Underwater non-dispersible concrete flocculant and preparation method thereof
Through the combination of polyacrylamide modified cellulose and porous silica nanoparticles, the problems of large water demand, large slump loss, and insufficient dispersion resistance of underwater non-dispersed concrete flocculants are solved, and concrete is realized Self-leveling, self-solidation and low strength losses reduce water quality pollution and have wide application prospects.
Patent Information
- Application Number
- CN202410971022.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
The existing underwater non-dispersible concrete flocculants have problems such as large water demand, large slump loss of mixture, insufficient dispersion resistance, long settling time and low strength.
Polyacrylamide modified cellulose, porous silica nanoparticles, fly ash, silica fume and polycarboxylic acid water reducing agent are mixed in a specific proportion, and the preparation method of modified cellulose and the pore-generating process of nanoparticles are used. A new underwater non-dispersible concrete flocculant was prepared to improve its viscosity, fluidity and dispersion resistance.
It has achieved the characteristics of self-leveling and self-condensing underwater, low strength loss, reducing water quality pollution, and improving the viscosity and fluidity of concrete. It is suitable for underwater construction and has broad application prospects.
Smart Images

Figure BDA0004953210690000091 
Figure BDA0004953210690000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flocculants, and in particular to an underwater non-dispersible concrete flocculant and a preparation method thereof. Background Art
[0002] When ordinary concrete mixture is poured into water, the flushing effect of water will separate the aggregate from the cement, and some of them will be carried away by water, losing the ability to cement the aggregate. Underwater non-dispersible concrete is to add admixtures mainly composed of flocculants to concrete. The "bridge" effect of the long molecular chain of the flocculant can form a stable spatial flexible network structure between cement particles and between cement and aggregates, thereby improving the cohesion of concrete, limiting the dispersion and segregation of concrete and avoiding cement loss.
[0003] At present, the commonly used underwater non-dispersible concrete flocculants are mainly divided into polypropylene series and cellulose series. Chinese invention patent application CN1216755A squeezes the plant juice and removes the residue, then cultivates at a constant temperature to obtain a culture solution; grinds the grain into powder, and performs water treatment to obtain gluten; mixes the above plant culture solution with gluten, stirs evenly and then cultivates to obtain a plant fiber protein adhesive; cement is evenly mixed with ultrafine silica powder, water reducer, and plant fiber protein adhesive. Chinese invention patent CN1326796C is an underwater anti-dispersible concrete admixture for construction, which is composed of methyl cellulose, polyacrylamide, sodium dodecyl benzene sulfonate, naphthalene-based high-efficiency water reducer, stearic acid, and zeolite powder. Chinese invention patent CN1003238B is an underwater concrete admixture for water injection, which is a mixture of polyacrylamide and shale ash or silica powder, and may contain anionic surfactants such as β-naphthalenesulfonic acid formaldehyde condensate.
[0004] The above flocculants often have the problems of large water demand, large slump loss of the mixture, insufficient anti-dispersion performance, long coagulation time and low strength. Summary of the invention
[0005] The purpose of the present invention is to provide an underwater non-dispersible concrete flocculant and a preparation method thereof. The newly mixed concrete added with the underwater non-dispersible concrete flocculant of the present invention has good viscosity and fluidity, and after the concrete is poured underwater, it has the characteristics of self-leveling and self-compacting, has good anti-dispersion, has low concrete strength loss during underwater construction, and reduces water pollution caused by pouring construction, and has broad application prospects.
[0006] The technical solution of the present invention is achieved in this way:
[0007] The invention provides an underwater non-dispersible concrete flocculant, which is prepared from the following raw materials in parts by weight: 2-4 parts of polyacrylamide modified cellulose, 0.5-0.7 parts of porous silicon dioxide nanoparticles, 0.2-0.4 parts of fly ash, 0.7-1 parts of silica fume and 3-5 parts of polycarboxylic acid water reducer.
[0008] As a further improvement of the present invention, the preparation method of the polyacrylamide-modified cellulose is as follows:
[0009] S1. Dissolving cellulose in an acid solution, adding maleic anhydride and concentrated sulfuric acid, heating to reflux reaction, to obtain carboxyl-modified cellulose;
[0010] S2. Activating the carboxyl-modified cellulose obtained in step S1 with 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide, adding acrylamide, heating and stirring the reaction, and obtaining acrylamide-modified cellulose;
[0011] S3. Add the acrylamide-modified cellulose obtained in step S2 into water, add an initiator, heat and stir to react, and obtain polyacrylamide-modified cellulose.
[0012] As a further improvement of the present invention, the acid solution in step S1 is a 1-2wt% acetic acid solution, the mass ratio of the cellulose, maleic anhydride and concentrated sulfuric acid is 10-12:5-7:0.5-1, and the reaction time is 5-7h.
[0013] As a further improvement of the present invention, the mass ratio of carboxyl modified cellulose, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide and acrylamide in step S2 is 10:5-7:4-6:3-5, the activation temperature is 0-4°C, the time is 0.5-1h, and the temperature of the heating and stirring reaction is 30-40°C, and the time is 7-10h.
[0014] As a further improvement of the present invention, in step S3, the mass ratio of acrylamide-modified cellulose to initiator is 100:1-2, the initiator is selected from at least one of potassium persulfate, sodium persulfate, and ammonium persulfate, and the temperature of the heating and stirring reaction is 50-60° C. and the time is 2-4 hours.
[0015] As a further improvement of the present invention, the preparation method of the porous silica nanoparticles is as follows: ethanol, water and ammonia water are stirred and mixed evenly, a porogen is added, an alkyl orthosilicate is added, heated and stirred for hydrolysis reaction, centrifuged, washed and dried to obtain porous silica nanoparticles.
[0016] As a further improvement of the present invention, the mass ratio of the ethanol, water, ammonia water, porogen and alkyl orthosilicate is 150-170:10-15:5-7:2-4:12-15, the porogen is selected from at least one of hexadecyltrimethylammonium bromide, hexadecyldimethylbenzylammonium bromide and hexadecyltrimethylammonium chloride, the alkyl orthosilicate is methyl orthosilicate or ethyl orthosilicate, and the temperature of the heated and stirred hydrolysis reaction is 35-45°C and the time is 12-15h.
[0017] As a further improvement of the present invention, the polycarboxylate water-reducing agent is polyacrylate or polystyrene ester.
[0018] As a further improvement of the present invention, the fly ash has a 45 μm sieve residue of ≤12%; and the silica ash has a 45 μm sieve residue of ≤0.01%.
[0019] The present invention further protects a method for preparing the above-mentioned underwater non-dispersible concrete flocculant, comprising the following steps: uniformly mixing polyacrylamide-modified cellulose, porous silica nanoparticles, fly ash, silica fume, and polycarboxylic acid water reducer to prepare the underwater non-dispersible concrete flocculant.
[0020] The present invention has the following beneficial effects:
[0021] The polyacrylamide modified cellulose prepared by the present invention has good water solubility by connecting acrylamide to cellulose molecules for modification, and the polyacrylamide modified cellulose prepared by initiation can significantly reduce the water bleeding rate of concrete and improve its anti-segregation ability, while also avoiding the problems of increased water demand and reduced fluidity of concrete. The preparation method is simple, the price is low, and it is convenient for wide application. At the same time, it also avoids the problems of high viscosity when a single polyacrylamide is added to mix concrete, high power requirements for mixing equipment, long mixing time, fast slump loss, and a large decrease in cohesion during underwater pouring, resulting in relatively low water and land strength, and the like.
[0022] The present invention also prepares porous silicon dioxide nanoparticles, and through sol-gel reaction and pore-forming effect, porous silicon dioxide nanoparticles with large specific surface area are obtained, which can increase the water retention capacity of concrete slurry. Under the synergistic effect of other inorganic materials such as fly ash and silica fume, it can not only cure quickly, but also ensure the initial strength.
[0023] The newly mixed concrete added with the underwater non-dispersible concrete flocculant of the present invention has good viscosity and fluidity, and after being poured underwater, the concrete has the characteristics of self-leveling and self-compacting, has good anti-dispersion, has low concrete strength loss during underwater construction, and reduces water pollution caused by pouring construction, and has broad application prospects. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] In the embodiment of the present invention: the fly ash 45 μm sieve residue is ≤12%; the silica ash 45 μm sieve residue is ≤0.01%; the polycarboxylate water reducer is a polyester polycarboxylate water reducer purchased from Shandong Tongsheng Building Materials Co., Ltd.; and the cellulose is hydroxyethyl cellulose.
[0026] Preparation Example 1 Preparation of polyacrylamide-modified cellulose
[0027] Here’s how:
[0028] S1. 10 g of cellulose was dissolved in 100 mL of 1 wt% acetic acid solution, 5 g of maleic anhydride and 0.5 g of concentrated sulfuric acid were added, and the reaction was heated under reflux for 5 h to obtain carboxyl-modified cellulose;
[0029] S2. 10 g of the carboxyl-modified cellulose obtained in step S1, 5 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 4 g of N-hydroxysuccinimide were dissolved in 200 mL of dichloromethane, activated at 0° C. for 0.5 h, and then 3 g of acrylamide was added. The mixture was heated to 30° C. and stirred for 7 h to obtain acrylamide-modified cellulose.
[0030] S3. Add 10 g of acrylamide-modified cellulose obtained in step S2 to 100 mL of water, add 0.1 g of potassium persulfate, heat to 50° C., and stir to react for 2 h to obtain polyacrylamide-modified cellulose.
[0031] Preparation Example 2 Preparation of polyacrylamide-modified cellulose
[0032] Here’s how:
[0033] S1. 12 g of cellulose was dissolved in 100 mL of 2 wt% acetic acid solution, 7 g of maleic anhydride and 1 g of concentrated sulfuric acid were added, and the reaction was heated under reflux for 7 h to obtain carboxyl-modified cellulose;
[0034] S2. 10 g of the carboxyl-modified cellulose obtained in step S1, 7 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 6 g of N-hydroxysuccinimide were dissolved in 200 mL of dichloromethane, activated at 4° C. for 1 h, and then 5 g of acrylamide was added. The mixture was heated to 40° C. and stirred for 10 h to obtain acrylamide-modified cellulose.
[0035] S3. Add 10 g of acrylamide-modified cellulose obtained in step S2 to 100 mL of water, add 0.2 g of ammonium persulfate, heat to 60° C., and stir to react for 4 h to obtain polyacrylamide-modified cellulose.
[0036] Preparation Example 3 Preparation of polyacrylamide-modified cellulose
[0037] Here’s how:
[0038] S1. 11 g of cellulose was dissolved in 100 mL of 1.5 wt% acetic acid solution, 6 g of maleic anhydride and 0.7 g of concentrated sulfuric acid were added, and the reaction was heated under reflux for 6 h to obtain carboxyl-modified cellulose;
[0039] S2. 10 g of the carboxyl-modified cellulose obtained in step S1, 6 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 5 g of N-hydroxysuccinimide were dissolved in 200 mL of dichloromethane, activated at 2° C. for 1 h, and then 4 g of acrylamide was added. The mixture was heated to 35° C. and stirred for 8 h to obtain acrylamide-modified cellulose.
[0040] S3. Add 10 g of acrylamide-modified cellulose obtained in step S2 to 100 mL of water, add 0.15 g of sodium persulfate, heat to 55° C., and stir to react for 3 h to obtain polyacrylamide-modified cellulose.
[0041] Comparative Preparation Example 1
[0042] Compared with Preparation Example 3, the difference is that step S3 is not performed.
[0043] The details are as follows:
[0044] S1. 11 g of cellulose was dissolved in 100 mL of 1.5 wt% acetic acid solution, 6 g of maleic anhydride and 0.7 g of concentrated sulfuric acid were added, and the reaction was heated under reflux for 6 h to obtain carboxyl-modified cellulose;
[0045] S2. 10 g of the carboxyl-modified cellulose obtained in step S1, 6 g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and 5 g of N-hydroxysuccinimide were dissolved in 200 mL of dichloromethane, activated at 2° C. for 1 h, and then 4 g of acrylamide was added. The mixture was heated to 35° C. and stirred for 8 h to obtain acrylamide-modified cellulose.
[0046] Preparation Example 4 Preparation of Porous Silica Nanoparticles
[0047] Here’s how:
[0048] 150 g of ethanol, 10 g of water, and 5 g of ammonia water were stirred and mixed for 20 min, 2 g of hexadecyltrimethylammonium chloride and 12 g of methyl orthosilicate were added, the mixture was heated to 35° C., the hydrolysis reaction was stirred for 12 h, the mixture was centrifuged, washed, and dried to obtain porous silica nanoparticles.
[0049] Preparation Example 5 Preparation of Porous Silica Nanoparticles
[0050] Here’s how:
[0051] 170 g of ethanol, 15 g of water and 7 g of ammonia water were stirred and mixed for 20 min, 4 g of hexadecyldimethylbenzyl ammonium bromide and 15 g of ethyl orthosilicate were added, the mixture was heated to 45° C., the hydrolysis reaction was stirred for 15 h, the mixture was centrifuged, washed and dried to obtain porous silica nanoparticles.
[0052] Preparation Example 6 Preparation of Porous Silica Nanoparticles
[0053] Here’s how:
[0054] 160 g of ethanol, 12 g of water and 6 g of ammonia water were stirred and mixed for 20 min, 3 g of hexadecyltrimethylammonium bromide and 13 g of ethyl orthosilicate were added, the mixture was heated to 40° C., the hydrolysis reaction was stirred for 13 h, the mixture was centrifuged, washed and dried to obtain porous silica nanoparticles.
[0055] Comparative Preparation Example 2
[0056] Compared with Preparation Example 6, the difference is that the porogen hexadecyltrimethylammonium bromide is not added.
[0057] The details are as follows:
[0058] 160 g of ethanol, 12 g of water and 6 g of ammonia water were stirred and mixed for 20 minutes, 13 g of ethyl orthosilicate was added, the mixture was heated to 40° C., the hydrolysis reaction was stirred for 13 hours, the mixture was centrifuged, washed and dried to obtain silica nanoparticles.
[0059] Example 1
[0060] 2 g of polyacrylamide-modified cellulose prepared in Preparation Example 1, 0.5 g of porous silica nanoparticles prepared in Preparation Example 4, 0.2 g of fly ash, 0.7 g of silica fume, and 3 g of polyester-type polycarboxylic acid water-reducing agent were stirred and mixed for 20 minutes to prepare an underwater non-dispersible concrete flocculant.
[0061] Example 2
[0062] 4 g of polyacrylamide-modified cellulose prepared in Preparation Example 2, 0.7 g of porous silica nanoparticles prepared in Preparation Example 5, 0.4 g of fly ash, 1 g of silica fume, and 5 g of polyester-type polycarboxylic acid water-reducing agent were stirred and mixed for 20 minutes to prepare an underwater non-dispersible concrete flocculant.
[0063] Example 3
[0064] 3 g of polyacrylamide-modified cellulose prepared in Preparation Example 3, 0.6 g of porous silica nanoparticles prepared in Preparation Example 6, 0.3 g of fly ash, 0.85 g of silica fume, and 4 g of polyester-type polycarboxylic acid water-reducing agent were stirred and mixed for 20 minutes to prepare an underwater non-dispersible concrete flocculant.
[0065] Comparative Example 1
[0066] Compared with Example 3, the difference is that the polyacrylamide-modified cellulose is prepared by Comparative Preparation Example 1.
[0067] The method comprises the following steps: 3 g of polyacrylamide-modified cellulose prepared in comparative preparation example 1, 0.6 g of porous silica nanoparticles prepared in preparation example 6, 0.3 g of fly ash, 0.85 g of silica fume, and 4 g of polyester-type polycarboxylic acid water-reducing agent are stirred and mixed for 20 minutes to prepare an underwater non-dispersible concrete flocculant.
[0068] Comparative Example 2
[0069] Compared with Example 3, the difference is that the porous silica nanoparticles prepared in Preparation Example 6 are replaced by the silica nanoparticles prepared in Comparative Preparation Example 2.
[0070] The method comprises the following steps: 3 g of polyacrylamide modified cellulose prepared in Preparation Example 3, 0.6 g of silicon dioxide nanoparticles prepared in Comparative Preparation Example 2, 0.3 g of fly ash, 0.85 g of silica fume, and 4 g of polyester polycarboxylic acid water reducer are stirred and mixed for 20 minutes to prepare an underwater non-dispersible concrete flocculant.
[0071] Comparative Example 3
[0072] Compared with Example 3, the difference is that the polyacrylamide-modified cellulose is replaced by cellulose.
[0073] The method comprises the following steps: 3 g of cellulose, 0.6 g of porous silica nanoparticles prepared in Preparation Example 6, 0.3 g of fly ash, 0.85 g of silica fume, and 4 g of polyester polycarboxylic acid water reducer are stirred and mixed for 20 minutes to prepare an underwater non-dispersible concrete flocculant.
[0074] Comparative Example 4
[0075] Compared with Example 3, the difference is that the polyacrylamide-modified cellulose is replaced by polyacrylamide.
[0076] The method comprises the following steps: 3g of polyacrylamide, 0.6g of porous silica nanoparticles prepared in Preparation Example 6, 0.3g of fly ash, 0.85g of silica fume and 4g of polyester polycarboxylic acid water reducer are stirred and mixed for 20 minutes to prepare an underwater non-dispersible concrete flocculant.
[0077] Comparative Example 5
[0078] Compared with Example 3, the difference is that no porous silica nanoparticles are added.
[0079] The method comprises the following steps: 3 g of polyacrylamide modified cellulose prepared in Preparation Example 3, 0.3 g of fly ash, 0.85 g of silica fume and 4 g of polyester polycarboxylic acid water reducer are stirred and mixed for 20 minutes to prepare an underwater non-dispersible concrete flocculant.
[0080] Test Example 1
[0081] The flocculants for underwater non-dispersible concrete flocculants prepared in Examples 1-3 and Comparative Examples 1-5 were added to concrete at an amount of 3% of the total weight of the cementitious materials. The properties of the resulting concrete were measured in accordance with DL / T 5117-2000 "Test Procedure for Underwater Non-dispersible Concrete". The results are shown in Table 1 below.
[0082] Table 1
[0083]
[0084]
[0085] It can be seen from the above table that the underwater non-dispersible concrete flocculants prepared in Examples 1-3 of the present invention and mixed with concrete have large slump, high strength, and a large water-to-land compressive strength ratio.
[0086] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An underwater non-dispersible concrete flocculant, characterized in that: The invention is prepared from the following raw materials in parts by weight: 2-4 parts of polyacrylamide modified cellulose, 0.5-0.7 parts of porous silicon dioxide nanoparticles, 0.2-0.4 parts of fly ash, 0.7-1 parts of silica ash and 3-5 parts of polycarboxylic acid water reducer.
2. The underwater non-dispersible concrete flocculant according to claim 1, characterized in that: The preparation method of the polyacrylamide modified cellulose is as follows: S1. Dissolving cellulose in an acid solution, adding maleic anhydride and concentrated sulfuric acid, heating to reflux reaction, to obtain carboxyl-modified cellulose; S2. Activating the carboxyl-modified cellulose obtained in step S1 with 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide, adding acrylamide, heating and stirring the reaction, and obtaining acrylamide-modified cellulose; S3. Add the acrylamide-modified cellulose obtained in step S2 into water, add an initiator, heat and stir to react, and obtain polyacrylamide-modified cellulose.
3. The underwater non-dispersible concrete flocculant according to claim 2, characterized in that: In step S1, the acid solution is a 1-2 wt% acetic acid solution, the mass ratio of the cellulose, maleic anhydride and concentrated sulfuric acid is 10-12:5-7:0.5-1, and the reaction time is 5-7 hours.
4. The underwater non-dispersible concrete flocculant according to claim 2, characterized in that: In step S2, the mass ratio of carboxyl modified cellulose, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, N-hydroxysuccinimide and acrylamide is 10:5-7:4-6:3-5, the activation temperature is 0-4°C, the time is 0.5-1h, and the heating and stirring reaction temperature is 30-40°C, and the time is 7-10h.
5. The underwater non-dispersible concrete flocculant according to claim 2, characterized in that: In step S3, the mass ratio of acrylamide-modified cellulose to initiator is 100:1-2, the initiator is selected from at least one of potassium persulfate, sodium persulfate, and ammonium persulfate, and the temperature of the heating and stirring reaction is 50-60° C. and the time is 2-4 hours.
6. The underwater non-dispersible concrete flocculant according to claim 1, characterized in that: The preparation method of the porous silica nanoparticles is as follows: ethanol, water and ammonia water are stirred and mixed evenly, a porogen is added, an alkyl orthosilicate is added, heated and stirred for hydrolysis reaction, centrifuged, washed and dried to obtain the porous silica nanoparticles.
7. The underwater non-dispersible concrete flocculant according to claim 6, characterized in that The mass ratio of the ethanol, water, ammonia water, porogen and alkyl orthosilicate is 150-170:10-15:5-7:2-4:12-15, the porogen is selected from at least one of hexadecyltrimethylammonium bromide, hexadecyldimethylbenzylammonium bromide and hexadecyltrimethylammonium chloride, the alkyl orthosilicate is methyl orthosilicate or ethyl orthosilicate, the temperature of the heated and stirred hydrolysis reaction is 35-45°C, and the time is 12-15h.
8. The underwater non-dispersible concrete flocculant according to claim 1, characterized in that: The polycarboxylate water reducer is polyacrylate or polystyrene ester.
9. The underwater non-dispersible concrete flocculant according to claim 1, characterized in that: The fly ash has a 45 μm sieve residue of ≤12%; the silica ash has a 45 μm sieve residue of ≤0.01%.
10. A method for preparing the underwater non-dispersible concrete flocculant according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: uniformly mixing polyacrylamide modified cellulose, porous silicon dioxide nanoparticles, fly ash, silica ash and polycarboxylic acid water reducing agent to prepare underwater non-dispersible concrete flocculant.
Citation Information
Patent Citations
Special additive for underwater undispersed shrinking-free grouting material
CN101519288A
Degradable cellulose-polyacrylamide composite water-retaining agent and preparation method thereof
CN112851860A
High-flow-state ultra-high performance concrete and preparation method thereof
CN117623694A
Modified methyl cellulose flocculant for underwater grouting and its manufacturing method
CN1911850A
Solvent-soluble substances characterized in that water-soluble cellulose ethers are chemically bonded to water-soluble, at least predominately synthetic polymers containing acrylic units
US4330441A