling to obtain the light water-retaining material. According to the scheme, the sludge incineration slag serves as a main raw material, the red mud, the rice husks and the lakebed sludge serve as auxiliary materials, the red mud is added, the sintering temperature is reduced, meanwhile, the pore forming agent is added, the porosity is increased, the prepared finished product has the advantages of being light, porous, large in specific surface area and high in water absorption rate, and the purposes of light weight and water retention are achieved; the utilization rate of solid waste resources is increased; and the development of circular economy is promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of sludge heavy utilization, and specifically to a lightweight water-retaining material prepared from sludge incineration furnace slag and a preparation method thereof. Background Art

[0002] The rapidly increasing number of various types of urban sludge faces increasing pressure for treatment and disposal. Sludge incineration is one of the commonly used sludge disposal methods, which can effectively remove organic matter and harmful substances in it and greatly reduce the volume of sludge. However, the efficient disposal and comprehensive utilization of sludge incineration ash has become a new problem that needs to be solved urgently. Sludge incineration slag refers to the inorganic residue left after sludge is burned at high temperature. It is rich in elements such as silicon and aluminum. The sum of the content of SiO2 and Al2O3 can usually reach more than 70%. Sludge incineration slag is still mainly disposed of by landfill. In the context of tight land resources and greater environmental risks, the landfill space available in many cities is decreasing, and the resource utilization of zero landfill has become the research focus in the field of sludge incineration. The resource utilization of sludge incineration slag mainly includes phosphorus recovery, brick making, use as lightweight aggregate, concrete admixture and adsorbent, etc.

[0003] The patent application with publication number CN115322007A introduces a method for making expanded clay using sludge incineration slag, which comprises drying water-containing sludge, slag, clay, fly ash, iron oxide and zeolite to constant weight, crushing and sieving, adding water to mix until moist, extruding and forming, and then drying and calcining to obtain expanded clay. However, the raw materials thereof have clay as the material with the largest mass proportion, while the mass proportion of sludge incineration slag is not the highest and is only 20 to 32.6%. Therefore, the disposal efficiency of the sludge incineration slag is not high. Summary of the invention

[0004] This application aims to explore new ways to utilize sludge incineration slag as resources, so as to achieve harmless, reduced, stabilized and resourceful disposal of sludge incineration slag, utilize sludge incineration ash as resources, reduce landfill land, save land resources and reduce environmental risks. At the same time, by adding solid wastes such as red mud, rice husks and silt, effective utilization of resources is achieved, solid waste emissions are reduced, products have high added value, and high-value utilization of waste is achieved.

[0005] A method for preparing a lightweight water-retaining material from sludge incineration slag, the method comprising: Raw material pretreatment: Dry the sludge incineration slag, red mud, waste mud and pore-forming agent separately.

[0006] Grinding: Grind the dried sludge incineration slag, red mud, waste mud and pore-forming agent into powder respectively to obtain sludge incineration slag powder, red mud powder, waste mud powder and pore-forming agent powder.

[0007] Prepare alkaline activator: prepare a mixed aqueous solution of Na2SiO3 and NaOH as solute, and cool it to 5-50℃.

[0008] Granulation: According to the weight proportions, 50-60 parts of sludge incineration slag powder, 20-25 parts of red mud powder, 20-25 parts of waste mud powder and 10-15 parts of pore-forming agent powder are mixed for granulation. During the granulation process, the alkali activator is sprayed onto the mixed powder to form granules.

[0009] Aging: The granules were stored at room temperature for 12-36 hours.

[0010] Drying: Dry the aged particles.

[0011] Pre-calcination: Heat the dried particles to 300-400°C.

[0012] High temperature calcination: The calcination temperature is 950-1100℃ and the calcination time is 5-15min.

[0013] After calcination, the mixture is cooled to obtain the light water-retaining material.

[0014] The slag after sludge incineration contains a variety of inorganic minerals such as SiO2, Al2O3, Fe2O3, etc., which are similar to clay compositions. From the perspective of elemental composition, sludge incineration slag is suitable as a raw material for synthesizing lightweight water-retaining materials (which can be in the form of ceramsite). The sludge incineration slag is activated by alkali and then sintered to prepare lightweight water-retaining materials. This solution also uses red mud as an aluminum-rich material, which helps the formation of a glass phase during the sintering process of ceramics, thereby promoting the mass transfer of ceramsite, reducing the calcination temperature, saving energy, and solving the problem of alkaline substances polluting the environment due to the accumulation of red mud. By adding red mud, the sintering temperature is reduced, energy is saved, and the volatilization of heavy metals in the sludge incineration slag is reduced during the sintering process. At the same time, a pore-forming agent is added to increase the porosity, so that the prepared finished product has the advantages of light weight, porous, large specific surface area, and high water absorption, achieving the purpose of lightweight water retention. In the above technical scheme, the mass proportion of sludge incineration slag reaches 40-60%, and the efficiency of disposing sludge incineration slag is relatively high.

[0015] During the alkali activation process, the alkali activator reacts chemically with the silicon dioxide, metal oxides, and metal ions in the sludge incineration slag. For example, NaOH reacts with SiO2 to generate Na2SiO3, and NaOH reacts with Al2O3 to generate NaAlO2. NaOH also reacts with heavy metal ions, and the product is solidified in the reaction system. Na2SiO3 and Ca 2+ Mg 2+The metal ions react to generate CaSiO3 and MgSiO3, and Na2SiO3 reacts with heavy metal ions. The products are solidified in the reaction system. After the above reactions, the heavy metal elements in the slag will also be wrapped and fixed in the reaction system, reducing their potential harm to the environment and improving the safety of the lightweight water-retaining material. The activated slag has a higher specific surface area, a more uniform pore size distribution and better mechanical strength. The ceramsite produced by this can have good water absorption, hardness and durability. The bulk density of the ceramsite measured by the test is 400-500kg / cm 3 , cylinder pressure strength is 1.5-2.5MPa, and water absorption rate is 30-50%.

[0016] A preferred embodiment of the method for preparing a lightweight water-retaining material from sludge incineration furnace slag is that the waste sludge is one or more of lake bottom sludge, river bottom sludge and construction waste mud.

[0017] By adopting the above technical solution, these waste muds contain substances such as silicon dioxide and silicates, which can react with alkaline activators. This option provides a solution for the treatment of lake bottom sludge, river bottom sludge and construction waste mud, reduces solid waste emissions, has high added value of products, and realizes high-value utilization of waste.

[0018] A preferred embodiment of the method for preparing a lightweight water-retaining material from sludge incineration furnace slag is that the pore-forming agent is one or both of raw rice husk and carbonized rice husk.

[0019] By adopting the above technical solution, one or both of raw rice husk and carbonized rice husk are used as pore-forming agents to reduce the effect of red mud forming glass phase to block pores during the ceramic sintering process. The pore-forming agent increases the porosity, and the inorganic components in the rice husk, such as silicates, also participate in the formation process of ceramsite, which has a positive effect on the structure and performance of ceramsite. Among them, raw rice husk refers to the rice husk that has been removed from the rice grains and has not been chemically treated such as carbonization, and is generally yellow. Carbonized rice husk refers to the charred material formed by heating the raw rice husk to a temperature below its ignition point so that it is not fully burned.

[0020] A preferred solution of the method for preparing the lightweight water-retaining material from sludge incineration slag is that, in the alkaline activator, the mass concentration of Na2SiO3 is 60-75%, and the mass concentration of NaOH is 6-8%.

[0021] By adopting the above technical solution, high concentration of Na2SiO3 can be combined with Ca2+ in sludge incineration slag and waste sludge. 2 + Mg 2+And other heavy metal ions react to form water-insoluble silicates. Lower concentrations of NaOH can react with SiO2 and further react with other metal ions to form water-insoluble silicates. The above reaction products can encapsulate heavy metal elements. The alkaline activator of this concentration has high safety and properties suitable for vegetation planting after the reaction.

[0022] A preferred solution of the method for preparing the lightweight water-retaining material from sludge incineration slag is that during the granulation process, the alkali activator is sprayed onto the mixed powder, and granules are formed by rolling, and the moisture content of the granules is maintained at 18-20%, and finally granules with a diameter of 5-10 mm are formed.

[0023] By adopting the above technical scheme, the alkaline activator has high permeability to the powder, and can react with the sludge incineration slag, waste mud, red mud and the like in the powder to play a role in bonding the raw materials. By continuously spraying the alkaline activator and continuously rolling the pellets, the pellets gradually become larger, thereby achieving granulation.

[0024] A preferred embodiment of the method for preparing lightweight water-retaining material from sludge incineration slag is that the pre-calcination is specifically: preheating from 40-60°C, heating to 300-400°C at a heating rate of 8-12°C / min, and the preheating time is 15-25min.

[0025] By adopting the above technical solution, the pre-burning step of this parameter can remove moisture, remove harmful gases, decompose organic matter, improve the bonding force of each raw material, and fix the shape of the product.

[0026] On the second aspect, the present application also proposes a lightweight water-retaining material prepared from sludge incineration slag, and adopts the following technical solution.

[0027] A lightweight water-retaining material prepared from sludge incineration slag is prepared according to the above method.

[0028] By adopting the above technical solution, the prepared lightweight water-retaining material has the advantages of being light and porous, having a large specific surface area, and being able to absorb a large amount of water and nutrients.

[0029] A preferred lightweight water-retaining material prepared from the sludge incineration slag is ceramsite with a bulk density of 400-500 kg / cm 3 , cylinder pressure strength is 1.5-2.5MPa, and water absorption rate is 30-50%.

[0030] By adopting the above technical scheme, the lightweight water-retaining material is light and porous, with a high water absorption rate. It can be applied to flower nutrient soil to achieve high-value utilization of sludge incineration slag.

[0031] In summary, the present application proposes a method for preparing ceramsite using sludge incineration slag as the main raw material, red mud, rice husk and other pore-forming agents, sludge and other waste mud as auxiliary materials, and reducing environmental pollution and improving resource utilization through the coordinated disposal of multiple solid wastes. The physical and chemical properties of the slag can be changed by alkali activation treatment, and the prepared ceramsite usually has a higher porosity, a lower density and good air permeability. The addition of red mud helps the formation of a glass phase in the ceramic during the sintering process, thereby promoting the mass transfer of the ceramsite and reducing the sintering temperature during the calcining process. At the same time, the addition of red mud can reduce the volatility of heavy metals in the sludge incineration slag during the sintering process, making it have low leaching. However, the formation of the glass phase also has the effect of blocking pores, so rice husk is used as a pore-forming agent, and its organic substances burn to release a certain amount of heat and gas, forming holes of a certain size, increasing the porosity, and at the same time, inorganic components in the rice husk, such as silicates, will also participate in the formation process of ceramsite, which has a positive effect on the structure and performance of ceramsite.

[0032] Compared with the method of preparing expanded clay from sludge incineration slag in the related art, this method uses sludge incineration slag as the main raw material and red mud, rice husk and lake bottom sludge as auxiliary materials. The coordinated treatment of multiple solid wastes not only reduces the proportion of other natural materials and reduces production costs, but also has the advantages of environmental protection and sustainability, reduces waste emissions, improves the utilization rate of solid waste resources and promotes the development of a circular economy. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is the overall structural diagram of the lightweight water-retaining material prepared from the sludge incineration slag in Example 1.

[0034] Figure 2 This is a diagram of the internal pores of the lightweight water-retaining material prepared from the sludge incineration slag of Example 1. DETAILED DESCRIPTION

[0035] Example 1 A method for preparing a lightweight water-retaining material from sludge incineration slag, the method comprising: Raw material pretreatment: sludge incineration furnace slag, red mud, waste mud and pore-forming agent are dried at 105°C for 24 hours. The waste mud is lake bottom mud. The pore-forming agent is raw rice husk.

[0036] Grinding: Use a ball mill to grind the dried sludge incineration slag, red mud, waste mud and pore-forming agent for 50-60 minutes respectively, grind them into powder, and pass them through a 100-mesh sieve to obtain sludge incineration slag powder, red mud powder, waste mud powder and pore-forming agent powder.

[0037] Prepare the alkaline activator: weigh 70 parts of Na2SiO3 and 7 parts of NaOH by mass, add 23 parts of water and mix and dissolve. Since the dissolution of solid sodium hydroxide releases a large amount of heat, the alkaline activator is generally prepared 24 hours before the test and cooled to room temperature for use. The room temperature can be 5-50°C.

[0038] Granulation: According to the weight proportions, 55 parts of sludge incineration slag powder, 22 parts of red mud powder, 22 parts of waste mud powder and 12 parts of pore-forming agent powder are mixed and put into a disc granulator for granulation. During the granulation process, the configured alkali activator is sprayed onto the mixed powder through a spray pot, and the granules are formed by continuous disc rolling, and the moisture content of the granules is kept at about 18-20%, and finally spherical particles with a diameter of 5-10mm are formed.

[0039] Aging: The spherical particles were stored at room temperature for 24 hours for aging.

[0040] Drying: The aged granules were dried at 105°C to constant weight.

[0041] The subsequent sintering is carried out in a muffle furnace in two stages, namely pre-calcination and high temperature calcination, as described below.

[0042] Pre-calcination: In a muffle furnace, the dried particles were preheated from 50°C to 350°C at a heating rate of 10°C / min for 20 minutes.

[0043] High temperature calcination: the calcination temperature is 1030℃ and the calcination time is 10min.

[0044] After the sintering process is completed, the pellets are taken out of the muffle furnace and cooled to room temperature to obtain the lightweight water-retaining material. Figure 1 The lightweight water-retaining material is ceramsite, and the internal pore structure of the ceramsite is referenced Figure 2 , which has abundant pores.

[0045] Example 2 This embodiment prepares a lightweight water-retaining material from sludge incineration slag. The method used is basically the same as that in Example 1, except that the waste sludge in this embodiment is riverbed sludge, and the raw material ratio and process parameters are adjusted as follows.

[0046] A method for preparing a lightweight water-retaining material from sludge incineration slag, the method comprising: Raw material pretreatment: The sludge incineration sludge, red mud, waste mud and pore-forming agent were dried by baking at 105°C for 24 hours.

[0047] Grinding: Use a ball mill to grind the dried sludge incineration slag, red mud, waste mud and pore-forming agent for 50-60 minutes respectively, grind them into powder, and pass them through a 100-mesh sieve to obtain sludge incineration slag powder, red mud powder, waste mud powder and pore-forming agent powder.

[0048] Prepare the alkaline activator: weigh 60 parts of Na2SiO3 and 8 parts of NaOH by mass, add 32 parts of water and mix and dissolve. Since the dissolution of solid sodium hydroxide releases a large amount of heat, the alkaline activator is generally prepared 24 hours before the test and cooled to room temperature for use. The room temperature can be 5-50°C.

[0049] Granulation: According to the weight proportions, 60 parts of sludge incineration slag powder, 20 parts of red mud powder, 20 parts of waste mud powder and 10 parts of pore-forming agent powder are mixed and put into a disc granulator for granulation. During the granulation process, the configured alkali activator is sprayed onto the mixed powder through a spray pot, and the granules are formed by continuous disc rolling, and the moisture content of the granules is kept at about 18-20%, and finally spherical particles with a diameter of 5-10mm are formed.

[0050] Aging: The spherical particles were stored at room temperature for 24 hours for aging.

[0051] Drying: The aged granules were dried at 105°C to constant weight.

[0052] The subsequent sintering is carried out in a muffle furnace in two stages, namely pre-calcination and high temperature calcination, as described below.

[0053] Pre-calcination: In a muffle furnace, the dried particles were preheated from 50°C to 400°C at a heating rate of 10°C / min for 15 minutes.

[0054] High temperature calcination: the calcination temperature is 1100℃ and the calcination time is 5min.

[0055] After the sintering process is completed, the pellets are taken out from the muffle furnace and cooled to room temperature to obtain the lightweight water-retaining material, which is ceramsite.

[0056] Example 3 This embodiment prepares a lightweight water-retaining material from sludge incineration slag. The method used is basically the same as that in Example 1, except that the waste sludge in this embodiment is construction waste mud, the pore-forming agent is carbonized rice husk, and the raw material ratio and process parameters are adjusted as follows.

[0057] A method for preparing a lightweight water-retaining material from sludge incineration slag, the method comprising: Raw material pretreatment: The sludge incineration sludge, red mud, waste mud and pore-forming agent were dried by baking at 105°C for 24 hours.

[0058] Grinding: Use a ball mill to grind the dried sludge incineration slag, red mud, waste mud and pore-forming agent for 50-60 minutes respectively, grind them into powder, and pass them through a 100-mesh sieve to obtain sludge incineration slag powder, red mud powder, waste mud powder and pore-forming agent powder.

[0059] Prepare the alkaline activator: weigh 75 parts of Na2SiO3 and 6 parts of NaOH by mass, add 19 parts of water and mix and dissolve. Since the dissolution of solid sodium hydroxide releases a large amount of heat, the alkaline activator is generally prepared 24 hours before the test and cooled to room temperature for use. The room temperature can be 5-50°C.

[0060] Granulation: According to the weight proportions, 50 parts of sludge incineration slag powder, 25 parts of red mud powder, 25 parts of waste mud powder and 15 parts of pore-forming agent powder are mixed and put into a disc granulator for granulation. During the granulation process, the configured alkali activator is sprayed onto the mixed powder through a spray pot, and the granules are formed by continuous disc rolling, and the moisture content of the granules is kept at about 18-20%, and finally spherical particles with a diameter of 5-10mm are formed.

[0061] Aging: The spherical particles were stored at room temperature for 24 hours for aging.

[0062] Drying: The aged granules were dried at 105°C to constant weight.

[0063] The sintering is then carried out in a muffle furnace in two stages, namely pre-calcination and high temperature calcination, as described below.

[0064] Pre-calcination: In a muffle furnace, the dried particles were preheated from 50°C to 300°C at a heating rate of 10°C / min for 25 min.

[0065] High temperature calcination: the calcination temperature is 950℃ and the calcination time is 15min.

[0066] After the sintering process is completed, the pellets are taken out from the muffle furnace and cooled to room temperature to obtain the lightweight water-retaining material, which is ceramsite.

[0067] Comparative Example 1 This comparative example prepares a light water-retaining material from sludge incineration slag, and the method used is basically the same as that of Example 1, except that the raw material of this comparative example does not contain red mud, and waste mud of equal mass is used to replace red mud. The specific method for preparing the light water-retaining material in this comparative example is as follows.

[0068] A method for preparing a lightweight water-retaining material from sludge incineration slag, the method comprising: Raw material pretreatment: sludge incineration furnace slag, waste mud and pore-forming agent are dried at 105°C for 24 hours. The waste mud is lake bottom mud. The pore-forming agent is raw rice husk.

[0069] Grinding: Use a ball mill to grind the dried sludge incineration slag, waste mud and pore-forming agent for 50-60 minutes respectively, grind them into powder, and pass them through a 100-mesh sieve to obtain sludge incineration slag powder, waste mud powder and pore-forming agent powder.

[0070] Prepare the alkaline activator: weigh 70 parts of Na2SiO3 and 7 parts of NaOH by mass, add 23 parts of water and mix and dissolve. Since the dissolution of solid sodium hydroxide releases a large amount of heat, the alkaline activator is generally prepared 24 hours before the test and cooled to room temperature for use. The room temperature can be 5-50°C.

[0071] Granulation: According to the weight proportions, 55 parts of sludge incineration slag powder, 44 parts of waste mud powder and 12 parts of pore-forming agent powder are mixed and put into a disc granulator for granulation. During the granulation process, the configured alkali activator is sprayed onto the mixed powder through a spray pot, and the granules are formed by continuous disc rolling, and the moisture content of the granules is maintained at about 18-20%, and finally spherical particles with a diameter of 5-10mm are formed.

[0072] Aging: The spherical particles were stored at room temperature for 24 hours for aging.

[0073] Drying: The aged granules were dried at 105°C to constant weight.

[0074] The subsequent sintering is carried out in a muffle furnace in two stages, namely pre-calcination and high temperature calcination, as described below.

[0075] Pre-calcination: In a muffle furnace, the dried particles were preheated from 50°C to 350°C at a heating rate of 10°C / min for 20 minutes.

[0076] High temperature calcination: the calcination temperature is 1030℃ and the calcination time is 10min.

[0077] After the sintering process is completed, the pellets are taken out from the muffle furnace and cooled to room temperature to obtain the lightweight water-retaining material, which is ceramsite.

[0078] Comparative Example 2 This comparative example prepares a light water-retaining material from sludge incineration slag. The method used is basically the same as that in Example 1, except that the raw material of this comparative example does not contain a pore-forming agent, and the pore-forming agent is replaced by waste sludge of equal mass.

[0079] The specific method for preparing the lightweight water-retaining material in this comparative example is as follows.

[0080] A method for preparing a lightweight water-retaining material from sludge incineration slag, the method comprising: Raw material pretreatment: sludge incineration sludge, red mud and waste mud are dried at 105℃ for 24h. The waste mud is lake bottom mud.

[0081] Grinding: Use a ball mill to grind the dried sludge incineration slag, red mud and waste mud for 50-60 minutes respectively, grind them into powder, and pass them through a 100-mesh sieve to obtain sludge incineration slag powder, red mud powder and waste mud powder.

[0082] Prepare the alkaline activator: weigh 70 parts of Na2SiO3 and 7 parts of NaOH by mass, add 23 parts of water and mix and dissolve. Since the dissolution of solid sodium hydroxide releases a large amount of heat, the alkaline activator is generally prepared 24 hours before the test and cooled to room temperature for use. The room temperature can be 5-50°C.

[0083] Granulation: According to the weight proportions, 55 parts of sludge incineration slag powder, 22 parts of red mud powder and 34 parts of waste mud powder are mixed and put into a disc granulator for granulation. During the granulation process, the configured alkali activator is sprayed onto the mixed powder through a spray pot, and the granules are formed by continuous disc rolling, and the moisture content of the granules is maintained at about 18-20%, and finally spherical particles with a diameter of 5-10mm are formed.

[0084] Aging: The spherical particles were stored at room temperature for 24 hours for aging.

[0085] Drying: The aged granules were dried at 105°C to constant weight.

[0086] The sintering is then carried out in a muffle furnace in two stages, namely pre-calcination and high temperature calcination, as described below.

[0087] Pre-calcination: In a muffle furnace, the dried particles were preheated from 50°C to 350°C at a heating rate of 10°C / min for 20 minutes.

[0088] High temperature calcination: the calcination temperature is 1030℃ and the calcination time is 10min.

[0089] After the sintering process is completed, the pellets are taken out from the muffle furnace and cooled to room temperature to obtain the lightweight water-retaining material, which is ceramsite.

[0090] Test Example 1 Take the ceramsite prepared in Examples 1-3 and Comparative Examples 1-2, and test some of its properties as follows: Bulk density is 400-500kg / cm 3 , cylinder pressure strength is 1.5-2.5MPa, and water absorption rate is 30-50%.

[0091] Table 1 Test data of various ceramsite properties Combined with Table 1, the bulk density, cylinder pressure strength and water absorption rate of the expanded clay in Examples 1-3 are comparable, and all achieved good results, and are suitable as water-retaining materials for the roots of flowers.

[0092] Comparative Example 1 Compared with Example 1, the raw material of Comparative Example 1 does not contain red mud, but waste mud of equal mass is used to replace red mud. The bulk density of the ceramsite in Comparative Example 1 is equivalent to that in Example 1, the cylinder pressure strength is significantly reduced, and the water absorption rate is slightly increased. Overall, the ceramsite of Example 1 is light, has high water absorption rate, and has high mechanical strength. This is consistent with the statement that red mud contributes to the formation of the glass phase during the sintering process of ceramics, thereby promoting the mass transfer of ceramsite and improving the mechanical strength of ceramsite.

[0093] Comparative Example 2 Compared with Example 1, the raw material of Comparative Example 2 does not contain a pore-forming agent, but uses waste mud of equal mass to replace the pore-forming agent. The bulk density of the ceramsite of Comparative Example 2 increases, which is due to its few pores. The ceramsite of Comparative Example 2 is heavier, and in application, such as as a water-retaining material for flowers, the pressure on the roots of plants is relatively large, so it is limited. The cylinder pressure strength of the ceramsite of Comparative Example 2 is equivalent to the cylinder pressure strength of the ceramsite of Example 1, and both have good mechanical strength. The water absorption rate of the ceramsite of Comparative Example 2 is significantly lower than that of the ceramsite of Example 1, and in application, such as as a water-retaining material for flowers, it is subject to certain restrictions.

[0094] Summarize In order to improve the utilization rate of sludge incineration slag and reduce the pollution of the environment caused by the large-scale stacking of sludge incineration slag and red mud, this application proposes to prepare ceramsite with sludge incineration slag as the main raw material and red mud, rice husk and silt as auxiliary materials, so as to improve the resource utilization of solid waste and reduce production costs. This application solves the problems of high production cost and waste of mineral resources in preparing ceramsite from traditional non-renewable resources. At the same time, this application utilizes the interaction between sludge incineration slag and red mud, rice husk, silt, etc. through a scientific and reasonable design method, which is conducive to the comprehensive utilization of various solid waste materials, reduces production costs, reduces the waste of non-renewable mineral resources, and achieves the purpose of improving the resource utilization rate of solid waste and protecting the ecological environment. The ceramsite prepared using this solid waste can be applied to flower nutrient soil, so that solid waste can be utilized as a resource, which can not only solve the environmental pollution problem caused by solid waste landfill, but also create diversified ecological value.

[0095] The above are only some embodiments of the present application, and the protection scope of the present application is not limited to the above embodiments. For ordinary technicians in this technical field, some improvements and modifications without departing from the creative design of the present application should also fall within the protection scope of the present application.

Claims

1. A method for preparing a lightweight water-retaining material from sludge incineration slag, characterized in that: The method comprises: Raw material pretreatment: Dry the sludge incineration slag, red mud, waste mud and pore-forming agent separately; Grinding: Grinding the dried sludge incineration slag, red mud, waste mud and pore-forming agent into powders respectively to obtain sludge incineration slag powder, red mud powder, waste mud powder and pore-forming agent powder; Prepare alkaline activator: prepare a mixed aqueous solution of Na2SiO3 and NaOH as solute, and cool it to 5~50℃; Granulation: 50-60 parts of sludge incineration slag powder, 20-25 parts of red mud powder, 20-25 parts of waste mud powder and 10-15 parts of pore-forming agent powder are mixed according to the weight proportions for granulation. During the granulation process, the alkali activator is sprayed onto the mixed powder to form granules. Aging: storing the particles at room temperature for 12-36 hours; Drying: Dry the aged particles; Pre-calcination: heating the dried particles to 300-400°C; High temperature calcination: the calcination temperature is 950-1100℃ and the calcination time is 5-15min; After calcination, the mixture is cooled to obtain the light water-retaining material.

2. The method for preparing a lightweight water-retaining material from sludge incineration slag according to claim 1, characterized in that: The waste mud is one or more of lake bottom mud, river bottom mud and construction waste mud.

3. The method for preparing a lightweight water-retaining material from sludge incineration slag according to claim 1, characterized in that: The pore-forming agent is one or both of raw rice husk and carbonized rice husk.

4. The method for preparing a lightweight water-retaining material from sludge incineration slag according to claim 1, characterized in that: Among the alkaline activators, the mass concentration of Na2SiO3 is 60-75%, and the mass concentration of NaOH is 6-8%.

5. The method for preparing a lightweight water-retaining material from sludge incineration slag according to claim 1, characterized in that: During the granulation process, the alkali activator is sprayed onto the mixed powder, and granules are formed by rolling, and the moisture content of the granules is maintained at 18-20%, and finally granules with a diameter of 5-10 mm are formed.

6. The method for preparing a lightweight water-retaining material from sludge incineration slag according to claim 1, characterized in that: The pre-calcination is specifically as follows: preheating starts from 40-60°C, heating to 300-400°C at a heating rate of 8-12°C / min, and the preheating time is 15-25min.

7. A lightweight water-retaining material prepared from sludge incineration slag, characterized in that: Prepared according to the method according to any one of claims 1 to 6.

8. The lightweight water-retaining material prepared from sludge incineration slag according to claim 7, characterized in that: The lightweight water-retaining material is ceramsite, and its bulk density is 400-500kg / cm 3 , cylinder pressure strength is 1.5-2.5MPa, and water absorption rate is 30-50%.

Citation Information

Patent Citations

  • Ceramsites prepared from solid wastes and preparation method and application of ceramsites

    CN107721455A

  • Geopolymer concrete based on household garbage incinerator slag and red mud and preparation method thereof

    CN111747696A

  • Method for preparing ceramsite from incineration disposal residues and oil-containing industrial sludge

    CN112876276A

  • Building ceramsite prepared from fly ash, sludge and slag and preparation process of building ceramsite

    CN113880477A

  • Ceramsite fired by fly ash as well as preparation method and application of ceramsite

    CN114292124A