High-workability low-carbon cementing material concrete

By using composite solid waste gelling materials and stone powder in concrete, combined with fly ash and silica fume, the problems of concrete and ease and strength under high mud content are solved, and high and easy and low carbon are achieved. Gelatinous material concrete.

CN118908653APending Publication Date: 2024-11-08CHONGQING HUAXI YITONG CONSTR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410964839.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

When the coarse and fine aggregates have high mud content, their sludge content is affected, resulting in difficulty in meeting the requirements.

Method used

Use composite solid waste gelling materials and stone powder to reduce the amount of silicate cement, form gelling materials by grinding steel slag, slag and desulfurization gypsum, and add stone powder to the formula, and combine fly ash and silica fume to optimize the particle shape and Surface characteristics to improve the flowability and strength of concrete.

Benefits of technology

It significantly improves the and ease of concrete, reduces the adverse effects of aggregate mud content on and ease of ease of aggregate, improves the strength performance of concrete, and reduces carbon emissions from cement production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004951443480000051
    Figure BDA0004951443480000051
  • Figure BDA0004951443480000052
    Figure BDA0004951443480000052
  • Figure BDA0004951443480000061
    Figure BDA0004951443480000061
Patent Text Reader

Abstract

The invention relates to the technical field of concrete, and particularly discloses high-workability low-carbon cementing material concrete. According to the invention, while the composite solid waste cementing material is introduced, the workability of the concrete is improved by utilizing the cooperation between each component in the composite solid waste cementing material and the stone powder, the adverse effect of the mud content of coarse and fine aggregates on the workability of the concrete is reduced, and the strength performance of the concrete is fully improved. In addition, due to the use of the composite solid waste cementing material, the use amount of Portland cement is reduced, the dependence of concrete production on Portland cement is reduced, and the problem of carbon emission caused by cement production is relieved while industrial solid waste is consumed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of concrete, and more particularly to a low-carbon cementitious material concrete with high workability. Background Art

[0002] Concrete is an important building material, mainly composed of cement, fine aggregate, coarse aggregate, water and admixtures added when necessary. It is widely used in many fields such as building structures, roads and bridges, water conservancy projects, and marine engineering. Workability refers to the performance of concrete mixtures that facilitate construction operations under corresponding engineering conditions and can obtain uniform and dense concrete. In order to ensure the quality of concrete and meet the design requirements for strength and durability, the premise is that workability must meet the requirements. In other words, if the workability of concrete does not meet the requirements, then it is difficult to meet the requirements for strength and durability.

[0003] In the related art, there is a concrete comprising the following raw material components by weight: 300 parts of Portland cement, 100 parts of mineral admixture, 1300 parts of coarse aggregate, 800 parts of fine aggregate, 140 parts of water, and 4.2 parts of polycarboxylate water reducer. The mineral admixture is fly ash, the coarse aggregate is 5-31.5 mm continuously graded crushed stone, and the fine aggregate is river sand.

[0004] With respect to the above-mentioned related technologies, the inventors believe that in the related technologies, crushed stone is selected as coarse aggregate and river sand is selected as fine aggregate. When the mud content of these two materials is high, the workability of concrete will be greatly affected, resulting in the difficulty of concrete having good strength performance. Summary of the invention

[0005] In the related art, when the mud content of coarse and fine aggregates is high, the workability of concrete will be greatly affected, resulting in the concrete being difficult to have good strength properties. In order to improve this defect, the present application provides a low-carbon cementitious material concrete with high workability.

[0006] The present application provides a low-carbon cementitious material concrete with high workability, which adopts the following technical solution: A low-carbon cementitious material concrete with high workability is made from the following raw materials in parts by weight: 80-120 parts of silicate cement, 220-240 parts of composite solid waste cementitious material, 100-120 parts of mineral admixture, 1300-1400 parts of coarse aggregate, 800-840 parts of fine aggregate, 40-48 parts of stone powder, 140-150 parts of water, and 4-4.8 parts of polycarboxylate water reducer; the composite solid waste cementitious material is made by grinding industrial solid waste, and the industrial solid waste includes 30-40wt% of steel slag, 48-62wt% of slag and 8-12wt% of desulfurized gypsum.

[0007] By adopting the above technical scheme, the present application grinds steel slag, slag and desulfurized gypsum and mixes them to obtain a composite solid waste cementitious material, and uses the composite solid waste cementitious material and silicate cement as cementitious materials together, and also adds stone powder to the formula. In the scheme of the present application, on the one hand, the grinding products of slag, steel slag and desulfurized gypsum are used together as cementitious materials, which reduces the amount of silicate cement, reduces the dependence of concrete production on silicate cement, and alleviates the carbon emission problem caused by cement production while consuming industrial solid waste. On the other hand, the steel slag grinding product has an ideal particle morphology and surface characteristics, the slag grinding product has a water-reducing effect and a suitable density, and the desulfurized gypsum grinding product has a regulating effect on the cement hydration rate. In addition, the stone powder selected in the present application plays a role in filling pores and producing a ball effect in concrete. Under the synergistic effect of these factors, the workability of concrete has been significantly improved, reducing the adverse effects of the mud content of coarse and fine aggregates on workability, which helps to fully improve the strength performance of concrete.

[0008] Preferably, the average particle size of the stone powder is 10-30 μm.

[0009] By adopting the above technical solution, the present application optimizes the average particle size of the stone powder, making the particle size of the stone powder close to the particle size of silicate cement, which helps to give full play to the ball effect of the stone powder and improve the workability of the concrete.

[0010] Preferably, the mineral admixture includes at least one of fly ash and silica fume.

[0011] By adopting the above technical solution, the present application optimizes the type of mineral admixtures. The spherical glass contained in fly ash has a smooth surface without edges and corners, stable performance, and can reduce the friction inside the concrete; the particle size of silica fume is smaller than that of cement and fly ash, which can improve the gradation of concrete. By using at least one of fly ash and silica fume to cooperate with stone powder, a synergistic effect can be produced, which helps to improve the workability of concrete.

[0012] Preferably, the fineness of the fly ash (residue on a 45 μm square sieve) is 5-8%.

[0013] By adopting the above technical solution, the present application optimizes the fineness range of fly ash, which helps to improve the workability of concrete.

[0014] Preferably, the specific surface area of ​​the silica fume is 18500-20000m 2 / kg.

[0015] By adopting the above technical solution, the present application optimizes the specific surface area range of silica fume, which helps to improve the workability of concrete.

[0016] Preferably, the concrete component also includes methoxy polyether.

[0017] By adopting the above technical solution, methoxy polyether has good bonding with clay-like substances. By adding methoxy polyether into concrete, methoxy polyether can replace polycarboxylate water reducer to adsorb with soil particles and stone powder, so that polycarboxylate water reducer can fully exert its water-reducing effect, which helps to improve the workability of concrete.

[0018] Preferably, the average molecular weight of the methoxy polyether is 1000-2000.

[0019] By adopting the above technical solution, the present application optimizes the average molecular weight of methoxy polyether, which helps to improve the workability of concrete.

[0020] Preferably, the weight ratio of the methoxy polyether to the polycarboxylic acid water-reducing agent is (1.8-3.2):1.

[0021] By adopting the above technical solution, the present application optimizes the usage ratio of methoxy polyether and polycarboxylic acid water reducer, which helps to improve the workability of concrete.

[0022] Preferably, the stone powder includes modified stone powder, and the modified stone powder is prepared according to the following method: (1) mixing silane coupling agent KH570, water and ethanol to obtain a silane-modified liquid; in this step, the silane coupling agent contains a vinyl group in its molecule; (2) mixing granite powder with silane-modified liquid, heating and filtering to obtain silane-treated stone powder; (3) Mixing silane-treated stone powder, water, an initiator and acrylic acid, reacting them under heating conditions, and then filtering them. Drying and sieving the obtained filter residue to obtain modified stone powder.

[0023] By adopting the above technical solution, the present application first uses silane coupling agent KH570 to treat granite powder, introduces carbon-carbon double bonds on the surface of granite powder, and obtains silane-treated stone powder. Then, under the action of an initiator, the carbon-carbon double bonds on the surface of the silane-treated stone powder and acrylic acid undergo cross-copolymerization to obtain modified stone powder with polyacrylic acid groups on the surface. By adding the above-mentioned modified stone powder, the polyacrylic acid groups can reduce the adsorption of polycarboxylic acid water reducer through electrostatic repulsion, so that the polycarboxylic acid water reducer can be more fully combined with cement particles, which helps to improve the workability of concrete.

[0024] Preferably, the molar ratio of the acrylic acid to the silane coupling agent KH570 is (4.7-6.4):1.

[0025] By adopting the above technical solution, the present application optimizes the molar ratio of acrylic acid and silane coupling agent KH570, which helps to improve the workability of concrete.

[0026] In summary, this application has the following beneficial effects: 1. While introducing the composite solid waste cementitious material, the present application utilizes the combination of the components in the composite solid waste cementitious material and the stone powder to improve the workability of the concrete, reduce the adverse effects of the mud content of coarse and fine aggregates on the workability of the concrete, and help to fully improve the strength performance of the concrete.

[0027] 2. The use of composite solid waste cementitious materials reduces the use of silicate cement, reduces the dependence of concrete production on silicate cement, and alleviates the carbon emission problem caused by cement production while consuming industrial solid waste. DETAILED DESCRIPTION

[0028] The present application is further described in detail below in conjunction with embodiments, preparation examples and comparative examples. The raw materials involved in the present application can all be obtained commercially.

[0029] Preparation example of modified stone powder The following is an explanation using Preparation Example 1.

[0030] Preparation Example 1 In this preparation example, the modified stone powder was prepared according to the following method: (1) mixing silane coupling agent KH570, water and ethanol in a weight ratio of 1:6:2 to obtain a silane modified liquid; (2) mixing granite powder with silane-modified liquid, heating at 75° C. for 2 h, filtering to obtain filter residue, and drying the filter residue at 105° C. to obtain silane-treated stone powder; in this step, the weight of silane coupling agent KH570 in the silane-modified liquid is 2% of the weight of the granite powder; (3) Mixing silane-treated stone powder, water, initiator and acrylic acid, heating at 65° C. for 1.5 h, and then filtering and drying to obtain modified stone powder; in this step, the initiator is azobisisobutyramidine hydrochloride, and the amount of the initiator is 2% of the weight of the silane-treated stone powder. The molar ratio of acrylic acid consumed in this step to the vinyltriethoxysilane used in step (1) is 2.2:1.

[0031] As shown in Table 1, the difference between Preparation Examples 1-5 is that the molar ratio between acrylic acid and silane coupling agent KH570 is different.

[0032] Table 1 Molar ratio between acrylic acid and silane coupling agent KH570 sample Molar Ratio Preparation Example 1 2.2:1 Preparation Example 2 3.6:1 Preparation Example 3 4.7:1 Preparation Example 4 5.5:1 Preparation Example 5 6.4:1 Example

[0033] Examples 1-5 The following description is given by taking Example 1 as an example.

[0034] Example 1 This embodiment provides a low-carbon cementitious material concrete with high workability, and the raw material formula is: 80kg of silicate cement, 220kg of composite solid waste cementitious material, 100kg of mineral admixture, 1300kg of coarse aggregate, 800kg of fine aggregate, 42kg of stone powder, 140kg of water, and 4.2kg of polycarboxylate water reducer. The silicate cement is P.O42.5 silicate cement, and the composite solid waste cementitious material is made by mixing and grinding steel slag, slag and desulfurized gypsum; the mineral admixture is fly ash, and the fineness of the fly ash (45μm square hole sieve residue) is 10%; the coarse aggregate is 5-31.5mm continuously graded crushed stone, the mud content of the coarse aggregate is 3.8%, and the mud content is 1.1%; the fine aggregate is river sand with a fineness modulus of 2.7, the mud content of the fine aggregate is 4.5%, and the mud content is 0.6%; the stone powder is granite stone powder with an average particle size of 5μm, and the water reduction rate of the polycarboxylic acid water reducer is 27%.

[0035] Among the raw materials of the above-mentioned composite solid waste cementitious materials, the steel slag is converter steel slag, the hydration activity coefficient (HAI) of the steel slag is 0.38, the alkalinity and f-CaO content meet the requirements of GB / T 0491-2017 "Steel Slag Powder for Cement and Concrete", and the 7d activity index of the steel slag after grinding alone is 66.8%, and the 28d activity index is 79.2; the alkalinity coefficient M0 of the slag is 1.035, the quality coefficient K is 2.147, and the activity index M a is 0.582; the content of dihydrate gypsum in desulfurized gypsum is 97%.

[0036] The composite solid waste cementitious material is prepared according to the following steps: The steel slag and slag were crushed by jaw crusher, and the desulfurized gypsum was dried at 105℃ for 24h. Then, the crushed products of steel slag, slag and desulfurized gypsum were ball milled by SMφ500mm×500mm ball mill to obtain a specific surface area of ​​455m 2 / kg of steel slag powder, with a specific surface area of ​​428m 2 / kg of slag powder and a specific surface area of ​​318m 2 / kg of desulfurized gypsum powder, steel slag powder, slag powder and desulfurized gypsum powder are mixed in a weight ratio of 30%, 62% and 8% to obtain a composite solid waste cementitious material.

[0037] The high-workability low-carbon cementitious material concrete in this embodiment is constructed in accordance with the method described in Section 6.4 "Concrete Construction" of the "TB10424-2018 Railway Concrete Engineering Construction Quality Acceptance Standard".

[0038] As shown in Table 2, the differences between Examples 1-5 mainly lie in the different raw material ratios of concrete and the composition of the composite solid waste cementitious material.

[0039] Table 2 Ratio of raw materials for concrete and composition of composite solid waste cementitious materials As shown in Table 3, the difference between Examples 5-9 is that the average particle size of the stone powder is different.

[0040] Table 3 Example 10 The difference between this embodiment and embodiment 7 is that the mineral admixture is a mixture of fly ash and silica ash in a weight ratio of 2:1, and the specific surface area of ​​the silica ash is 16000m 2 / kg.

[0041] As shown in Table 4, the difference between Examples 10-14 is that the fineness of the fly ash (residue on a 45 μm square sieve) is different.

[0042] Table 4 Fly ash fineness sample Fineness / % Example 10 10 Embodiment 11 9 Example 12 8 Embodiment 13 6 Embodiment 14 5 As shown in Table 5, the difference between Examples 14-18 is that the specific surface areas of silica fume are different.

[0043] Table 5 Specific surface area of ​​silica fume sample <![CDATA[Specific surface area of silica fume / m 2 / kg]]> Embodiment 14 16000 Embodiment 15 17000 Example 16 18500 Embodiment 17 19200 Embodiment 18 20000 Embodiment 19 The difference between this embodiment and embodiment 8 is that the components of the concrete further include methoxy polyether (MPEG), the average molecular weight of the methoxy polyether is 600, and the weight ratio of the methoxy polyether to the polycarboxylate water reducer is 1:1.

[0044] As shown in Table 6, the difference between Examples 19-23 is that the average molecular weight of the methoxy polyether is different.

[0045] Table 6 sample Average molecular weight of methoxy polyether Embodiment 19 600 Embodiment 20 750 Embodiment 21 1000 Embodiment 22 1200 Embodiment 23 2000 As shown in Table 7, the difference between Examples 23-27 is that the weight ratio of methoxy polyether to polycarboxylate water reducer (abbreviated as MPEG:ad) is different.

[0046] Table 7 Weight ratio of methoxy polyether to polycarboxylate water reducer sample MPEG:ad Embodiment 23 1:1 Embodiment 24 1.4:1 Embodiment 25 1.8:1 Embodiment 26 2.6:1 Embodiment 27 3.2:1 Embodiment 28 The difference between this embodiment and Example 27 is that the stone powder is the modified stone powder of Preparation Example 1.

[0047] As shown in Table 8, the difference between Examples 28-32 is that the preparation examples of modified stone powder are different.

[0048] Table 8 Preparation example of modified stone powder sample Preparation Example Embodiment 28 Preparation Example 1 Embodiment 29 Preparation Example 2 Embodiment 30 Preparation Example 3 Embodiment 31 Preparation Example 4 Embodiment 32 Preparation Example 5 Comparative Example Comparative Example 1 A concrete comprises the following raw material components: 300kg of silicate cement, 100kg of mineral admixture, 1300kg of coarse aggregate, 800kg of fine aggregate, 140kg of water, and 4.2kg of polycarboxylate water reducer. The mineral admixture is fly ash, the coarse aggregate is 5-31.5mm continuously graded crushed stone, and the fine aggregate is river sand. The silicate cement is P.O42.5 silicate cement; the mineral admixture is fly ash, and the fineness of the fly ash (45μm square hole sieve residue) is 10%; the coarse aggregate is 5-31.5mm continuously graded crushed stone, the mud content of the coarse aggregate is 3.8%, and the mud block content is 1.1%; the fine aggregate is river sand with a fineness modulus of 2.7, the mud content of the fine aggregate is 4.5%, and the mud block content is 0.6%; the water reduction rate of the polycarboxylate water reducer is 27%.

[0049] Comparative Example 2 The difference between this comparative example and Example 1 is that the raw material components of the concrete do not include stone powder.

[0050] Comparative Example 3 The difference between this comparative example and Example 1 is that the composite solid waste cementitious material is replaced by P.O42.5 silicate cement.

[0051] Comparative Example 4 The difference between this comparative example and comparative example 1 is that the coarse and fine aggregates are cleaned and screened (using a 0.075 mm sieve) before use. After screening, the mud content and mud block content of the coarse aggregate are both 0; the mud content of the fine aggregate is 0.1%, and the mud block content is 0.

[0052] Performance testing methods 1. Workability Evaluation The slump expansion of concrete is used as the evaluation standard for workability. Due to the influence of the mud content of aggregate, the workability of concrete deteriorates and the fluidity decreases. Therefore, enhanced fluidity is used as the standard for improving workability.

[0053] The detection method steps are as follows: 1. Preparation stage: Ensure that the slump cone, base plate and tamping rod comply with the requirements of Concrete Slump Tester (JG / T 248). Place the base plate on a solid horizontal surface and mark concentric circles, including the center position and circles with diameters of 200mm, 300mm, 500mm, 600mm, 700mm, 800mm and 900mm respectively.

[0054] 2. Wetting and placing the slump cone: Wet the base plate and slump cone with a sponge or towel, and make sure there is no visible water on the inner wall of the slump cone and the base plate. Place the slump cone in the center of the base plate, with the lower edge coinciding with the 200mm scale circle.

[0055] 3. Loading: The concrete mixture should be evenly loaded into the slump cylinder in three layers. Each layer should be evenly tamped 25 times in a spiral shape from the edge to the center with a tamping rod. After the top layer is loaded, remove the loading funnel, scrape off the excess concrete mixture, and smooth it along the cylinder mouth.

[0056] 4. Lift the slump cone: remove the excess concrete around the chassis, and then quickly lift the slump cone upward in the vertical direction to a height of 300mm at a uniform speed.

[0057] 5. Measurement: Determine the time required for the concrete to expand to the 500mm mark (T500), starting from the moment the collapse cone is lifted off the bottom plate, accurate to 0.1 second.

[0058] The test was repeated 5 times for each group, and the average value of the 5 measurements was recorded as the expansion time.

[0059] Taking the expansion time of comparative example 1 as a benchmark, the ratio between the expansion time measured in each embodiment and comparative example and the expansion time of comparative example 1 was calculated, and the ratio was recorded as the relative expansion time. The results are shown in Table 9.

[0060] 2. Strength evaluation With reference to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", the 90d compressive strength of the concrete in each embodiment and comparative example was tested, and the compressive strength of Comparative Example 1 was used as a benchmark to calculate the ratio between the compressive strength measured in each embodiment and comparative example and the compressive strength of Comparative Example 1, and the ratio was recorded as relative strength. The results are shown in Table 9.

[0061] Table 9 Test results Combining Examples 1-5 and Comparative Example 1 and Table 9, it can be seen that the relative expansion time measured in Examples 1-9 is less than that in Comparative Example 1, while the relative strength is greater than that in Comparative Example 1, indicating that the concrete of the present application can fully improve the workability of concrete and improve the strength performance of concrete even when the mud content of coarse and fine aggregates is high, and to a certain extent overcomes the adverse effects of the mud content of aggregates on the performance of concrete.

[0062] From Example 1 and Comparative Examples 2-3 and Table 9, it can be seen that when the composite solid waste cementitious material of the present application is not used in combination with stone powder, the influence of the mud content of the aggregate is still quite obvious, the rheology of the concrete is difficult to be improved sufficiently, and the strength of the concrete is relatively low.

[0063] Combining Comparative Example 1 and Comparative Example 4 with Table 9, it can be seen that after removing the soil particles in the aggregate by washing and screening, the rheology of the concrete is greatly improved and the strength is also greatly improved, indicating that the soil particles in the aggregate are the key factors affecting the rheology and strength properties of the concrete in Comparative Example 1. However, considering the high cost of washing and screening operations, it is still difficult to apply in actual production.

[0064] It can be seen from Examples 5-9 and Table 9 that when the average particle size of the stone powder is in the range of 10-30 μm, the rheology of the concrete is better and the strength is higher.

[0065] It can be seen from Example 9, Examples 10-14 and Table 9 that the use of fly ash and silica fume as mineral admixtures can further improve the rheology of concrete and help improve the strength of concrete. Moreover, when the fineness of fly ash (45 μm square hole sieve residue) is 5-8%, the rheology of concrete is better and the strength is higher.

[0066] Combining Examples 14-18 and Table 9, it can be seen that when the specific surface area of ​​silica fume is 18500-20000m 2 / kg, the workability of concrete can be greatly improved and the strength performance can also be greatly improved.

[0067] It can be seen from Example 18, Examples 19-23 and Table 9 that the addition of methoxy polyether further improves the workability of concrete and increases the strength of concrete. When the average molecular weight of methoxy polyether is 1000-2000, the workability and compressive strength of concrete can be well improved.

[0068] It can be seen from Examples 23-27 and Table 9 that when the weight ratio of methoxy polyether to polycarboxylate water-reducing agent is (1.8-3.2):1, the workability and compressive strength of concrete can be well improved.

[0069] It can be seen from Example 27, Examples 28-32 and Table 9 that when the stone powder is modified stone powder, the workability and compressive strength of the concrete can be further improved. Among them, when the molar ratio between acrylic acid and silane coupling agent KH570 is (4.7-6.4):1, the test results of the workability and compressive strength of the concrete are more ideal.

[0070] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A low-carbon cementitious material concrete with high workability, characterized in that: The composite solid waste cementitious material is made of the following raw materials in parts by weight: 80-120 parts of silicate cement, 220-240 parts of composite solid waste cementitious material, 100-120 parts of mineral admixture, 1300-1400 parts of coarse aggregate, 800-840 parts of fine aggregate, 40-48 parts of stone powder, 140-150 parts of water, and 4-4.8 parts of polycarboxylic acid water reducer; the composite solid waste cementitious material is made by grinding industrial solid waste, and the industrial solid waste includes 30-40wt% of steel slag, 48-62wt% of slag and 8-12wt% of desulfurized gypsum.

2. The high-workability low-carbon cementitious material concrete according to claim 1, characterized in that: The average particle size of the stone powder is 10-30 μm.

3. The high workability low carbon cementitious material concrete according to claim 2, characterized in that: The mineral admixture includes at least one of fly ash and silica fume.

4. The high workability low carbon cementitious material concrete according to claim 3, characterized in that: The fineness of the fly ash (residue on a 45 μm square sieve) is 5-8%.

5. The high workability low carbon cementitious material concrete according to claim 3, characterized in that: The specific surface area of ​​the silica fume is 18500-20000m 2 / kg.

6. The high workability low carbon cementitious material concrete according to claim 2, characterized in that: The concrete also includes methoxy polyether as a component.

7. The high workability low carbon cementitious material concrete according to claim 6, characterized in that: The average molecular weight of the methoxy polyether is 1000-2000.

8. The high-workability low-carbon cementitious material concrete according to claim 7, characterized in that: The weight ratio of the methoxy polyether to the polycarboxylic acid water reducer is (1.8-3.2):

1.

9. The high workability low carbon cementitious material concrete according to claim 1, characterized in that: The stone powder includes modified stone powder, and the modified stone powder is prepared according to the following method: (1) mixing silane coupling agent KH570, water and ethanol to obtain a silane-modified liquid; in this step, the silane coupling agent contains a vinyl group in its molecule; (2) mixing granite powder with silane-modified liquid, heating and filtering to obtain silane-treated stone powder; (3) Mixing silane-treated stone powder, water, an initiator and acrylic acid, reacting them under heating conditions, and then filtering them. Drying and sieving the obtained filter residue to obtain modified stone powder.

10. The high-workability low-carbon cementitious material concrete according to claim 9, characterized in that: The molar ratio between the acrylic acid and the silane coupling agent KH570 is (4.7-6.4):1.