Modified attapulgite, river bank ecological base material and preparation methods of modified attapulgite and river bank ecological base material

Through the combination of modified concave and concave rock stone and zeolite composite materials, the problem of insufficient corrosion resistance and adsorption of ecological substrates is solved, and more efficient pollutant purification and improved river bank slope protection stability are achieved.

CN118908612AActive Publication Date: 2024-11-08HUBEI UNIV OF TECH
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410953131.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

The existing ecological substrates have shortcomings in corrosion resistance and adsorption, and it is difficult to effectively slow down river bank erosion and reduce surface source pollution.

Method used

The modified concave and concave rock stone and zeolite composite material are used to modify concave rock stone and biochar through hydrothermal iron to enhance the fertilizer and water retention properties of the substrate, and the adsorption capacity is improved through the zeolite-based composite material.

Benefits of technology

It significantly improves the adsorption and retention capabilities of the substrate, enhances the purification effect of pollutants, and improves the stability and erosion resistance of river bank slope protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908612A_ABST
    Figure CN118908612A_ABST
Patent Text Reader

Abstract

The invention discloses modified attapulgite, a river bank ecological base material and a preparation method thereof. The preparation method of the modified attapulgite comprises the following steps: taking charcoal and potassium hydroxide, adding water, stirring, performing suction filtration, drying and grinding a product, and sieving to obtain powder; mixing the powder with attapulgite powder, carrying out pyrolytic reaction in a protective gas atmosphere, and washing a product until the pH value is 6.5-7.0 after the reaction is ended, so as to obtain attapulgite-based biochar; the preparation method comprises the following steps: adding a ferric chloride solution and a thiourea solution into attapulgite-based biochar, stirring, drying, calcining the product in a protective gas atmosphere, mixing with water, adjusting the pH value of the system to 6.5-7.5, standing, and finally washing and drying. The modified attapulgite prepared by the invention has a unique layered chain structure and rod-like crystals, can play roles of adsorption, complexation and ion exchange on pollutants in the environment, and has relatively strong capability of adsorbing and immobilizing nitrogen and phosphorus in soil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of slope erosion prevention, pollution control and ecological restoration, and in particular relates to a modified attapulgite, a riverbank ecological substrate and a preparation method thereof. Background Art

[0002] With the rapid development of economy and society, human demand for natural resources is growing. However, this growth is accompanied by serious disturbance and damage to the ecological environment. Due to the increasing frequency of human activities, the riverbank and water environment have suffered serious pollution, especially agricultural activities, industrial emissions and urbanization, which have brought unprecedented pollution pressure to these environments. These activities not only deteriorate the ecological environment, but also affect water quality and flood control capabilities, posing a threat to the health of aquatic ecosystems. Therefore, ecological protection technology has emerged. Ecological revetment is an important part of the river ecosystem. It not only enhances the landscape value of the river bank, but also enhances the stability and anti-erosion ability of the bank slope. More importantly, ecological revetment has a significant effect in intercepting and purifying non-point source pollution. The control mechanism of river ecological revetment on pollutants is mainly through vegetation interception of particulate matter and its attached pollutants in surface runoff, absorption by vegetation roots, adsorption of pollutants by soil, and transformation and degradation of pollutants by soil microorganisms.

[0003] Ecological substrate refers to a composite material formed by a mixture of soil, cementitious materials, coarse aggregate, organic matter and plant seeds. It has the characteristics of strong durability, stable structure and good permeability. At the same time, it provides a suitable environment for plant growth. Its developed root system continues to grow along the internal pores of the substrate until deep into the slope, connecting the ecological substrate and the slope into a whole, which has the function of improving the stability of the slope, purifying water bodies and improving the ecosystem.

[0004] At present, the research on ecological substrates is still in its early stages, mainly focusing on standardizing the mix design of ecological substrates, preparation processes, balancing the mechanical properties of ecological substrates and vegetation needs, while there is less research on the corrosion resistance and adsorption of ecological substrates. Therefore, it is crucial to further improve the adsorption and corrosion resistance of improved ecological substrates, effectively slow down riverbank erosion, and reduce non-point source pollution. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention aims to provide a modified attapulgite, a riverbank ecological substrate and a preparation method thereof. The modified attapulgite and zeolite composite material are used to prepare an ecological substrate, which has the effects of reducing soil density, increasing soil porosity, and improving soil consistency, and enhancing the fertilizer and water retention performance of the ecological slope protection substrate.

[0006] The purpose of the present invention is achieved through the following technical solutions: A method for preparing modified attapulgite comprises the following steps: (1) Take biochar and potassium hydroxide, add water and stir, then filter, and the product is dried, ground and sieved in sequence to obtain powder; KOH mainly plays an activation role, reacting with the active oxygen-containing substances in the biochar. KOH is completely converted into K2CO3, resulting in the formation of a large amount of gaseous products and phenols, increasing the oxygen content and specific surface area in the biochar.

[0007] (2) mixing the powder from step (1) with attapulgite powder, performing a pyrolysis reaction under a protective gas atmosphere, and washing the product after the reaction to a pH of 6.5-7.0 to obtain attapulgite-based biochar; (3) Add ferric chloride solution and thiourea solution to the attapulgite-based biochar, then ultrasonically stir and dry, calcine the product in a protective gas atmosphere, mix it with water, adjust the pH of the system to 6.5-7.5 and let it stand, finally wash and dry, and thus obtain modified attapulgite, i.e., hydrothermal iron-modified attapulgite.

[0008] In step (3), thiourea and ferric chloride have a synergistic activation effect.

[0009] Preferably, in step (1), the mass ratio of biochar to potassium hydroxide is 1:3.

[0010] Preferably, in step (1), the mass ratio of the added amount of water to the KOH is 5:3. Preferably, in step (1), the drying temperature is 80°C.

[0011] Preferably, in step (1), the pore size of the sieve is 0.42 mm.

[0012] Preferably, in step (1), the biochar is prepared by the following method: at least one of rape straw, potato, corn straw, coconut shell, walnut shell and chestnut shell is pyrolyzed at high temperature; the biochar particle size is 200-400 mesh.

[0013] Preferably, in step (2), the attapulgite powder is passed through a sieve with a pore size of 0.42 mm before use.

[0014] Preferably, in step (2), the mass ratio of the attapulgite powder to the powder of step (1) is 1:1-2.

[0015] Preferably, in step (2), the protective gas is nitrogen.

[0016] Preferably, in step (2), the temperature of the pyrolysis reaction is 450-550°C, and the pyrolysis time is 1 hour. More preferably, the temperature of the pyrolysis reaction is 500°C.

[0017] Preferably, in step (2), deionized water is used for washing.

[0018] Preferably, in step (3), the mass ratio of attapulgite-based biochar to ferric chloride solution is 1.6-2:5.

[0019] Preferably, in step (3), the mass ratio of attapulgite-based biochar to thiourea solution is 1-2:5.

[0020] Preferably, in step (3), the concentration of the ferric chloride solution is 2 mol·L -1 .

[0021] Preferably, in step (3), the concentration of the thiourea solution is 1 mol·L -1 .

[0022] Preferably, in step (3), the temperature of ultrasonic stirring is 80°C.

[0023] Preferably, in step (3), the drying temperature is 105°C.

[0024] Preferably, in step (3), the protective gas is nitrogen.

[0025] Preferably, in step (3), the calcination temperature is 700° C. and the calcination time is 2 h.

[0026] Preferably, in step (3), the pH of the system is adjusted by adding NaOH solution.

[0027] Preferably, in step (3), the standing time is 24 hours.

[0028] Preferably, in step (3), the drying temperature is 50-70°C.

[0029] The modified attapulgite is prepared by the above-mentioned preparation method of modified attapulgite.

[0030] A riverbank ecological substrate is prepared from the following components in parts by mass: 100-120 parts of planting soil, 3-6 parts of the modified attapulgite, 1-3 parts of zeolite-based composite materials, 0-3 parts of biochar, 1-3 parts of cement, 1-2 parts of greening additives and 5-10 parts of organic materials.

[0031] Preferably, the zeolite-based composite material is prepared according to the following preparation method: zeolite and attapulgite are ground, mixed after passing through a 2 mm aperture sieve, added with cement and a foaming agent to form a blank, and cured in a steam box for 24 hours, wherein the mass ratio of zeolite, cement and attapulgite is 5~10:1~3:1~3.

[0032] Zeolite-based composite materials have the characteristics of large specific surface area, rich pores, multiple adsorption sites, and good ion exchange performance. + -N works well.

[0033] Preferably, the foaming agent is a carbonate, and more preferably, the carbonate is at least one of calcium carbonate, magnesium carbonate and sodium bicarbonate. The foaming agent can adjust the porosity and pore size of the material, effectively reduce the surface tension of the liquid, and increase the surface activity of the target material.

[0034] Preferably, the amount of the foaming agent added is 0.10% to 0.15% of the total mass of the zeolite, cement and attapulgite.

[0035] Preferably, the curing environment temperature is 60°C and the humidity is 90%.

[0036] Preferably, the preparation method of biochar is as follows: at least one of rape straw, potato, corn straw, coconut shell, walnut shell and chestnut shell is cracked at high temperature to obtain the biochar; the particle size of the biochar is 200-400 mesh.

[0037] Preferably, the cement is PO 42.5 grade ordinary Portland cement.

[0038] Preferably, the greening additive is ferrous sulfate, which adjusts the alkaline environment produced by cement hydration without significantly affecting the strength of the substrate, making it suitable for the survival and reproduction of plants and functional microorganisms.

[0039] Preferably, the organic material is soybean powder particles with a particle size of 2 mm, and the main components are soybean powder, corn powder, fish bone powder, and traditional Chinese medicine residues.

[0040] The preparation method of the above-mentioned riverbank ecological substrate includes the following steps: drying, crushing, and sieving the planting soil to remove coarse particles; weighing modified attapulgite, biochar, zeolite-based composite materials, cement and greening additives according to proportion, adding water and mixing them evenly with the planting soil to obtain an initial improved material; and finally adding organic materials.

[0041] Preferably, the amount of water added is determined according to actual conditions, and the moisture content of the riverbank ecological substrate after adding water is 15-20%.

[0042] Compared with the prior art, the beneficial effects of the present invention include: (1) The hydrothermal iron-modified attapulgite of the present invention has a unique layered chain structure and rod-shaped crystals, which can play a role in adsorption, complexation and ion exchange of pollutants in the environment. It is composed of a large amount of SiO2 and Al2O3 minerals, which can undergo secondary hydration reaction with Ca(OH)2 produced by cement hydration in the ecological slope protection substrate to generate hydrated calcium silicate with a low Ca / Si ratio, hydrated calcium silicate (CSH) and hydrated calcium aluminate (CAH), which can produce secondary reinforcement on the substrate and improve the bonding strength of the substrate; at the same time, it can also improve the reactivity of attapulgite and neutralize the adverse effects of cement alkalinity on vegetation growth.

[0043] The present invention makes the attapulgite evenly dispersed on the surface of the biochar through thermal co-lysis with the biochar, so as to form a composite material with higher anion exchange capacity and stronger ability to adsorb and fix nitrogen and phosphorus in the soil.

[0044] (2) The particle size of the biochar of the present invention is between 200 and 400 meshes, which can increase the maximum adsorption of phosphorus by the soil and reduce the phosphorus desorption rate of the soil. It has a strong filling effect, can enhance the agglomeration effect of the ecological slope protection substrate, and has the advantages of large specific surface area, rich pore structure and strong ion adsorption and exchange capacity. Biochar is considered to be a potential soil conditioner, which has the effects of reducing soil density, increasing soil porosity, improving soil consistency, and enhancing the fertilizer and water retention properties of the ecological slope protection substrate.

[0045] (3) The zeolite-based composite material of the present invention further improves the adsorption capacity, porosity and specific surface area of ​​zeolite, making it have excellent adsorption of NH4 + -N performance, and has low cost, wide distribution, non-toxicity and good ion exchange performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 The present invention is a statistical curve chart of the planting days and germination rate of Bermuda grass planted using the riverbank ecological substrate prepared in various embodiments and comparative examples.

[0047] Figure 2 It is a statistical chart of the total nitrogen adsorption efficiency of sewage by the riverbank ecological substrate prepared in each embodiment and comparative example, wherein 0%, 1%, 2%, 3% and 4% correspond to different proportions of biochar content, respectively.

[0048] Figure 3 It is a statistical chart of the total phosphorus adsorption efficiency of the riverbank ecological substrate prepared in each embodiment and comparative example for sewage, wherein 0%, 1%, 2%, 3% and 4% correspond to different proportions of biochar content, respectively.

[0049] Figure 4 This is the total nitrogen adsorption kinetic curve of substrate No. 4, substrate No. 14 and substrate No. 15.

[0050] Figure 5 This is the total phosphorus adsorption kinetic curve of substrate No. 4, substrate No. 14 and substrate No. 15. DETAILED DESCRIPTION

[0051] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0052] The zeolite described in the embodiment is chlorite, which was purchased from Lingshou County Huibang Mineral Products Co., Ltd.; The attapulgite was purchased from Lingshou County Chengnuo Mineral Products Co., Ltd.; the biochar was purchased from Henan Coconut Carbon Environmental Protection Materials Co., Ltd.; and the cement was PO 42.5 grade ordinary Portland cement.

[0053] The planting soil was selected from the southern area experimental soil of the Key Laboratory of Intelligent Perception of River and Lake Health and Ecological Restoration of the Ministry of Education in Wuhan, Hubei Province; the greening additive was ferrous sulfate; and the organic material was soybean powder, which was purchased from Tianbao Bioengineering Co., Ltd.

[0054] The modified attapulgite described in the examples and comparative examples is prepared according to the following steps: (1) Take biochar and potassium hydroxide, add water and ultrasonically stir for 1 h (mass ratio of biochar: potassium hydroxide: water = 1:3:5), then filter, dry and grind the product, and pass it through a 0.42 mm pore size sieve to obtain a powder; (2) 5 g of the powder prepared in step (1) was mixed with 5 g of attapulgite powder (previously sieved with a 0.42 mm pore size) and incubated at 10 °C min-1 under a nitrogen atmosphere. -1 The temperature was raised to 500°C at a heating rate of 100°C for 1 hour of pyrolysis reaction. After the reaction, the product was washed with deionized water to a pH of 6.5-7.0 to obtain attapulgite-based biochar. (3) Add 10 g of ferric chloride solution to 4 g of attapulgite biochar (attapulgite biochar: ferric chloride solution = 2:5, actually introduced by FeCl3·6H2O, the concentration of ferric chloride solution is 2 mol·L -1 ) and 20g thiourea solution (concentration 1mol·L -1 ), then ultrasonically stirred at 80°C and dried at 105°C, the product was calcined in a nitrogen atmosphere at 700°C for 2h. Then mixed with water and treated with NaOH solution (concentration 2mol·L -1 ) adjust the pH of the system to 6.5-7.5 and let it stand for 24 hours, and finally wash it with deionized water for multiple times and dry it (drying temperature is 60°C, time is 12 hours), so as to prepare the modified attapulgite, that is, hydrothermal iron-modified attapulgite.

[0055] The zeolite-based composite material of the embodiments and comparative examples is prepared according to the following method: grinding green zeolite and attapulgite, mixing after passing through a 2 mm aperture sieve, adding cement (PO 42.5 grade ordinary Portland cement) and a foaming agent to form a blank, and curing in a steam box for 24 hours, wherein the mass ratio of zeolite to attapulgite is 4:6, the cement is 10% of the total mass of zeolite, cement and attapulgite, and the foaming agent is sodium bicarbonate, and the addition amount accounts for 0.10% of the total mass of zeolite, cement and attapulgite.

[0056] Example 1 A riverbank ecological substrate is prepared from the following components in parts by mass: 100 parts of planting soil, 3 parts of the above-mentioned modified attapulgite, 1 part of a zeolite-based composite material, 0 parts of biochar, 3 parts of cement, 1.5 parts of greening additives and 7 parts of organic materials.

[0057] The riverbank ecological substrate is prepared according to the following method: the planting soil is dried, crushed, sieved, and coarse particles are removed; modified attapulgite, zeolite-based composite materials, cement, and greening additives are weighed in proportion, water is added (water is added until the moisture content of the prepared riverbank ecological substrate is 15-20%), and the planting soil is mixed evenly to obtain an initial improved material, and finally organic materials are added.

[0058] Example 2 A riverbank ecological substrate is prepared from the following components in parts by mass: 100 parts of planting soil, 3 parts of the above-mentioned modified attapulgite, 1 part of a zeolite-based composite material, 2 parts of biochar, 3 parts of cement, 1.5 parts of greening additives and 7 parts of organic materials.

[0059] The riverbank ecological substrate is prepared according to the following method: the planting soil is dried, crushed, and sieved to remove coarse particles; modified attapulgite, biochar, zeolite-based composite materials, cement and greening additives are weighed according to proportion, water is added (water is added until the moisture content of the prepared riverbank ecological substrate is 15-20%) and mixed evenly with the planting soil to obtain an initial improvement, and finally organic materials are added.

[0060] Example 3 A riverbank ecological substrate is prepared from the following components in parts by mass: 100 parts of planting soil, 5 parts of the above-mentioned modified attapulgite, 1 part of a zeolite-based composite material, 2 parts of biochar, 3 parts of cement, 1.5 parts of greening additives and 7 parts of organic materials.

[0061] The riverbank ecological substrate was prepared according to the method described in Example 2.

[0062] Comparative Example 1 Planting soil is used as the ecological base material.

[0063] Comparative Example 2 This comparative example provides a riverbank ecological substrate, which is based on Example 1, except that the modified attapulgite is omitted and other raw materials remain unchanged. The preparation method of the riverbank ecological substrate is as described in Example 1.

[0064] Comparative Example 3 This comparative example provides a riverbank ecological substrate, based on Example 1, only the amount of modified attapulgite is changed to "1 part", and other raw materials remain unchanged. The preparation method of the riverbank ecological substrate is as shown in Example 1.

[0065] Comparative Example 4 This comparative example provides a riverbank ecological substrate, based on Example 1, only the number of modified attapulgite is changed to "5 parts", and other raw materials remain unchanged. The preparation method of the riverbank ecological substrate is as shown in Example 1.

[0066] Comparative Example 5 This comparative example provides a riverbank ecological substrate, based on Example 1, only the number of modified attapulgite is changed to "7 parts", and other raw materials remain unchanged. The preparation method of the riverbank ecological substrate is as shown in Example 1.

[0067] Comparative Examples 6-10 A riverbank ecological substrate is prepared from the following components in parts by mass: 100 parts of planting soil, the modified attapulgite, 1 part of zeolite-based composite material, 1 part of biochar, 3 parts of cement, 1.5 parts of greening additives and 7 parts of organic materials. Among them, the modified attapulgite is used in 0, 1, 3, 5 and 7 parts respectively, corresponding to Comparative Example 6, Comparative Example 7, Comparative Example 8, Comparative Example 9 and Comparative Example 10 respectively.

[0068] The riverbank ecological substrate was prepared according to the method described in Example 1.

[0069] Comparative Example 11 This comparative example provides a riverbank ecological substrate, which is based on Example 2, except that the modified attapulgite is omitted and other raw materials remain unchanged. The preparation method of the riverbank ecological substrate is as shown in Example 2.

[0070] Comparative Example 12 This comparative example provides a riverbank ecological substrate, based on Example 2, only the amount of modified attapulgite is changed to "1 part", and other raw materials remain unchanged. The preparation method of the riverbank ecological substrate is as shown in Example 2.

[0071] Comparative Example 13 This comparative example provides a riverbank ecological substrate, based on Example 2, only the number of modified attapulgite is changed to "7 parts", and other raw materials remain unchanged. The preparation method of the riverbank ecological substrate is as shown in Example 2.

[0072] Comparative Examples 14-18 A riverbank ecological substrate is prepared from the following components in parts by mass: 100 parts of planting soil, the modified attapulgite, 1 part of zeolite-based composite material, 3 parts of biochar, 3 parts of cement, 1.5 parts of greening additives and 7 parts of organic materials. Among them, the modified attapulgite is used in 0, 1, 3, 5 and 7 parts, which correspond to Comparative Example 14, Comparative Example 15, Comparative Example 16, Comparative Example 17 and Comparative Example 18 respectively.

[0073] The riverbank ecological substrate was prepared according to the method described in Example 1.

[0074] Comparative Examples 19-23 A riverbank ecological substrate is prepared from the following components in parts by mass: 100 parts of planting soil, the modified attapulgite, 1 part of zeolite-based composite material, 4 parts of biochar, 3 parts of cement, 1.5 parts of greening additives and 7 parts of organic materials. Among them, the modified attapulgite is used in 0, 1, 3, 5 and 7 parts respectively, corresponding to Comparative Example 19, Comparative Example 20, Comparative Example 21, Comparative Example 22 and Comparative Example 23.

[0075] The riverbank ecological substrate was prepared according to the method described in Example 1.

[0076] The effects of various prepared ecological substrates on plant growth were evaluated. The specific steps were as follows: 1500 Bermudagrass seeds (20 g / m 2 ), water regularly after sowing, observe the vegetation growth status every day in the first 20 days, keep the soil moist, record the germination rate of vegetation samples every day in the first 20 days, and continuously observe and record the average plant height of the samples every 5 days.

[0077]

[0078]

[0079] Figure 1 The following is a statistical curve of the planting days and germination rate of Bermuda grass planted on the riverbank ecological substrate prepared in each embodiment and comparative example. Figure 1 It can be seen that at different stages of the experiment, the addition amount of modified attapulgite and biochar showed different trends and effects on seed germination. The germination details are shown in Table 1.

[0080] See also Figure 1 In the early stage of germination (days 1 to 4), it was observed that the effects of modified attapulgite and biochar in different ratios on the germination of Cynodon dactylon seeds were relatively small. During this period, the germination rate differences among the groups were not significant, and the overall performance of seed germination was relatively balanced. Entering the middle stage (days 5 to 15), it is a critical period for rapid seed germination. At this stage, the effects of different ratios of ecological substrates on seed germination rate became very obvious, and the improvement of modified attapulgite and biochar had an inhibitory effect on seed germination. In the late stage (after the 16th day), the number of seed germination observed was small, and the germination process basically stopped.

[0081] Specifically, when the proportion of modified attapulgite (i.e. the ratio of modified attapulgite to planting soil) is greater than 5% and the proportion of biochar (i.e. the ratio of biochar to planting soil) is greater than 2%, the addition of modified attapulgite and biochar has a significant inhibitory effect on seed germination. This may be because modified attapulgite and biochar increase the soil pH. When the soil is alkaline, it may inhibit the enzyme activity of the seeds, affect the seeds' absorption of water and nutrients, and thus inhibit germination.

[0082] As an important component of ecological bank protection, plants are very important for the anti-erosion ability of bank slope soil. Plant roots can greatly improve the ability of bank slope to fix soil and sand, thereby reducing soil erosion. The plant growth experiment of the river bank ecological substrate prepared in Examples 1 to 3 proved that the substrate can provide a better environment for plant growth, and therefore, the river bank ecological substrate has excellent anti-erosion performance.

[0083] Figure 2 The statistical diagram of the total nitrogen adsorption efficiency of the riverbank ecological substrate prepared in each embodiment and comparative example on sewage, wherein 0%, 1%, 2%, 3% and 4% correspond to different proportions of biochar content, and the nitrogen content of sewage is 1 mg / L. The substrate corresponding to comparative example 1 is not counted here, so there are 25 groups of samples in total. The specific operation of the statistics is: the total nitrogen is determined according to the National Environmental Protection Standard of the People's Republic of China HJ 636-2012 "Determination of Total Nitrogen in Water Quality by Alkaline Potassium Persulfate Digestion Ultraviolet Spectrophotometry".

[0084] from Figure 2 It can be seen that different matrix combinations have different adsorption effects on nitrogen. The matrix combinations with nitrogen adsorption efficiency exceeding 80% are 8# (1% modified attapulgite + 1% biochar), 9# (3% modified attapulgite + 1% biochar), 10# (5% modified attapulgite + 1% biochar), 11# (7% modified attapulgite + 1% biochar), 13# (1% modified attapulgite + 2% biochar), 14# (3% modified attapulgite + 2% biochar), 15# (5% modified attapulgite + 2% biochar), 19# (3% modified attapulgite + 3% biochar, among which 15# has the best adsorption efficiency for nitrogen.

[0085] Figure 3 The statistical graph of the total phosphorus adsorption efficiency of the riverbank ecological substrate prepared in each embodiment and comparative example on sewage, wherein 0%, 1%, 2%, 3% and 4% correspond to different proportions of biochar content, and the phosphorus content of sewage is 1 mg / L. The substrate corresponding to comparative example 1 is not counted here, so there are 25 groups of samples in total. The specific operation of the statistics is: the total phosphorus is determined in accordance with the National Environmental Protection Standard of the People's Republic of China GB 11893-89 "Determination of Total Phosphorus in Water Quality by Platinum Acid Spectrophotometry").

[0086] from Figure 3 It can be seen that different matrix combinations have different adsorption effects on phosphorus. The matrix combinations with phosphorus adsorption efficiency exceeding 85% are 4# (3% modified attapulgite + 0% biochar), 10# (9% modified attapulgite + 1% biochar), 8# (1% modified attapulgite + 1% biochar), 9# (3% modified attapulgite + 1% biochar), 11# (7% modified attapulgite + 1% biochar), 12# (0% modified attapulgite + 2% biochar), 13# (1% modified attapulgite + 2% biochar), 14# (3% modified attapulgite + 2% biochar), 17# (0% modified attapulgite + 3% biochar), 18# (1% modified attapulgite + 3% biochar), and 22# (0% modified attapulgite + 4% biochar), among which 14# has the best adsorption efficiency for phosphorus.

[0087] Figure 4 The total nitrogen adsorption kinetic curves of substrate No. 4, substrate No. 14 and substrate No. 15 are as follows: Use an electronic balance to accurately weigh 1g of combined substrates with different ratios, for a total of 3 mass ratios. Set up 3 parallel samples for each substrate, put them into a 100mL centrifuge tube, add 50mL of 5mg / L NH4Cl solution, cover with a lid and place on a shaker, oscillate continuously at 150r / min and 25°C, and set the oscillation times to 0.5h, 1h, 2h, 3h, 5h, 7h, 9h, 12h and 24h, respectively. After the oscillation is completed, take out the centrifuge tube, and use HJ 636-2012 "Determination of total nitrogen in water quality - alkaline potassium persulfate digestion ultraviolet spectrophotometry" to measure the total nitrogen concentration of the solution. Figure 4 It can be seen that the adsorption process is mainly divided into three stages. In the early stage (0-5 hours), the adsorption rate of TN (total nitrogen) by all substrates is fast, and the adsorption amount increases significantly with time; in the middle stage (5-12 hours), the adsorption rate decreases; in the late stage (12-24 hours), the slope of the adsorption kinetic curve drops to the minimum, indicating that the adsorption rate slows down further. After 24 hours, the adsorption amount of TN by substrates with different ratios shows the rule of 14#>15#>4#.

[0088] Figure 5The total phosphorus absorption kinetic curves of substrate No. 4, substrate No. 14 and substrate No. 15. The specific operation is: use an electronic balance to accurately weigh 1g of combined substrates with different ratios, a total of 3 mass ratios, set up 3 parallel samples for each substrate, put them into 100mL centrifuge tubes, add 50ml of 5mg / L KH2PO4 solution respectively, cover with a lid and put on a shaker, oscillate continuously under the operating conditions of 150r / min and 25℃, and set the oscillation time to 0.5h, 1h, 2h, 3h, 5h, 7h, 9h, 12h and 24h respectively. After the oscillation is completed, take out the centrifuge tube and use GB 11893-89 "Determination of total phosphorus in water quality - Platinum acid spectrophotometry" to measure the total phosphorus concentration of the solution. From Figure 5 It can be seen that the adsorption process is mainly divided into three stages. In the early stage (0-5 hours), the adsorption rate of TP (total phosphorus) by all substrates is fast, and the adsorption amount increases significantly with the extension of time; in the middle stage (5-12 hours), the adsorption rate decreases; in the late stage (12-24 hours), the slope of the adsorption kinetic curve drops to the minimum, indicating that the adsorption rate slows down further. After 24 hours, the adsorption amount of TP by different ratios of substrates shows the rule of 15#>14#>4#.

[0089] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing modified attapulgite, characterized in that: The steps include: (1) Take biochar and potassium hydroxide, add water, stir and filter, dry, grind and sieve the product to obtain powder; (2) mixing the powder with attapulgite powder, performing a pyrolysis reaction under a protective gas atmosphere, and washing the product to a pH of 6.5 to 7.0 after the reaction to obtain attapulgite-based biochar; (3) Adding ferric chloride solution and thiourea solution to the attapulgite-based biochar, stirring and drying, calcining the product in a protective gas atmosphere, mixing it with water, adjusting the pH of the system to 6.5-7.5 and letting it stand, and finally washing and drying to prepare the modified attapulgite.

2. The method for preparing modified attapulgite according to claim 1, characterized in that: In step (1), the mass ratio of the biochar to potassium hydroxide is 1:3; The mass ratio of the amount of water added in step (1) to potassium hydroxide is 5:3; The mass ratio of the attapulgite powder in step (2) to the powder in step (1) is 1:1-2.

3. The method for preparing modified attapulgite according to claim 1, characterized in that: The protective gases in step (2) and step (3) are both nitrogen; The temperature of the pyrolysis reaction in step (2) is 450-550°C, and the pyrolysis reaction time is 1 hour; The method of adjusting the pH of the system in step (3) is: adjusting by adding NaOH solution; The calcination temperature in step (3) is 700°C and the calcination time is 2h; The standing time in step (3) is 24 hours.

4. The method for preparing modified attapulgite according to claim 1, characterized in that: In step (3), the mass ratio of the attapulgite-based biochar to the ferric chloride solution is 1.6-2:5; In step (3), the mass ratio of the attapulgite-based biochar to the thiourea solution is 1-2:5; The concentration of the ferric chloride solution in step (3) is 2 mol·L -1 ; The concentration of the thiourea solution in step (3) is 1 mol·L -1 .

5. The modified attapulgite prepared by the method for preparing the modified attapulgite according to any one of claims 1 to 4.

6. A riverbank ecological substrate, characterized in that: The composition is prepared from the following components in parts by mass: 100-120 parts of planting soil, 3-6 parts of modified attapulgite as claimed in claim 5, 1-3 parts of zeolite-based composite materials, 0-3 parts of biochar, 1-3 parts of cement, 1-2 parts of greening additives and 5-10 parts of organic materials.

7. The riverbank ecological substrate according to claim 6, characterized in that: The zeolite-based composite material is prepared according to the following preparation method: zeolite and attapulgite are ground, sieved and mixed, cement and foaming agent are added to form a blank, and then cured in a steam box, wherein the mass ratio of zeolite, cement and attapulgite is 5-10:1-3:1-3.

8. The riverbank ecological substrate according to claim 7, characterized in that: The foaming agent is carbonate, and the cement is PO 42.5 grade ordinary Portland cement; The greening additive is ferrous sulfate; The organic material is soybean powder.

9. The riverbank ecological substrate according to claim 8, characterized in that: The carbonate is at least one of calcium carbonate, magnesium carbonate and sodium bicarbonate; The amount of the foaming agent added is 0.10% to 0.15% of the total mass of the zeolite, cement and attapulgite; The curing environment temperature is 60° C. and the humidity is 90%.

10. The method for preparing the riverbank ecological substrate according to any one of claims 6 to 9, characterized in that: The following steps are involved: The modified attapulgite, biochar, zeolite-based composite material, cement and greening additive are weighed in proportion, water is added and mixed evenly with the planting soil to obtain an initial improved product, and then organic materials are added.

Citation Information

Patent Citations

  • Preparation method of ferrous sulfide / attapulgite composite

    CN108043425A

  • Fired soil heavy metal remover and preparation method thereof

    CN109226216A

  • Attapulgite / cement porous composite adsorption material as well as preparation method and application thereof

    CN114405458A

  • Preparation and application of KOH modified charcoal / attapulgite composite material

    CN118253281A

  • Eco-friendly green soil composition for slope afforestation and eco-friendly method of slope afforestation using the same