Superfine spherical manganese oxide as well as preparation method and application thereof

Through the surface modification and high-temperature spherical slurry process of ultrafine spherical manganese oxide powder, the problems of high friction resistance and poor rheology performance in petroleum cementing are solved, the replacement efficiency and cementing quality are improved, and high-density cementing slurry is achieved The stability and fluidity of the oil and gas wells extend the mining life.

CN118908625APending Publication Date: 2024-11-08SICHUAN MAIKEWEI NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410891492.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

During the petroleum cementing process, conventional cement slurry systems have problems such as high friction resistance, poor rheology performance and low replacement efficiency, which affect the cementing operation efficiency and quality.

Method used

Ultrafine spherical manganese oxide powder is used as the weighting material, and prepared by surface modification and high-temperature spherification technology, high density with density ≥4.6g/cm3, particle size distribution D50<6μm, D90<20μm, and particle spherical rate ≥96%. , micron-scale spherical weighted material used to improve the fluidity and dispersion of cement slurry.

Benefits of technology

It significantly reduces the friction resistance of cement slurry, improves the replacement efficiency and cementing quality, extends the mining years of oil and gas wells, and reduces drilling tool wear, replacing high-end weighting agents imported from abroad.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908625A_ABST
    Figure CN118908625A_ABST
Patent Text Reader

Abstract

The invention relates to superfine spherical manganese oxide as well as a preparation method and application thereof. The preparation method mainly comprises the following steps: 1) selecting high-quality manganese oxide with Mn content of more than or equal to 65% and density of more than or equal to 4.6 g / cm < 3 > as a raw material; 2) impurity removal and drying of manganese oxide powder are carried out, so that the water content is less than or equal to 1.0%, and the content of water-soluble alkali metal (based on calcium) in the manganese oxide powder is less than or equal to 100mg / kg; (3) carrying out airflow superfine grinding on the manganese oxide powder; (4) selecting and grading the manganese oxide powder, and screening out the manganese oxide powder with the particle size of less than or equal to 20 microns; 5) carrying out surface modification treatment on the screened manganese oxide powder; according to the superfine spherical manganese oxide powder obtained through the method, the particle size distribution D50 is smaller than 6 micrometers, the particle size distribution D90 is smaller than 20.0 micrometers, and an electron microscope image shows that the surface of the manganese oxide powder is smooth, and the sphericity degree is good; the high-density cement paste prepared by adding 10-30% of the manganese oxide powder can obviously improve the rheological property of the cement paste, reduce the friction resistance of the cement paste and improve the displacement efficiency, and meanwhile, set cement is higher in strength and more compact, and is beneficial to improving the well cementation quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal mineral product processing and admixtures for oil well cementing, and in particular to ultrafine spherical manganese oxide and a preparation method and application thereof. Background Art

[0002] During the oil and gas exploration and development process, when cementing operations are carried out under complex conditions such as high-pressure oil and gas layers, salt-gypsum layers, high-pressure water layers and unstable formations, in order to increase the liquid column pressure to stabilize the formation, prevent blowout and salt-gypsum layer creep from damaging casing or drilling tools, etc., it is necessary to use high-density or ultra-high-density cement slurry systems for cementing, so that the liquid column pressure and formation pressure can reach a relative balance during the cementing process. In petroleum cementing operations, conventional cement slurry systems often face problems such as high friction resistance, poor rheological properties and low displacement efficiency. These problems not only affect the efficiency of cementing operations, but may also have an adverse effect on cementing quality. In order to solve these problems, researchers began to explore adding special weighting material additives to cement slurry, such as spherical manganese oxide powder, to obtain high-density and ultra-high-density cement slurry systems. The different properties of weighting materials will directly affect the performance of the configured high-density cement slurry, and will also have a very significant impact on the overall cementing quality. Therefore, the development of high-performance weighting materials is of great significance to the development of cementing work.

[0003] During the cementing process, the flow of cement slurry in the pipeline will be affected by friction resistance, resulting in high friction resistance. This not only places high demands on cementing equipment, but also reduces the cement slurry displacement efficiency and affects the cementing quality. Spherical manganese oxide powder, due to its unique spherical structure and small particle size, can play a lubricating role in cement slurry, reduce the friction coefficient between cement slurry and pipeline wall, and thus effectively reduce friction resistance. High-density cement slurry systems formulated with conventional weighting materials often show poor rheological properties during the cementing process, often resulting in incomplete displacement, leaving voids or forming unstable interfaces. Due to the addition of spherical manganese oxide powder, the displacement efficiency of cement slurry is significantly improved. Its excellent fluidity and dispersibility enable cement slurry to more easily enter the tiny gaps in the wellbore, achieve more complete displacement, reduce the formation of voids and unstable interfaces, and help extend the production life of oil and gas wells.

[0004] In summary, spherical manganese oxide powder, as an important admixture, has significant advantages in changing the high friction resistance and poor rheological properties of conventional cement slurry systems and improving the cement slurry displacement efficiency. However, there are still relatively few studies on the preparation method and application of spherical manganese oxide powder. Therefore, developing a simple, efficient and economical method for preparing ultrafine spherical manganese oxide and applying it in the field of oil cementing is of great significance for improving cementing quality and promoting the sustainable development of the oil industry. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide an ultrafine spherical manganese oxide and a preparation method and application thereof. The ultrafine spherical manganese oxide prepared by the method has a density of ≥4.6 g / cm 3 , particle size distribution D50<6μm, D90<20μm, particle sphericity ≥96%, which belongs to high-density, micron-level spherical weighting material. This high-density, micron-level spherical weighting material is applied to drilling fluid and cement slurry. Compared with traditional weighting materials, it has excellent characteristics such as good sedimentation stability, corrosion resistance, and reduced drill tool wear. It is of great significance to replace imported high-end weighting agent products from abroad.

[0006] The objective of the present invention is achieved through the following technical solutions:

[0007] The invention discloses an ultrafine spherical manganese oxide, which is obtained by subjecting ultrafine manganese oxide powder modified by a surface modifier to high-temperature spheroidization; the modification refers to mixing the surface modifier with the ultrafine manganese oxide powder so that the modifier is uniformly adsorbed on the surface of the ultrafine manganese oxide powder.

[0008] In a preferred embodiment of the present scheme, the particle size D50 of the ultrafine manganese oxide powder is 3.0 μm to 5.5 μm, and D90 is 10.0 μm to 20.0 μm.

[0009] In a preferred embodiment of the present scheme, the surface modifier includes but is not limited to any one of coupling agents such as γ-methacryloxypropyltrimethoxysilane, di(octylphenol polyoxyethylene ether) phosphite, quaternary ammonium salts, and polyoxyethylene ether surfactants; the mixing ratio of the surface modifier to the classified ultrafine manganese oxide powder is 0.5 to 2:100.

[0010] The method for preparing the ultrafine spherical manganese oxide comprises the following steps:

[0011] S1, removing impurities and drying manganese oxide powder;

[0012] S2, air flow ultrafine grinding of manganese oxide powder;

[0013] S3, classifying the manganese oxide powder after the airflow ultrafine grinding to obtain ultrafine manganese oxide powder;

[0014] S4, mixing and stirring the surface modifier with the classified ultrafine manganese oxide powder to obtain the surface-modified ultrafine manganese oxide powder;

[0015] S5. The surface-modified ultrafine manganese oxide powder is fed into a spheroidizing device, and spheroidized in a high-temperature spheroidizing furnace to obtain ultrafine spherical manganese oxide powder.

[0016] In a preferred embodiment of the present solution, the method further comprises step S0;

[0017] S0, manganese oxide powder raw material selection, the manganese oxide powder Mn content ≥ 65%, density ≥ 4.6g / cm 3 .

[0018] In a preferred embodiment of the present invention, the manganese oxide powder is a mixture of one or more of manganese monoxide, manganese dioxide, dimanganese trioxide, and trimanganese tetraoxide.

[0019] Further preferably, the manganese oxide powder is trimanganese tetraoxide. In addition, in the mixed manganese powder, the higher the proportion of trimanganese tetraoxide, the more conducive it is to reducing the difficulty of pre-treatment of the mixture.

[0020] In a preferred embodiment of the present scheme, the surface modifier includes but is not limited to any one of coupling agents such as γ-methacryloxypropyltrimethoxysilane, di(octylphenol polyoxyethylene ether) phosphite, quaternary ammonium salts, and polyoxyethylene ether surfactants; and / or

[0021] The mixing ratio of the surface modifier to the classified ultrafine manganese oxide powder is 0.5 to 2:100.

[0022] In the present disclosure, the modifier is uniformly adsorbed on the powder surface; the physical and chemical properties of the surface of the ultrafine manganese oxide powder are adjusted to enhance its dispersibility and fluidity, and reduce the mutual attraction and adhesion between particles, thereby optimizing the performance of the powder during the spheroidization process.

[0023] In a preferred embodiment of the present scheme, the step S1 is specifically as follows: putting the manganese oxide powder into a decontamination tank, adding a 0.1 mol / L to 1.0 mol / L chelating agent aqueous solution to remove soluble alkaline earth metals in the manganese oxide powder, and then drying the manganese oxide powder for inspection to obtain manganese oxide powder that meets the requirements.

[0024] In a preferred embodiment of the present scheme, the moisture content of the manganese oxide powder after impurity removal and drying in S1 is ≤1.0%, and the content of water-soluble alkali metal (calculated as calcium) is ≤100 mg / kg.

[0025] In a preferred embodiment of this scheme, the complexing agent in step S1 is a mixture of one or more of disodium ethylenediaminetetraacetate, sodium salt of ethylenediaminetetramethylenephosphine, AA / AMPS polymer, sodium salt of hydroxyethylidene diphosphine; and / or

[0026] The amount of complexing agent added is 0.02% to 0.3% based on the mass of manganese oxide powder.

[0027] In a preferred embodiment of the present scheme, in the step S2, the airflow ultrafine grinding of manganese oxide powder is performed by using an airflow pulverizer; the airflow pulverizer is any one of a collision-type airflow pulverizer, a flat airflow pulverizer, a fluidized bed airflow pulverizer, and an impact-type airflow pulverizer.

[0028] The manganese oxide powder after impurities removal is put into the air flow mill for crushing. The manganese oxide powder is accelerated by compressed gas, and then the manganese oxide powder is driven to be ejected through the nozzle with supersonic air flow, so that the manganese oxide powder tumbles, collides, and rubs against each other to achieve the purpose of ultrafine crushing.

[0029] In a preferred embodiment of the present scheme, in the step S3, the particle size D50 of the classified ultrafine manganese oxide powder is 3.0 μm to 5.5 μm, and D90 is 10.0 μm to 20.0 μm.

[0030] In a preferred embodiment of this solution, step S3 is specifically as follows:

[0031] The jet-milled manganese oxide powder is passed through a high-precision eddy current classifier to classify the ultrafine manganese oxide powder that meets the particle size requirements. The large particles that do not meet the particle size requirements will be returned to the jet mill for re-milling to screen the ultrafine manganese oxide powder with the appropriate particle size.

[0032] Further preferably, the pulverization in step S2 can be performed by airflow ultrafine pulverization or a combination of airflow ultrafine pulverization and Raymond mill, and the airflow classification can be performed by high-precision eddy current classification.

[0033] In a preferred embodiment of the present scheme, in the step S5, the spheroidizing device is any one of a flame high-temperature spheroidizing furnace, a plasma high-temperature spheroidizing furnace, and a supersonic flame spray gun.

[0034] In step S5, the surface-modified ultrafine manganese oxide powder is fed into a spheroidizing device, and the surface of the manganese oxide powder is softened and melted by a high-temperature flame. The sufficient contact time between the high-temperature flame and the manganese oxide powder is controlled within a certain range. Under the action of surface tension, a spherical shape is formed, and then it is rapidly cooled to obtain an ultrafine spherical manganese oxide powder.

[0035] In a preferred embodiment of the present scheme, the flame temperature of the spheroidizing furnace during the spheroidizing process of the manganese oxide powder in S5 is 1600°C to 2200°C.

[0037] Furthermore, in a preferred embodiment of the present invention, the high temperature spheroidizing furnace is provided with an air flow pressure system, an oxidizing atmosphere gas distribution system, and a heating system. The spheroidizing process needs to be carried out under oxidizing atmosphere conditions, and the surface of the manganese oxide powder is softened and melted by high temperature, and spherical shapes are formed under the action of surface tension, and then rapidly cooled to obtain ultrafine spherical manganese oxide powder.

[0038] In a preferred embodiment of the present scheme, the manganese oxide powder in S5 is transported to a cooling device via airflow to complete surface homogenization of the spherical micro-powder particles, and finally the micron-sized spherical weighting material is collected by a micro-powder collecting device.

[0039] Application of the ultrafine spherical manganese oxide mentioned above, or the ultrafine spherical manganese oxide prepared by the above method, in drilling fluid and cement slurry.

[0040] In the present disclosure, the high-purity manganese oxide powder selected in step S0 is subjected to impurity removal and drying treatment to obtain manganese oxide powder in which the water content and soluble alkaline earth metal meet the requirements; the treated high-purity manganese oxide powder is subjected to ultrafine grinding-airflow classification to obtain micropowder particles with a particle size distribution of D90≤20.0μm; the obtained micropowder particles are subjected to surface modification treatment to make the surface of the micropowder particles have lipophilic and non-hydrophilic groups; the purpose of the surface modification treatment is to solve the key technical problem that micron-level powder materials are easy to agglomerate, so that the particle size of the micron-level powder particles after the subsequent high-temperature spheroidization process remains basically the same as that before spheroidization, with a particle size D90≤20.0μm, and there is no phenomenon that the particles are significantly enlarged due to agglomeration.

[0041] In the high-temperature spheroidization process disclosed in the present invention, the micro powder particles are transported to the high-temperature spheroidization furnace through the air flow pressure system, the oxidizing atmosphere is maintained under the action of the oxidizing atmosphere gas distribution system, the heating system heats the temperature to 1600°C to 2200°C, and the particles melt. Finally, the ultrafine manganese oxide micro powder particles are cooled and formed to prepare micron-sized spherical weighting agent particles, thereby achieving the adjustment of the surface uniformity and sphericity of the spherical material. The sphericity of the prepared micron-sized spherical weighting material is ≥96%; the density is 4.5 to 5.6 g / cm 3 , particle size distribution D90 is 6.0μm~20.0μm.

[0042] The beneficial effects of the present invention are:

[0043] (1) The present disclosure has a density of ≥4.6 g / cm 3 High-purity manganese oxide powder is used as a basic raw material to prepare ultrafine spherical manganese oxide powder. High-purity manganese oxide powder is a product of a manganese ore dressing plant. The raw material is easily available and inexpensive, which reduces the production cost of ultrafine spherical manganese oxide powder weighting materials;

[0044] (2) The present disclosure uses a coupling agent or a surfactant to modify the surface of the powder, which solves the key technical problem that the micron-sized powder material is easy to agglomerate, so that the particle size of the micron-sized powder during the spheroidization process of the high-temperature spheroidization device remains basically the same as that before spheroidization, with a particle size D50 < 6 μm, and the particles do not increase significantly due to agglomeration;

[0045] (3) The high-temperature spheroidization device can adjust the surface uniformity and sphericity of the spherical material by precisely controlling the temperature, oxidizing atmosphere, and airflow conveying pressure. The sphericity of the prepared ultrafine spherical manganese oxide powder weighting material is ≥96%;

[0046] (4) The ultrafine spherical manganese oxide powder prepared in the present invention has a small particle size and a smooth surface, and therefore has the advantages of good filling and fluidity, and is not easy to bridge. After being added to cement slurry, it can reduce the thickening phenomenon, reduce friction, enhance dispersibility, and improve the bottom displacement efficiency;

[0047] (5) The ultrafine spherical manganese oxide powder particles prepared in the present invention are densely packed, the filling amount can reach the maximum, the porosity is low, and the filling is uniform and consistent, which is conducive to controlling the density of cement slurry and achieving dense packing. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 This is an electron micrograph of the micrometer-sized non-spherical manganese oxide prepared in Comparative Example 1 of the present invention;

[0049] Figure 2 This is an electron micrograph of the micron-sized spherical manganese oxide prepared in Example 1 of the present invention;

[0050] Figure 3 This is an electron micrograph of the spherical manganese oxide prepared in Comparative Example 2 of the present invention;

[0051] Figure 4 This is a photo of the fluidity of the micron-sized non-spherical manganese oxide prepared in Comparative Example 1 of the present invention;

[0052] Figure 5 This is a photograph of the fluidity of the micron-sized spherical manganese oxide prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0053] The present invention is further described in detail below through specific embodiments, but this should not be construed as limiting the scope of the present invention to the following examples. Without departing from the above-mentioned method concept of the present invention, various substitutions or changes made according to common technical knowledge and conventional means in the art should be included in the scope of the present invention.

[0054] Example 1

[0055] An ultrafine spherical manganese oxide, the raw material selected has a Mn content of 68% and a density of 4.6g / cm 3 The preparation method of high-purity manganese tetraoxide ore powder comprises the following steps:

[0056] (1) Select a density of 4.6 g / cm 3The manganese tetroxide powder is removed and dried; the manganese tetroxide powder is put into a removal tank, and a 0.2% complexing agent is a mixed aqueous solution of ethylenediaminetetraacetic acid disodium and AA / AMPS polymer to remove soluble alkaline earth metals in the micro-powder particles, and then the micro-powder particles are dried and sent for inspection, and the moisture content is 0.6%, and the soluble alkaline earth metal content (calculated as calcium) is 60 mg / kg, which meets the standard requirements;

[0057] (2) The impurity-free micro-powder particles are put into an impact airflow mill, the particles are accelerated by compressed gas, and then the powder is ejected through a nozzle with a supersonic airflow, causing the powder to tumble, collide, and rub against each other to achieve the purpose of ultrafine grinding;

[0058] (3) The fine powder particles after air flow pulverization are passed through a high-precision eddy current classifier to classify the particle powders that meet the particle size requirements. The large particles that do not meet the particle size requirements are returned to the air flow pulverizer for re-pulverization to obtain the classified ultrafine manganese oxide powder with a particle size D50 of 3.0 μm and a D90 of 11.0 μm;

[0059] (4) selecting γ-methacryloxypropyltrimethoxysilane coupling agent as a surface modifier, mixing it with the classified ultrafine manganese oxide powder in a ratio of 1:50 and stirring for 15 minutes, so that the modifier is uniformly adsorbed on the powder surface; then, in a box dryer, using hot air at normal pressure as a drying medium to evaporate the solvent in the pores of the ultrafine manganese oxide powder, and performing a drying process;

[0060] (5) feeding the surface-modified ultrafine manganese oxide powder into a flame high-temperature spheroidizing furnace, softening and melting the surface of the manganese oxide powder by the heat generated by the high-temperature flame, the high-temperature flame and the manganese oxide powder are fully contacted for about 0.5 seconds, the flame temperature of the spheroidizing furnace is 1900° C., and under the action of surface tension, a spherical shape is formed, and then rapidly cooled, and finally the micron-sized spherical weighted material is collected by a micro powder collecting device;

[0061] (6) The density of the prepared micron-sized spherical weighting agent is 4.6 g / cm 3 The particle size distribution D50 is 1.5μm, D90 is 6.0μm, and the sphericity rate is 97%. Figure 2 shown.

[0062] Example 2

[0063] The raw material selection has a Mn content of 69% and a density of 4.9g / cm 3 High purity manganese dioxide ore powder.

[0064] The preparation method of ultrafine spherical manganese oxide comprises the following steps:

[0065] (1) Select a density of 4.9 g / cm 3 The manganese dioxide ore powder is removed and dried; the manganese dioxide powder is put into the impurity removal tank, and a 0.3% complexing agent, ethylenediaminetetramethylenephosphonic acid aqueous solution, is added to remove the soluble alkaline earth metals in the micro powder particles, and then the micro powder particles are dried and sent for inspection. The moisture content is 0.4%, and the soluble alkaline earth metal content (calculated as calcium) is 55 mg / kg, which meets the standard requirements;

[0066] (2) The impurity-free micro-powder particles are put into a fluidized bed airflow mill. After being frozen, filtered, and dried, the compressed air is injected into the pulverizing chamber through a nozzle to form a supersonic airflow, so that the material is fluidized. The accelerated material converges at the intersection of the jet airflows of several nozzles, generating violent collision, friction, and shearing to achieve the purpose of ultrafine pulverization;

[0067] (3) The fine powder particles after air flow pulverization are passed through a high-precision eddy current classifier to classify the particle powders that meet the particle size requirements. The large particles that do not meet the particle size requirements are returned to the air flow pulverizer for re-pulverization to obtain the classified ultrafine manganese oxide powder with a particle size D50 of 5.0 μm and a D90 of 12.0 μm;

[0068] (4) selecting di(octylphenol polyoxyethylene ether) phosphite coupling agent as a surface modifier, mixing it with the classified ultrafine manganese dioxide powder in a ratio of 1:50 and stirring for 15 minutes, so that the modifier is uniformly adsorbed on the powder surface; then, in a box dryer, using hot air at normal pressure as a drying medium to evaporate the solvent in the pores of the ultrafine manganese oxide powder, and performing a drying process;

[0069] (5) feeding the modified ultrafine manganese dioxide powder into a flame high-temperature spheroidizing furnace, softening and melting the surface of the manganese oxide powder by the heat generated by the high-temperature flame, the full contact time between the high-temperature flame and the manganese oxide powder is about 0.5 s, the flame temperature of the spheroidizing furnace is 1900° C., and under the action of surface tension, the powder is formed into a spherical shape, and then rapidly cooled, and finally the micron-sized spherical weighted material is collected by a micro powder collecting device;

[0070] (6) The density of the prepared micron-sized spherical weighting agent is 4.9 g / cm 3 , particle size distribution D50 is 3.5μm, D90 is 6.0μm, and the sphericity rate is 98%.

[0071] Example 3

[0072] The raw material selection has a Mn content of 69% and a density of 4.9g / cm 3 High purity manganese tetraoxide, manganese dioxide mixed manganese oxide ore powder.

[0073] The preparation method of ultrafine spherical manganese oxide comprises the following steps:

[0074] (1) Select a density of 4.9 g / cm 3 The high-purity manganese tetraoxide and manganese dioxide mixed powder particles (ratio 7:3) are removed and dried. The mixed powder particles are put into the impurity removal tank, and 0.3% of the complexing agent ethylenediaminetetramethylenephosphonic acid aqueous solution is added to remove the soluble alkaline earth metals in the mixed powder. Then the micro powder particles are dried and sent for inspection. The moisture content is 0.5%, and the soluble alkaline earth metal content (calculated as calcium) is 70mg / kg, which meets the standard requirements;

[0075] (2) The mixed powder particles after impurity removal are put into the collision type airflow pulverizer, and the high-speed airflow is used to drive the materials to move at high speed in the pulverizing chamber, so that the materials collide, rub and shear violently, thereby achieving the purpose of ultrafine pulverization;

[0076] (3) The mixed micro-powder particles after air flow milling are passed through a high-precision eddy current classifier to classify ultrafine manganese oxide powder that meets the particle size requirements. The large particles that do not meet the particle size requirements are returned to the air flow mill and milled again to obtain the classified ultrafine manganese oxide powder with a particle size D50 of 3.0 μm and a D90 of 10.5 μm;

[0077] (4) selecting γ-methacryloxypropyltrimethoxysilane coupling agent as a surface modifier, mixing it with the classified mixed micropowder particles in a ratio of 1:50 and stirring for 15 minutes, so that the modifier is uniformly adsorbed on the powder surface; then, in a box dryer, using hot air at normal pressure as a drying medium to evaporate the solvent in the pores of the ultrafine manganese oxide powder, and performing a drying process;

[0078] (5) feeding the modified ultrafine mixed manganese oxide powder into a plasma high-temperature spheroidizing furnace, using the high temperature and high energy of the plasma to melt and evaporate the particle surface, and then rapidly cooling the melted and evaporated micropowder particles into a spherical shape under the action of the plasma, and finally collecting the micron-sized spherical weighting material through a micropowder collecting device;

[0079] (6) The density of the prepared micron-sized spherical weighting agent is 4.9 g / cm 3 , particle size distribution D50 is 2.0μm, D90 is 8.0μm, and the sphericity rate is 94%.

[0080] Example 4

[0081] The raw material selection has a Mn content of 70% and a density of 4.7g / cm 3 High-purity trimanganese tetroxide, manganese monoxide, and dimanganese trioxide mixed manganese oxide ore powder, and the ratio of high-purity trimanganese tetroxide, manganese monoxide, and dimanganese trioxide is 5:3:2.

[0082] The preparation method of ultrafine spherical manganese oxide comprises the following steps:

[0083] (1) Select a density of 4.7 g / cm 3 The high-purity manganese tetraoxide, manganese monoxide, and manganese trioxide mixed powder particles are removed and dried. The mixed powder particles are put into the impurity removal tank, and a 0.15% complexing agent, which is a mixed aqueous solution of ethylenediaminetetraacetic acid disodium and hydroxyethylidene diphosphonic acid, is added to remove the soluble alkaline earth metals in the mixed powder. The micro powder particles are then dried and sent for inspection. The moisture content is 0.8%, and the soluble alkaline earth metal content (calculated as calcium) is 80 mg / kg, which meets the standard requirements.

[0084] (2) The mixed powder particles after impurity removal are put into a flat air flow mill. Compressed air enters the air flow distribution chamber through the inlet, generating negative pressure. The material particles enter the mixing chamber and are then sprayed into the grinding chamber by the high-speed air flow ejected from the nozzle. The micro powder particles rotate at a very high speed under the high-speed air flow ejected from the nozzle, making a circular motion. The particles collide and rub against each other and against the inner wall of the grinding chamber, thereby achieving the purpose of ultrafine grinding.

[0085] (3) The mixed micro-powder particles after air flow milling are passed through a high-precision eddy current classifier to classify ultrafine manganese oxide powder that meets the particle size requirements. The large particles that do not meet the particle size requirements are returned to the air flow mill and milled again to obtain the classified ultrafine manganese oxide powder with a particle size D50 of 4.5 μm and a D90 of 12.0 μm;

[0086] (4) selecting a quaternary ammonium salt surfactant as a modifier, mixing it with the classified mixed micro-powder particles in a ratio of 1:50 and stirring for 15 minutes, so that the modifier is uniformly adsorbed on the powder surface; then, in a box dryer, using normal pressure hot air as a drying medium to evaporate the solvent in the pores of the ultrafine manganese oxide powder, and performing a drying process;

[0087] (5) The modified ultrafine mixed manganese oxide powder is fed into a supersonic flame spray gun spheroidizing furnace, and a fuel gas (such as hydrogen, propane, propylene or acetylene-methane-propane mixed gas, etc.) and a combustion aid (such as oxygen) are introduced into the combustion chamber in a certain proportion for mixing. Then, the high-temperature gas generated by the explosive combustion passes through the expansion tube at a supersonic speed, and a quantitative amount of powder is fed into the high-temperature combustion gas along the tungsten carbide central sleeve in the combustion head. The high-temperature combustion gas and the manganese oxide powder are fully contacted for about 0.5 seconds, and the surface of the manganese oxide powder is softened and melted. The flame temperature of the spheroidizing furnace is 2000°C. Under the action of surface tension, a sphere is formed, and then it is rapidly cooled. Finally, the micron-sized spherical weighting material is collected by a micro powder collection device.

[0088] (6) The density of the prepared micron-sized spherical weighting agent is 4.7 g / cm 3, particle size distribution D50 is 3μm, D90 is 7.0μm, and the sphericity rate is 95%.

[0089] Comparative Example 1

[0090] The raw material selection has a Mn content of 68% and a density of 4.5g / cm 3 The preparation method comprises the following steps:

[0091] (1) Select a density of 4.5 g / cm 3 The manganese tetroxide powder is put into the impurity removal tank, and 0.2% of the complexing agent is a mixed aqueous solution of ethylenediaminetetraacetic acid disodium and AA / AMPS polymer to remove the soluble alkaline earth metals in the micro-powder particles. The micro-powder particles are then dried and sent for inspection. The moisture content is 0.6%, and the soluble alkaline earth metal content (calculated as calcium) is 60 mg / kg, which meets the standard requirements.

[0092] (2) The impurity-free micro-powder particles are put into an impact airflow mill, the particles are accelerated by compressed gas, and then the powder is ejected through a nozzle with a supersonic airflow, causing the powder to tumble, collide, and rub against each other to achieve the purpose of ultrafine grinding;

[0093] (3) The fine powder particles after air flow pulverization are passed through a high-precision eddy current classifier to classify the particle powders that meet the particle size requirements. The large particles that do not meet the particle size requirements are returned to the air flow pulverizer for re-pulverization to obtain the classified ultrafine manganese oxide powder with a particle size D50 of 5.5 μm and a D90 of 15.0 μm;

[0094] (4) selecting γ-methacryloxypropyltrimethoxysilane coupling agent as a modifier, mixing it with the classified mixed micro-powder particles in a ratio of 1:50 and stirring for 15 minutes, so that the modifier is uniformly adsorbed on the powder surface; then, entering into a box dryer, using normal pressure hot air as a drying medium, evaporating the solvent in the pores of the ultrafine manganese oxide powder, and performing a drying process;

[0095] (5) The density of the prepared micron-sized non-spherical weighting agent is 4.5 g / cm 3 The particle size distribution D50 is 4.5μm and D90 is 12.0μm. The scanning electron microscope photo is shown in Figure 1 shown.

[0096] Comparative Example 2

[0097] The raw material selection has a Mn content of 70% and a density of 4.7g / cm 3The high-purity manganese tetraoxide, manganese monoxide, and manganese trioxide mixed manganese oxide ore powder, the ratio of high-purity manganese tetraoxide, manganese monoxide, and manganese trioxide is 5:3:2; the preparation method comprises the following steps:

[0098] (1) Select a density of 4.7 g / cm 3 The high-quality manganese tetraoxide, manganese monoxide, and manganese trioxide mixed powder particles are removed and dried. The mixed powder particles are put into the impurity removal tank, and a 0.15% complexing agent, which is a mixed aqueous solution of ethylenediaminetetraacetic acid disodium and hydroxyethylidene diphosphonic acid, is added to remove the soluble alkaline earth metals in the mixed powder. Then the micro powder particles are dried and sent for inspection. The moisture content is 0.8%, and the soluble alkaline earth metal content (calculated as calcium) is 80mg / kg, which meets the standard requirements;

[0099] (2) The mixed powder particles after impurities removal are put into a flat airflow pulverizer. Compressed air enters the airflow distribution chamber through the inlet, generating negative pressure. The material particles enter the mixing chamber and are then sprayed into the pulverizing chamber by the high-speed airflow ejected from the nozzle. The micro powder particles rotate at a very high speed under the high-speed airflow ejected from the nozzle, performing a circular motion. The particles collide and rub against each other and against the inner wall of the pulverizing chamber, thereby achieving the purpose of pulverization.

[0100] (3) The mixed micro-powder particles after air flow pulverization are sent to a flame high-temperature spheroidizing furnace, and the heat generated by the high-temperature flame softens and melts the surface of the manganese oxide powder. The high-temperature flame and the manganese oxide powder are fully in contact for about 0.5 seconds. The flame temperature of the spheroidizing furnace is 1900° C. Under the action of surface tension, the mixed micro-powder particles are formed into a spherical shape, and then rapidly cooled. Finally, a spherical weighting material with a coarse particle size is collected by a micro-powder collecting device;

[0101] (4) The density of the prepared spherical weighting agent with a coarse particle size is 4.7 g / cm 3 The particle size distribution D50 is 12.0μm and D90 is 19.0μm. The scanning electron microscope photo is shown in Figure 3 shown.

[0102] Experimental example

[0103] Indoor cement slurry test

[0104] For the prepared weighted stabilizer, the cement slurry performance test is as follows:

[0105] The cement slurry performance test is carried out in accordance with GB / T 19139-2012 "Test Methods for Oil Well Cement". (The cement slurry preparation is carried out in accordance with Chapter 5 of GB / T 19139-2012, and the stability test is carried out in accordance with 6.4 of GB / T 19139-2012)

[0106] (1) Comparative test of manganese oxide cement slurry systems with different processes

[0107] Cement slurry formula: oil well G grade cement + 15% embodiment weighting agent + 35% high temperature strength stabilizer microsilicon + 90% iron ore powder weighting agent HW-1S + 3% filler active silicon dioxide CEA-1 + 0.5% oil well cement anti-gas channeling agent latex fiber mixture FLOK-2 + water + 3.5% fluid loss reducer sulfonated styrene resin HX-11L + 2% retarder vinyl acrylamide polymer HX-36L + 2% drag reducer naphthaldehyde sulfonated resin HX-21L + 2.5% salt + 0.5% suspending agent polyethylene macromolecular polymer O-SP + 0.2% defoaming agent silicone ether copolymer DF-A.

[0108] Experimental conditions: 135℃*86MPa*69min (constant temperature 30min), cement slurry density: 2.45g / cm 3 .

[0109] The experimental results are shown in Table 1.

[0110] Table 1 Cement slurry properties

[0111]

[0112] The fluidity photograph of the micron-sized non-spherical manganese oxide prepared in Comparative Example 1 is as follows: Figure 4 As shown, the fluidity photograph of the micron-sized spherical manganese oxide prepared in Example 1 of the present invention is as follows Figure 5 shown.

[0113] From the comparative test results of spherical and non-spherical manganese oxide prepared by different processes in the same cement slurry system in Table 1, it can be seen that when the cement slurry density is the same and the formula is basically the same (except for the weighting material), the rheology, fluidity and sedimentation stability of the high-density cement slurry prepared with spherical manganese oxide are significantly better than those of the high-density cement slurry system prepared with non-spherical manganese oxide.

[0114] (2) Comparative test of different dosages

[0115] Cement slurry formula: oil well G grade cement + Example 1 spherical weighting agent + 35% high temperature strength stabilizer microsilicon + iron ore powder weighting agent HW-1S + 3% filler active silicon dioxide CEA-1 + 0.5% oil well cement anti-gas channeling agent latex fiber mixture FLOK-2 + water + 3.5% fluid loss reducer sulfonated styrene resin HX-11L + 2% retarder vinyl acrylamide polymer HX-36L + 2% drag reducer naphthaldehyde sulfonated resin HX-21L + 2.5% salt + 0.5% suspending agent polyethylene macromolecular polymer O-SP + 0.2% defoaming agent silicone ether copolymer DF-A.

[0116] Experimental conditions: 135℃*86MPa*69min (constant temperature 30min), cement slurry density: 2.45g / cm 3 .

[0117] The experimental results are shown in Table 2.

[0118] Table 2 Cement slurry properties

[0119]

[0120] It can be seen from Table 2 that in a high-density cement slurry system with the same density and basically the same formula, the comparative test results of different addition amounts of spherical manganese oxide prepared in Example 1 show that as the addition amount of spherical manganese oxide increases, the rheology, fluidity and sedimentation stability of the prepared high-density cement slurry have a significantly improved trend.

[0121] (3) Comparative test of high-density cement slurry at different experimental temperatures

[0122] Cement slurry formula: oil well G grade cement + 15% Example 4 weighting agent + 35% high temperature strength stabilizer microsilicon + 90% iron ore powder weighting agent HW-1S + 3% filler active silicon dioxide CEA-1 + 0.5% oil well cement anti-gas channeling agent latex fiber mixture FLOK-2 + water + 3.5% fluid loss reducer sulfonated styrene resin HX-11L + 2% retarder vinyl acrylamide polymer HX-36L + 2% drag reducer naphthaldehyde sulfonated resin HX-21L + 2.5% salt + 0.5% suspending agent polyethylene macromolecular polymer O-SP + 0.2% defoaming agent silicone ether copolymer DF-A.

[0123] Experimental conditions: 135 / 140 / 150℃*86MPa*69min (constant temperature 30min), cement slurry density: 2.45g / cm 3 The experimental results are shown in Table 3.

[0124] Table 3 Cement slurry properties

[0125]

[0126]

[0127] It can be seen from Table 3 that in a high-density cement slurry system with the same density and basically the same formula, the spherical manganese oxide prepared by the process of Example 4 and cured under high temperature experimental conditions of 135°C-150°C basically do not affect the rheology, fluidity and sedimentation stability of the cement slurry system.

[0128] (4) Comparative test of cement slurries with different densities

[0129] Cement slurry formula: oil well G grade cement + Example 1 weighting agent + 35% high temperature strength stabilizer microsilicon + iron ore powder weighting agent HW-1S + 3% filler active silicon dioxide CEA-1 + 0.5% oil well cement anti-gas channeling agent latex fiber mixture FLOK-2 + water + 3.5% fluid loss reducer sulfonated styrene resin HX-11L + 2% retarder vinyl acrylamide polymer HX-36L + 2% drag reducer naphthaldehyde sulfonated resin HX-21L + 2.5% salt + 0.5% suspending agent polyethylene macromolecular polymer O-SP + 0.2% defoaming agent silicone ether copolymer DF-A.

[0130] Experimental conditions: 135℃*86MPa*69min (constant temperature 30min), cement slurry density: 2.45g / cm 3 The experimental results are shown in Table 4.

[0131] Table 4 Cement slurry properties

[0132]

[0133] It can be seen from Table 4 that with the increase of the density of the spherical manganese oxide system in Example 1, the fluidity index n value of the cement slurry decreases and the consistency coefficient K increases, which is mainly attributed to the decrease in the water-solid ratio of the system. Properly increasing the amount of spherical manganese oxide and the amount of water can make the comprehensive properties of the cement slurry easier to adjust.

[0134] It can be seen from the above data table that the high-density cement slurry for oil and gas well cementing provided by the present invention has a maximum density of 2.45 g / cm at ultra-high temperature of 135°C-150°C. 3 The sedimentation stability of ultrafine spherical manganese oxide is better than that of non-spherical weighting agent and can be controlled at 0.04g / cm 3 Ultrafine spherical manganese oxide can significantly improve the suspension capacity of drilling fluid and improve the rheological properties of high-density cement slurry system; while the rheological properties of high-density cement slurry system with non-spherical manganese oxide or coarse-grained manganese oxide are still very poor. Ultra-high-density cement slurry has good rheological properties, water loss reduction, sedimentation stability and adjustable thickening time, which can meet the requirements of cement slurry cementing operations in deep well and ultra-deep well cementing environment. The results of scanning electron microscopy (SEM) and other tests show that micro-manganese is small and uniform, which not only reduces the friction of drilling fluid, but also has strong Brownian motion in the drilling fluid, which reduces the sedimentation caused by gravity.

[0135] The above is only a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not deviate from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.

Claims

1. An ultrafine spherical manganese oxide, characterized in that: The ultrafine spherical manganese oxide is obtained by subjecting ultrafine manganese oxide powder modified by a surface modifier to high-temperature spheroidization; The modification refers to mixing the surface modifier with the ultrafine manganese oxide powder so that the modifier is uniformly adsorbed on the surface of the ultrafine manganese oxide powder.

2. A method for preparing the ultrafine spherical manganese oxide according to claim 1, characterized in that: The following steps are involved: S1, removing impurities and drying manganese oxide powder; S2, air flow ultrafine grinding of manganese oxide powder; S3, classifying the manganese oxide powder after the airflow ultrafine grinding to obtain ultrafine manganese oxide powder; S4, mixing and stirring the surface modifier with the classified ultrafine manganese oxide powder to obtain the surface-modified ultrafine manganese oxide powder; S5. The surface-modified ultrafine manganese oxide powder is fed into a spheroidizing device, and spheroidized in a high-temperature spheroidizing furnace to obtain ultrafine spherical manganese oxide powder.

3. The method according to claim 2, characterized in that: Also includes step S0; S0, manganese oxide powder raw material selection, the manganese oxide powder Mn content ≥ 65%, density ≥ 4.6g / cm 3 .

4. The method according to claim 2, characterized in that: The manganese oxide powder is a mixture of one or more of manganese monoxide, manganese dioxide, dimanganese trioxide and trimanganese tetraoxide.

5. The method according to claim 2, characterized in that: The surface modifier includes but is not limited to any one of coupling agents such as γ-methacryloxypropyltrimethoxysilane, di(octylphenol polyoxyethylene ether) phosphite, quaternary ammonium salts, and polyoxyethylene ether surfactants; and / or The mixing ratio of the surface modifier to the classified ultrafine manganese oxide powder is 0.5 to 2:

100.

6. The method according to claim 2, characterized in that: The step S1 is specifically as follows: The manganese oxide powder is put into a decontamination tank, and a 0.1 mol / L to 1.0 mol / L chelating agent aqueous solution is added to remove the soluble alkaline earth metal in the manganese oxide powder. The manganese oxide powder is then dried and sent for inspection to obtain manganese oxide powder that meets the requirements.

7. The method according to claim 2, characterized in that: The complexing agent in step S1 is a mixture of one or more of ethylenediaminetetraacetic acid disodium, ethylenediaminetetramethylenephosphine sodium salt, AA / AMPS polymer, and hydroxyethylidene diphosphine sodium salt; and / or The amount of complexing agent added is 0.02% to 0.3% based on the mass of manganese oxide powder.

8. The method according to claim 2, characterized in that: In the step S3, the particle size D50 of the classified ultrafine manganese oxide powder is 3.0 μm to 5.5 μm, and the particle size D90 is 10.0 μm to 20.0 μm.

9. The method according to claim 2, characterized in that: During the spheroidization of manganese oxide powder in S5, the flame temperature of the spheroidizing furnace is 1600°C to 2200°C.

10. Use of the ultrafine spherical manganese oxide according to claim 1, or the ultrafine spherical manganese oxide prepared by the method according to any one of claims 2 to 9, in drilling fluid and cement slurry.

Citation Information

Cited By