Basalt composite fiber water permeable brick and preparation method thereof

By using basalt composite fibers and modified pyrite slag in permeable bricks, a three-dimensional structure is constructed to improve compressive strength and adsorption capacity, the problem of insufficient adsorption of existing permeable bricks in load bearing heavy pressure and heavy metals is solved, and the further development is achieved. Efficient water purification effect.

CN118908660AInactive Publication Date: 2024-11-08陈全
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411025534.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing permeable bricks are insufficient in bearing heavy pressure and have poor adsorption of heavy metals in rainwater, making it difficult to effectively reduce groundwater pollution.

Method used

Using basalt composite fibers and modified pyrite slag, a three-dimensional spatial structure is constructed through chitosan, polyethyleneimine and crosslinking agent, which increases the adsorption effect on heavy metals, and improves the resistance of permeable bricks through materials such as silicate cement. Pressure strength and water permeability.

Benefits of technology

It significantly improves the compressive strength and water permeability of permeable bricks, and effectively absorbs heavy metal elements in rainwater, improving the water quality environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004968556750000071
    Figure BDA0004968556750000071
Patent Text Reader

Abstract

The invention relates to the technical field of water permeable bricks, in particular to a basalt composite fiber water permeable brick and a preparation method thereof. Adding the modified pyrite slag, basalt composite fiber, fly ash, coarse aggregate and fine aggregate in parts by mass, uniformly mixing, adding a small amount of water and a water reducing agent, and uniformly stirring to obtain a primary mixture; adding the Portland cement, the exciting agent, the residual water reducing agent and the water into the primary mixture, and uniformly stirring to obtain a secondary mixture; putting the secondary mixture into a water permeable brick mold, uniformly inserting and tamping, flattening the surface, and carrying out static pressure molding; the water permeable brick mold obtained after static pressure forming is demolded, and after standing is conducted, water curing is conducted to obtain the water permeable brick. According to the basalt composite fiber water permeable brick adopting the components and the preparation method thereof, the compressive strength and the water permeability of the water permeable brick are improved, and heavy metal elements in rainwater are adsorbed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of permeable bricks, and in particular to a basalt composite fiber permeable brick and a preparation method thereof. Background Art

[0002] Permeable bricks, also known as seepage bricks and drainage bricks, are a kind of building material with high strength and high permeability. They are mainly used in urban roads, squares, parking lots and other places to enhance the permeability of the ground, reduce rainwater runoff, and improve the microclimate and groundwater recharge of the city. This type of brick is made by special technology, and its internal structure contains a large number of interconnected pores, which can quickly penetrate rainwater and store a certain amount of water, which helps to alleviate the urban heat island effect and reduce the pressure on the rainwater collection system.

[0003] When rainwater flows through cities and industrial areas, it may dissolve and carry heavy metal pollutants in the air and on the ground, such as lead, mercury, cadmium, chromium, etc. These heavy metals come from surface pollution sources such as automobile exhaust emissions, industrial wastewater discharge, pesticide and fertilizer use. Once rainwater containing heavy metals enters the water body or infiltrates into the groundwater, it may pollute the water quality.

[0004] Compared with traditional hard paving materials, permeable bricks may be slightly insufficient in bearing heavy pressure, and have poor adsorption of heavy metals in rainwater. A new type of permeable brick is urgently needed. Summary of the invention

[0005] The purpose of the present invention is to provide a basalt composite fiber water-permeable brick and a preparation method thereof, so as to improve the compressive strength and water permeability of the water-permeable brick and adsorb heavy metal elements in rainwater.

[0006] To achieve the above-mentioned purpose, the present invention provides a basalt composite fiber permeable brick and a preparation method thereof, wherein the mass proportions of the components are 50-80 parts of silicate cement, 18-30 parts of basalt composite fiber, 15-25 parts of fly ash, 12-25 parts of coarse aggregate, 12-25 parts of fine aggregate, 12-20 parts of modified pyrite slag, 8-12 parts of water reducer, 1-5 parts of activator and 20-50 parts of water.

[0007] Preferably, the activator comprises one or more of caustic, carbonate, alkali metal hydroxide, silicate and carbonate.

[0008] Preferably, the particle size of the coarse aggregate is in the range of 4.75-9.25 mm.

[0009] Preferably, the particle size of the fine aggregate is in the range of 1.37-4.25 mm.

[0010] The preparation method of the above-mentioned basalt composite fiber permeable brick comprises the following steps:

[0011] S1. preparing modified pyrite slag: adding a dispersant to the pyrite slag and then ball milling, centrifuging and drying, adding deionized water and ultrasonically dispersing to obtain a pyrite slag suspension, adding a sodium hydroxide solution of polyethyleneimine, heating and stirring, slowly adding an acetic acid solution of chitosan, stirring until the mixture is uniform, maintaining the temperature, adding a cross-linking agent for cross-linking reaction, vacuum filtering and washing, and drying to obtain the modified pyrite slag;

[0012] S2, primary mixing: add the modified pyrite slag, basalt composite fiber, fly ash, coarse aggregate and fine aggregate in S1 according to the mass proportion, mix well, add a small amount of water and water reducing agent, stir well to obtain the primary mixture;

[0013] S3, secondary mixing: add silicate cement, activator, remaining water reducing agent and water to the primary mixture in S1, and stir evenly to obtain a secondary mixture;

[0014] S4, static pressure molding: put the secondary mixture in S3 into the permeable brick mold, tamp it evenly, smooth the surface, and static pressure mold it;

[0015] S5. Demould the mold of the permeable brick formed by static pressure in S4, and perform water curing after standing to obtain the permeable brick.

[0016] Preferably, in S1, the dispersant is one or more of ethanol and methanol, and the ball milling conditions are a rotation speed of 200-600 rpm and a time of 6-9 h.

[0017] Preferably, in S1, the heating temperature is 40-60°C, the ultrasonic dispersion conditions are: power 220-500W, time 5-20min,

[0018] Preferably, in S1, the cross-linking agent is one or more of glutaraldehyde, carbodiimide and N-succinimidyl-3-(2-pyridyldithio)-propionate.

[0019] Preferably, in S1, during washing, ethanol and deionized water are used successively for repeated washing.

[0020] Preferably, in S4, the static pressure molding pressure is 2-6 MPa, and the holding time is 45-90 s.

[0021] Therefore, the present invention adopts the above technical solution, and its beneficial effects are:

[0022] 1. The modified pyrite slag provided by the present invention has a three-dimensional structure constructed by coating the pyrite slag with chitosan, polyethyleneimine and a cross-linking agent. The cross-linking agent introduces a complexing group on the surface of the modified pyrite slag to increase the adsorption effect of heavy metals (Cd, Pb, Cu);

[0023] 2. The modified pyrite slag provided by the present invention chelates metal ions in rainwater and sewage through free hydroxyl and amino groups in chitosan and amino groups in polyethyleneimine, thereby increasing the adsorption of heavy metals in rainwater by permeable bricks;

[0024] 3. The present invention enhances the strength, corrosion resistance and high temperature resistance of the permeable brick by adding basalt composite fiber.

[0025] The technical solution of the present invention is further described in detail below through embodiments. DETAILED DESCRIPTION

[0026] The present invention is further described below in conjunction with embodiments. Unless otherwise defined, the technical terms or scientific terms used in the present invention should be the common meanings understood by people with ordinary skills in the field to which the present invention belongs. The above-mentioned features or features mentioned in the specific examples mentioned in the present invention can be combined arbitrarily, and these specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0027] Example 1

[0028] S1. Preparation of modified pyrite slag: Add ethanol dispersant to pyrite slag and then ball mill with a ball-to-material ratio of 6:1. The ball milling conditions are a speed of 500 rpm and a time of 9 hours. After centrifugation, dry in a drying oven at 60°C for 20 hours. Add deionized water and ultrasonically disperse at a power of 500 W for 12 minutes to obtain a pyrite slag suspension.

[0029] Then add 1 mol / L sodium hydroxide solution of polyethyleneimine, heat and stir at 50°C for 50 min, slowly add acetic acid solution of chitosan (dissolve 30 g chitosan powder in 0.5 wt% acetic acid solution) dropwise, and stir until mixed evenly.

[0030] The temperature was maintained, and glutaraldehyde cross-linking agent was added to carry out cross-linking reaction for 7 hours. After vacuum filtration, the mixture was repeatedly washed with ethanol and deionized water in sequence, and dried at 60° C. for 24 hours to obtain modified pyrite slag.

[0031] S2, primary mixing: add 12 parts of modified pyrite slag in S1, 18 parts of basalt composite fiber, 15 parts of fly ash, 12 parts of coarse aggregate and 12 parts of fine aggregate according to mass proportions, mix well, add 8 parts of water and 4 parts of water reducing agent, stir well to obtain a primary mixture.

[0032] S3. Secondary mixing: add 50 parts of Portland cement, 2 parts of activator, the remaining 4 parts of water reducer and 12 parts of water to the primary mixture in S2, and stir evenly to obtain a secondary mixture.

[0033] S4, static pressure molding: put the secondary mixture in S3 into the permeable brick mold, tamp it evenly, smooth the surface, and static pressure molding. The static pressure molding pressure is 3MPa, and the holding time is 60s.

[0034] S5. Demould the mold of the permeable brick formed by static pressure in S4, and perform water curing after standing to obtain the permeable brick.

[0035] Example 2

[0036] S1. Preparation of modified pyrite slag: Add ethanol dispersant to pyrite slag and then ball mill with a ball-to-material ratio of 6:1. The ball milling conditions are a speed of 500 rpm and a time of 9 hours. After centrifugation, dry in a drying oven at 60°C for 20 hours. Add deionized water and ultrasonically disperse at a power of 500 W for 12 minutes to obtain a pyrite slag suspension.

[0037] Then add 1 mol / L sodium hydroxide solution of polyethyleneimine, heat and stir at 50°C for 50 min, slowly add acetic acid solution of chitosan (dissolve 30 g chitosan powder in 0.5 wt% acetic acid solution) dropwise, and stir until mixed evenly.

[0038] The temperature was maintained, and a carbodiimide cross-linking agent was added to carry out a cross-linking reaction for 7 hours. After vacuum filtration, the mixture was repeatedly washed with ethanol and deionized water in sequence, and dried at 60° C. for 24 hours to obtain modified pyrite slag.

[0039] S2, primary mixing: add 20 parts of modified pyrite slag in S1, 30 parts of basalt composite fiber, 25 parts of fly ash, 25 parts of coarse aggregate and 25 parts of fine aggregate according to mass proportions, mix well, then add 20 parts of water and 6 parts of water reducing agent, stir well to obtain a primary mixture.

[0040] S3, secondary mixing: add 80 parts of Portland cement, 5 parts of activator, the remaining 6 parts of water reducer and 30 parts of water to the primary mixture in S2, stir evenly to obtain the secondary mixture.

[0041] S4, static pressure molding: put the secondary mixture in S3 into the permeable brick mold, tamp it evenly, smooth the surface, and static pressure molding. The static pressure molding pressure is 3MPa, and the holding time is 60s.

[0042] S5. Demould the mold of the permeable brick formed by static pressure in S4, and perform water curing after standing to obtain the permeable brick.

[0043] Example 3

[0044] S1. Preparation of modified pyrite slag: Add ethanol dispersant to pyrite slag and then ball mill with a ball-to-material ratio of 6:1. The ball milling conditions are a speed of 500 rpm and a time of 9 hours. After centrifugation, dry in a drying oven at 60°C for 20 hours. Add deionized water and ultrasonically disperse at a power of 500 W for 12 minutes to obtain a pyrite slag suspension.

[0045] Then add 1 mol / L sodium hydroxide solution of polyethyleneimine, heat and stir at 50°C for 50 min, slowly add acetic acid solution of chitosan (dissolve 30 g chitosan powder in 0.5 wt% acetic acid solution) dropwise, and stir until mixed evenly.

[0046] The temperature was maintained, and a carbodiimide cross-linking agent was added to carry out a cross-linking reaction for 7 hours. After vacuum filtration, the mixture was repeatedly washed with ethanol and deionized water in sequence, and dried at 60° C. for 24 hours to obtain modified pyrite slag.

[0047] S2, primary mixing: add 15 parts of modified pyrite slag in S1, 20 parts of basalt composite fiber, 20 parts of fly ash, 20 parts of coarse aggregate and 20 parts of fine aggregate according to mass proportions, mix well, then add 15 parts of water and 5 parts of water reducing agent, stir well to obtain a primary mixture.

[0048] S3, secondary mixing: add 75 parts of Portland cement, 3 parts of activator, the remaining 4 parts of water reducer and 30 parts of water to the primary mixture in S2, stir evenly to obtain the secondary mixture.

[0049] S4, static pressure molding: put the secondary mixture in S3 into the permeable brick mold, tamp it evenly, smooth the surface, and static pressure molding. The static pressure molding pressure is 3MPa, and the holding time is 60s.

[0050] S5. Demould the mold of the permeable brick formed by static pressure in S4, and perform water curing after standing to obtain the permeable brick.

[0051] Example 4

[0052] S1. Preparation of modified pyrite slag: Add ethanol dispersant to pyrite slag and then ball mill with a ball-to-material ratio of 6:1. The ball milling conditions are a speed of 500 rpm and a time of 9 hours. After centrifugation, dry in a drying oven at 60°C for 20 hours. Add deionized water and ultrasonically disperse at a power of 500 W for 12 minutes to obtain a pyrite slag suspension.

[0053] Then add 1 mol / L sodium hydroxide solution of polyethyleneimine, heat and stir at 50°C for 50 min, slowly add acetic acid solution of chitosan (dissolve 30 g chitosan powder in 0.5 wt% acetic acid solution) dropwise, and stir until mixed evenly.

[0054] The temperature was maintained, and glutaraldehyde cross-linking agent was added to carry out cross-linking reaction for 7 hours. After vacuum filtration, the mixture was repeatedly washed with ethanol and deionized water in sequence, and dried at 60° C. for 24 hours to obtain modified pyrite slag.

[0055] S2, primary mixing: add 18 parts of modified pyrite slag in S1, 20 parts of basalt composite fiber, 20 parts of fly ash, 20 parts of coarse aggregate and 20 parts of fine aggregate according to mass proportions, mix well, then add 20 parts of water and 4 parts of water reducing agent, stir well to obtain a primary mixture.

[0056] S3, secondary mixing: add 70 parts of Portland cement, 3 parts of activator, the remaining 6 parts of water reducer and 30 parts of water to the primary mixture in S2, stir evenly to obtain the secondary mixture.

[0057] S4, static pressure molding: put the secondary mixture in S3 into the permeable brick mold, tamp it evenly, smooth the surface, and static pressure molding. The static pressure molding pressure is 3MPa, and the holding time is 60s.

[0058] S5. Demould the mold of the permeable brick formed by static pressure in S4, and perform water curing after standing to obtain the permeable brick.

[0059] Comparative Example 1

[0060] S1. Primary mixing: Add 20 parts of fly ash, 20 parts of coarse aggregate and 20 parts of fine aggregate by mass, mix well, then add 20 parts of water and 4 parts of water reducing agent, stir well to obtain the primary mixture.

[0061] S2. Secondary mixing: add 70 parts of Portland cement, 3 parts of activator, the remaining 6 parts of water reducer and 30 parts of water to the primary mixture in S1, and stir evenly to obtain a secondary mixture.

[0062] S3, static pressure molding: put the secondary mixture in S2 into the permeable brick mold, tamp it evenly, smooth the surface, and static pressure molding. The static pressure molding pressure is 3MPa, and the holding time is 60s.

[0063] S4, demoulding the mold of the permeable brick formed by static pressure in S3, and curing in water after standing to obtain the permeable brick.

[0064] Test Example 1

[0065] a. Compressive strength test

[0066] The permeable bricks obtained in Examples 1-4 and Comparative Example 1 were placed in a press respectively, pressurized until the permeable bricks were destroyed, and the compressive strength was recorded. The results are shown in Table 1.

[0067] b. Water permeability test

[0068] The upper surface area of ​​the permeable bricks in Examples 1-4 and Comparative Example 1 was calculated, and the sides of the permeable bricks were sealed so that water could only penetrate from the upper and lower surfaces of the permeable bricks. The sealed permeable bricks were immersed in water in a vacuum device, and taken out after soaking for 30 minutes. The permeability coefficient was measured in a permeability coefficient test device, and the results are shown in Table 1.

[0069] c. Water retention test

[0070] The permeable bricks in Examples 1-4 and Comparative Example 1 were dried and weighed, and then placed in a water tank, filled with water until the permeable bricks were submerged, and taken out after soaking for 24 hours. The surface moisture was absorbed and weighed. The water retention obtained is shown in Table 1.

[0071] Table 1. Comparison of the performance of permeable bricks in Examples 1-4 and Comparative Example 1

[0072]

[0073] d. Heavy metal element adsorption test

[0074] Take the permeable bricks in Examples 1-4 and Comparative Example 1, inject sewage containing heavy metal elements (Cd, Pb, Cu) from the top of the permeable bricks, collect the sewage that passes through the permeable bricks, and analyze the heavy metal content of the sewage before and after entering the permeable bricks. The results are shown in Table 1.

[0075] It can be seen from the data in Table 1 that after adding basalt composite fibers and modified pyrite slag, the permeable bricks provided in Examples 1-4 are superior to the permeable bricks in Comparative Example 1 in terms of compressive strength, water permeability, water retention and heavy metal removal effect.

[0076] Therefore, the present invention adopts a basalt composite fiber permeable brick with the above components and a preparation method thereof to improve the compressive strength and water permeability of the permeable brick and adsorb heavy metal elements in rainwater.

[0077] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A basalt composite fiber permeable brick, characterized in that: The mass proportions of the components are: 50-80 parts of silicate cement, 18-30 parts of basalt composite fiber, 15-25 parts of fly ash, 12-25 parts of coarse aggregate, 12-25 parts of fine aggregate, 12-20 parts of modified pyrite slag, 8-12 parts of water reducer, 1-5 parts of activator and 20-50 parts of water.

2. The basalt composite fiber water-permeable brick according to claim 1, characterized in that: The activator includes one or more of caustic, carbonate, alkali metal hydroxide, silicate and carbonate.

3. The basalt composite fiber permeable brick according to claim 1, characterized in that: The particle size range of coarse aggregate is 4.75-9.25mm.

4. The basalt composite fiber water-permeable brick according to claim 1, characterized in that: The particle size of fine aggregate ranges from 1.37 to 4.25 mm.

5. A method for preparing the basalt composite fiber permeable brick according to any one of claims 1 to 4, characterized in that: The following steps are included: S1. preparing modified pyrite slag: adding a dispersant to the pyrite slag and then ball milling, centrifuging and drying, adding deionized water and ultrasonically dispersing to obtain a pyrite slag suspension, adding a sodium hydroxide solution of polyethyleneimine, heating and stirring, slowly adding an acetic acid solution of chitosan, stirring until the mixture is uniform, maintaining the temperature, adding a cross-linking agent for cross-linking reaction, vacuum filtering and washing, and drying to obtain the modified pyrite slag; S2, primary mixing: add the modified pyrite slag, basalt composite fiber, fly ash, coarse aggregate and fine aggregate in S1 according to the mass proportion, mix well, add a small amount of water and water reducing agent, stir well to obtain the primary mixture; S3, secondary mixing: add silicate cement, activator, remaining water reducing agent and water to the primary mixture in S2, and stir evenly to obtain a secondary mixture; S4, static pressure molding: put the secondary mixture in S3 into the permeable brick mold, tamp it evenly, smooth the surface, and static pressure mold it; S5. Demould the mold of the permeable brick formed by static pressure in S4, and perform water curing after standing to obtain the permeable brick.

6. The method for preparing a basalt composite fiber permeable brick according to claim 5, characterized in that: In S1, the dispersant is one or more of ethanol and methanol, and the ball milling conditions are a rotation speed of 200-600 rpm and a time of 6-9 h.

7. The method for preparing a basalt composite fiber permeable brick according to claim 5, characterized in that: In S1, the heating temperature is 40-60°C, and the ultrasonic dispersion conditions are power 220-500W and time 5-20min.

8. The method for preparing a basalt composite fiber permeable brick according to claim 5, characterized in that: In S1, the cross-linking agent is one or more of glutaraldehyde, carbodiimide and N-succinimidyl-3-(2-pyridyldithio)-propionate.

9. The method for preparing a basalt composite fiber permeable brick according to claim 5, characterized in that: In S1, during washing, ethanol and deionized water are used to wash repeatedly.

10. The method for preparing a basalt composite fiber water-permeable brick according to claim 5, characterized in that: In S4, the static pressure molding pressure is 2-6 MPa, and the holding time is 45-90 s.