Concrete based on co-doped hybrid fibers and production process thereof

By using compound mixed fibers and functional additives in concrete, the problem of insufficient mechanical properties and corrosion resistance in the prior art is solved, and the performance of concrete is significantly improved and its service life is extended.

CN118908671AInactive Publication Date: 2024-11-08ZHEJIANG LONGYOU TONGQU BUILDING MATERIALS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411404443.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-10
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing low-shrinkage stable concrete has shortcomings in its mechanical properties and corrosion resistance, which affects its quality and service life.

Method used

The mechanical properties and corrosion resistance of concrete are enhanced by the preparation method of modified basalt fibers and modified polyvinyl alcohol fibers by combining functional additives and silane coupling agents.

Benefits of technology

It significantly improves the mechanical properties and corrosion resistance of concrete, extends its service life, and ensures the quality and quality of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of concrete, in particular to concrete based on co-doped hybrid fibers and a production process of the concrete. The concrete is prepared from the following raw materials in parts by weight: 480 to 550 parts of Portland cement, 200 to 230 parts of fly ash, 800 to 1000 parts of gravel, 1000 to 1100 parts of sand, 200 to 280 parts of expanded perlite, 20 to 30 parts of nano titanium dioxide, 40 to 70 parts of wollastonite, 25 to 40 parts of kaolin, 15 to 25 parts of carbide slag powder, 30 to 50 parts of composite fiber, 6 to 10 parts of functional additive, 15 to 25 parts of silane coupling agent, 5 to 10 parts of water reducing agent and 260 to 300 parts of water. Wherein the composite fiber is formed by mixing modified basalt fiber and modified polyvinyl alcohol fiber according to the ratio of (1-1.5): 1; the concrete produced by the invention not only has excellent mechanical properties, but also has very good corrosion resistance, and the service life of the concrete is prolonged to a certain extent while the quality of the concrete is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of concrete, in particular to concrete based on composite mixed fibers and a production process thereof. Background Art

[0002] Concrete is a composite material made of gel material, aggregate and water in appropriate proportions and hardened after a certain period of time. Concrete has the characteristics of abundant raw materials, low price and simple production process, so its usage is increasing. At the same time, concrete also has the characteristics of high compressive strength, good durability and wide range of strength grades. These characteristics make it widely used. It is not only used in various civil engineering projects, but also in shipbuilding, machinery industry, marine development, geothermal engineering, etc. Concrete is also an important material.

[0003] In the patent document with application number "CN202211595675.6", a low-shrinkage stable concrete and a preparation method thereof are disclosed. The low-shrinkage stable concrete is obtained by curing the concrete mixture into a mold, and the concrete mixture includes the following components in parts by weight: 304-320 parts of silicate cement, 76-80 parts of fly ash, 1000-1060 parts of coarse aggregate, 700-760 parts of fine aggregate, 170-180 parts of mixing water, 80-90 parts of internal curing expansion particles, and 3.8-4.0 parts of polycarboxylic acid water reducer. Although the concrete prepared according to the above patent document has good thermal insulation function, its own mechanical properties and corrosion resistance are relatively insufficient, which affects its quality or quality to a certain extent. Therefore, the present invention provides a concrete based on composite mixed fibers and a production process thereof to solve the above-mentioned technical problems. Summary of the invention

[0004] The purpose of the present invention is to provide a concrete based on composite mixed fibers and its production process, the produced concrete not only has excellent mechanical properties, but also has good corrosion resistance, which ensures the quality of the concrete while also extending its service life to a certain extent.

[0005] To achieve the above object, the present invention provides the following technical solutions: A concrete based on composite mixed fibers is composed of the following raw materials in parts by weight: 480-550 parts of silicate cement, 200-230 parts of fly ash, 800-1000 parts of crushed stone, 1000-1100 parts of sand, 200-280 parts of expanded perlite, 20-30 parts of nano titanium dioxide, 40-70 parts of wollastonite, 25-40 parts of kaolin, 15-25 parts of carbide slag powder, 30-50 parts of composite fibers, 6-10 parts of functional additives, 15-25 parts of silane coupling agents, 5-10 parts of water reducers and 260-300 parts of water; wherein the composite fibers are formed by mixing modified basalt fibers and modified polyvinyl alcohol fibers in a ratio of 1-1.5:1.

[0006] Furthermore, the preparation method of the modified basalt fiber is: The first step is to add γ-glycidyloxypropyltrimethoxysilane at a dosage ratio of 50 to 80 g / L into a 5 to 10 g / L graphene oxide aqueous phase dispersion, adjust the pH to 4.3 to 4.8, and then keep the reaction at a temperature of 55 to 65° C. for 1 to 2 hours; after the reaction is completed, the resultant components are naturally cooled to room temperature, and after solid-liquid separation, water washing and drying treatment in sequence, the obtained pre-treated graphene oxide is stored and used; In the second step, the pretreated graphene oxide is uniformly dispersed in deionized water at a solid-liquid ratio of 20 to 50 g / L to form a pretreated graphene oxide aqueous dispersion, and then basalt fibers with a length of 8 to 12 mm are uniformly dispersed in the pretreated graphene oxide aqueous dispersion at a solid-liquid ratio of 40 to 70 g / L, and vacuum cured at a temperature of 80 to 85° C. for 3 to 4 hours; after the curing is completed, the basalt fibers are fished out and vacuum dried to obtain modified basalt fibers.

[0007] Furthermore, the preparation method of the modified polyvinyl alcohol fiber is as follows: first, the polyvinyl alcohol fiber with a length of 10 to 15 mm is cleaned and dried, and then it is put into a modification liquid with a mass 20 to 40 times that of the polyvinyl alcohol fiber, mixed and stirred evenly, and then immersed and rolled at a temperature of 20 to 40°C for 5 to 10 minutes; after the immersion and rolling is completed, the polyvinyl alcohol fiber is fished out and vacuum dried at a temperature of 80 to 100°C for 5 to 10 minutes; after drying, it is washed and dried again, and the obtained is the modified polyvinyl alcohol fiber.

[0008] Furthermore, the modified liquid is prepared by mixing and stirring deionized water, 4-6% of dimethyl silicone oil, 0.8-1.5% of nano cerium dioxide, 0.5-1.0% of 3-aminopropylmethyldiethoxysilane, and 1.5-2.0% of polyethylene wax.

[0009] Furthermore, the preparation method of the functional additive comprises the following steps: Step 1: Magnesium oxide, 3-hydroxy-1,3,5-pentanetriolic acid, montmorillonite and anhydrous ethanol are put into a ball mill according to a mass ratio of 10-15:1:2-3:10-20, and the ball mill is filtered after 3-5 hours. The obtained filter material is washed and dried, and then calcined at a temperature of 450-550° C. for 30-50 minutes, and finally crushed to 150-250 meshes, and the obtained solid powder is stored and used for standby; Step 2: The solid powder is ball-milled and mixed with 8-12% of pentasodium phosphate and 150-250 mesh size for 2-3 hours, and then the obtained mixture is put into water with a mass of 10-15 times that of the solid powder, and after ultrasonic dispersion for 20-30 minutes, sodium lignin sulfonate with a mass of 1.5-2.0 times that of pentasodium phosphate and sodium alginate with a mass of 8-10 times are added thereto respectively, and after stirring to completely dissolve, a calcium chloride aqueous solution is added dropwise thereto while stirring, and after stirring and dispersing for 40-60 minutes, the mixed components are filtered and dried in turn, and the final product is a functional additive.

[0010] Furthermore, the concentration of the calcium chloride aqueous solution is 3-5wt%, and the drop rate thereof is 70-100 drops / min; and the mass of calcium chloride in the mixed component is 40-60% of the sodium alginate.

[0011] Furthermore, the silane coupling agent is selected from any one of 3-aminopropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, and N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane.

[0012] Furthermore, the water reducing agent is selected from any one of sodium lignin sulfonate, sodium sulfite and calcium saccharide.

[0013] Furthermore, the silicate cement is 42.5R silicate cement, the fly ash is F1 grade fly ash, the crushed stone is continuously graded crushed stone with a particle size of 5 to 25 mm; and the sand is river sand with a fineness modulus of 2.6 to 2.8.

[0014] A production process for composite-blended mixed fiber concrete comprises the following steps: accurately weighing each raw material according to the formula amount, mixing and stirring each raw material except composite fiber and water, then adding water, mixing and stirring evenly, adding the remaining raw materials, and mechanically stirring for 3 to 5 minutes to obtain the composite-blended mixed fiber concrete.

[0015] Compared with the prior art, the present invention has the following beneficial effects: The present invention grafts and modifies graphene oxide by γ-glycidyloxypropyltrimethoxysilane to obtain pre-treated graphene oxide. Then, basalt fiber is dispersed in the pre-treated graphene oxide aqueous dispersion, and after vacuum curing treatment, the basalt fiber is grafted with graphene oxide under the "bridge" effect of γ-glycidyloxypropyltrimethoxysilane, and finally the three-dimensional spatial structure of the basalt fiber is effectively broadened to prepare modified basalt fiber. The polyvinyl alcohol fiber is modified by the modifying liquid, which can not only significantly improve the dispersion performance of the polyvinyl alcohol fiber in the concrete system, but also enhance the mechanical properties of the concrete. In addition, the functional additive prepared by the present invention not only has an excellent expansion effect, but also can effectively enhance the mechanical strength of the concrete. Under the synergistic effect of the modified basalt fiber agent and the modified polyvinyl alcohol fiber, the mechanical properties of the concrete are effectively guaranteed while also ensuring its quality. Furthermore, the use of the composite fiber in the present invention can improve the concrete's resistance to chloride ion penetration, thereby improving its anti-corrosion performance and extending its service life to a certain extent. DETAILED DESCRIPTION

[0016] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0017] Embodiment 1: A concrete based on composite mixed fibers, comprising the following raw materials in parts by weight: 480 parts of silicate cement, 200 parts of fly ash, 800 parts of crushed stone, 1000 parts of sand, 200 parts of expanded perlite, 20 parts of nano titanium dioxide, 40 parts of wollastonite, 25 parts of kaolin, 15 parts of carbide slag powder, 30 parts of composite fibers, 6 parts of functional additives, 15 parts of 3-aminopropyltriethoxysilane, 5 parts of sodium lignin sulfonate and 260 parts of water; Among them, the composite fiber is a mixture of modified basalt fiber and modified polyvinyl alcohol fiber; The silicate cement used is 42.5R silicate cement, the fly ash is F1 grade fly ash, the crushed stone is continuously graded crushed stone with a particle size of 15mm; the sand used is river sand with a fineness modulus of 2.6.

[0018] The preparation method of modified basalt fiber is: The first step is to add γ-glycidyloxypropyltrimethoxysilane to 5g / L of graphene oxide aqueous dispersion at a dosage ratio of 50g / L, adjust the pH to 4.3 and then keep the reaction at 55°C for 1h; after the reaction is completed, the resultant components are naturally cooled to room temperature, and after solid-liquid separation, water washing and drying treatment, the obtained pre-treated graphene oxide is stored and used; In the second step, the pretreated graphene oxide is uniformly dispersed in deionized water at a solid-liquid ratio of 20 g / L to form a pretreated graphene oxide aqueous dispersion, and then basalt fibers with a length of 8 mm are uniformly dispersed in the pretreated graphene oxide aqueous dispersion at a solid-liquid ratio of 40 g / L, and vacuum cured at a temperature of 80°C for 3 hours; after the curing is completed, the basalt fibers are fished out and vacuum dried to obtain modified basalt fibers.

[0019] The preparation method of modified polyvinyl alcohol fiber is as follows: firstly, polyvinyl alcohol fiber with a length of 10 mm is cleaned and dried, and then it is put into a modification liquid with a mass 20 times that of the polyvinyl alcohol fiber, mixed and stirred evenly, and then impregnated and rolled at a temperature of 20°C for 5 minutes; after the impregnation and rolling is completed, the polyvinyl alcohol fiber is fished out and vacuum dried at a temperature of 80°C for 5 minutes; after drying, it is washed and dried to obtain the modified polyvinyl alcohol fiber; the modification liquid is prepared by mixing and stirring deionized water and 4% of dimethyl silicone oil, 0.8% of nano cerium dioxide, 0.5% of 3-aminopropylmethyldiethoxysilane, and 1.5% of polyethylene wax, respectively.

[0020] The preparation method of the functional additive comprises the following steps: Step 1: put magnesium oxide, 3-hydroxy-1,3,5-pentanetriolic acid, montmorillonite and anhydrous ethanol into a ball mill according to a mass ratio of 10:1:2:10, filter the ball mill after 3 hours, wash and dry the filter material, calcine it at 450°C for 30 minutes, and finally crush it to 150 mesh. The solid powder is stored and used for standby; Step 2: The solid powder is ball-milled with 8% sodium phosphate pentasodium phosphate and 150 mesh size for 2 hours, and then the mixture is put into water with a mass of 10 times that of the solid powder. After ultrasonic dispersion for 20 minutes, sodium lignin sulfonate with a mass of 1.5 times that of sodium phosphate pentasodium and sodium alginate with a mass of 8 times are added thereto respectively. After stirring to completely dissolve, a calcium chloride aqueous solution is added dropwise thereto while stirring. After stirring and dispersing for 40 minutes, the mixed components are filtered and dried in turn, and the final product is a functional additive; wherein the concentration of the calcium chloride aqueous solution is 3wt%, and the drop rate is 70 drops / min; and the mass of calcium chloride in the mixed component is 40% of the sodium alginate.

[0021] A production process for composite-blended mixed fiber concrete comprises the following steps: accurately weighing each raw material according to the formula amount, mixing and stirring each raw material except composite fiber and water, then adding water, mixing and stirring evenly, adding the remaining raw materials, and mechanically stirring for 3 minutes to obtain composite-blended mixed fiber concrete.

[0022] Embodiment 2:

[0023] The production process of a concrete based on composite mixed fibers provided in this embodiment is basically the same as that in Embodiment 1, except that the specific composition of the concrete and the preparation methods of the modified basalt fiber, the modified polyvinyl alcohol fiber, and the functional additive are not completely the same. The specific composition of the concrete and the preparation methods of the modified basalt fiber, the modified polyvinyl alcohol fiber, and the functional additive in this embodiment are as follows: A concrete based on composite mixed fibers is composed of the following raw materials in parts by weight: 500 parts of silicate cement, 220 parts of fly ash, 900 parts of crushed stone, 1050 parts of sand, 240 parts of expanded perlite, 25 parts of nano titanium dioxide, 50 parts of wollastonite, 30 parts of kaolin, 20 parts of carbide slag powder, 40 parts of composite fibers, 8 parts of functional additives, 20 parts of γ-methacryloxypropyltrimethoxysilane, 8 parts of sodium sulfite and 280 parts of water; wherein the composite fibers are formed by mixing modified basalt fibers and modified polyvinyl alcohol fibers in a ratio of 1.2:1.

[0024] The preparation method of modified basalt fiber is: The first step is to add γ-glycidyloxypropyltrimethoxysilane to 8g / L of graphene oxide aqueous dispersion at a dosage ratio of 60g / L, adjust the pH to 4.5 and then keep the reaction at 60°C for 1.5h; after the reaction is completed, the resultant components are naturally cooled to room temperature, and after solid-liquid separation, water washing and drying treatment in sequence, the obtained pre-treated graphene oxide is stored and used; In the second step, the pretreated graphene oxide is uniformly dispersed in deionized water at a solid-liquid ratio of 40 g / L to form a pretreated graphene oxide aqueous dispersion, and then basalt fibers with a length of 10 mm are uniformly dispersed in the pretreated graphene oxide aqueous dispersion at a solid-liquid ratio of 60 g / L, and vacuum cured at a temperature of 80°C for 3 hours; after the curing is completed, the basalt fibers are fished out and vacuum dried to obtain modified basalt fibers.

[0025] The preparation method of modified polyvinyl alcohol fiber is as follows: first, polyvinyl alcohol fiber with a length of 12 mm is cleaned and dried, and then it is put into a modification liquid with a mass 30 times that of the polyvinyl alcohol fiber, mixed and stirred evenly, and then immersed and rolled for 10 minutes at a temperature of 30°C; after the immersion and rolling is completed, the polyvinyl alcohol fiber is fished out and vacuum dried at a temperature of 90°C for 10 minutes; after drying, it is washed and dried again to obtain the modified polyvinyl alcohol fiber.

[0026] The modified liquid is prepared by mixing deionized water, 4-6% of dimethyl silicone oil, 0.8-1.5% of nano cerium dioxide, 0.5-1.0% of 3-aminopropylmethyldiethoxysilane and 1.5-2.0% of polyethylene wax uniformly.

[0027] The preparation method of the functional additive comprises the following steps: Step 1: Magnesium oxide, 3-hydroxy-1,3,5-pentanetriolic acid, montmorillonite and anhydrous ethanol are put into a ball mill according to a mass ratio of 12:1:2.5:15, and the ball mill is filtered after 4 hours. The filter material is washed and dried, and then calcined at a temperature of 500°C for 40 minutes. Finally, it is crushed to 200 meshes, and the obtained solid powder is stored for standby use; Step 2: The solid powder is ball-milled with 10% of the mass of pentasodium phosphate and 200 mesh size for 2 hours, and then the obtained mixture is put into water with a mass of 12 times that of the mass of the solid powder. After ultrasonic dispersion for 25 minutes, sodium lignin sulfonate with a mass of 1.5 times that of pentasodium phosphate and sodium alginate with a mass of 8 times are added thereto respectively, and after stirring to completely dissolve, a calcium chloride aqueous solution is added dropwise thereto while stirring. After stirring and dispersing for 50 minutes, the mixed components are filtered and dried in turn, and the final product is a functional additive; wherein the concentration of the calcium chloride aqueous solution is 4wt%, and the dropping rate is 80 drops / min; and the mass of calcium chloride in the mixed component is 50% of the sodium alginate.

[0028] Embodiment 3:

[0029] The production process of a concrete based on composite mixed fibers provided in this embodiment is basically the same as that in Embodiment 1, except that the specific composition of the concrete and the preparation methods of the modified basalt fiber, the modified polyvinyl alcohol fiber, and the functional additive are not completely the same. The specific composition of the concrete and the preparation methods of the modified basalt fiber, the modified polyvinyl alcohol fiber, and the functional additive in this embodiment are as follows: A concrete based on composite mixed fibers is composed of the following raw materials in parts by weight: 550 parts of silicate cement, 230 parts of fly ash, 1000 parts of crushed stone, 1100 parts of sand, 280 parts of expanded perlite, 30 parts of nano titanium dioxide, 70 parts of wollastonite, 40 parts of kaolin, 25 parts of carbide slag powder, 50 parts of composite fibers, 10 parts of functional additives, 25 parts of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, 10 parts of calcium saccharide and 300 parts of water; wherein the composite fibers are formed by mixing modified basalt fibers and modified polyvinyl alcohol fibers in a ratio of 1.5:1.

[0030] The preparation method of modified basalt fiber is: The first step is to add γ-glycidyloxypropyltrimethoxysilane into 10g / L graphene oxide aqueous phase dispersion at a dosage ratio of 80g / L, adjust the pH to 4.8 and keep the reaction at 65°C for 2h; after the reaction is completed, the resultant components are naturally cooled to room temperature, and after solid-liquid separation, water washing and drying treatment, the obtained pre-treated graphene oxide is stored and used; In the second step, the pretreated graphene oxide is uniformly dispersed in deionized water at a solid-liquid ratio of 50 g / L to form a pretreated graphene oxide aqueous dispersion, and then basalt fibers with a length of 12 mm are uniformly dispersed in the pretreated graphene oxide aqueous dispersion at a solid-liquid ratio of 70 g / L, and vacuum cured at a temperature of 85°C for 4 hours; after the curing is completed, the basalt fibers are fished out and vacuum dried to obtain modified basalt fibers.

[0031] The preparation method of modified polyvinyl alcohol fiber is as follows: firstly, polyvinyl alcohol fiber with a length of 15 mm is cleaned and dried, and then it is put into a modification liquid with a mass 40 times that of the polyvinyl alcohol fiber, mixed and stirred evenly, and then impregnated and rolled at a temperature of 40°C for 10 minutes; after the impregnation and rolling is completed, the polyvinyl alcohol fiber is fished out and vacuum dried at a temperature of 100°C for 10 minutes; after drying, it is washed and dried to obtain the modified polyvinyl alcohol fiber; the modification liquid is prepared by mixing and stirring deionized water and 6% of dimethyl silicone oil, 1.5% of nano cerium dioxide, 1.0% of 3-aminopropylmethyldiethoxysilane, and 2.0% of polyethylene wax, respectively.

[0032] The preparation method of the functional additive comprises the following steps: Step 1: Magnesium oxide, 3-hydroxy-1,3,5-pentanetriolic acid, montmorillonite and anhydrous ethanol are put into a ball mill according to a mass ratio of 15:1:3:20, and the ball mill is filtered after 5 hours. The filter material is washed and dried, and then calcined at a temperature of 550°C for 50 minutes. Finally, it is crushed to 250 meshes, and the obtained solid powder is stored for standby use; Step 2: The solid powder is ball-milled with 12% of pentasodium phosphate and 250 mesh size for 3 hours, and then the mixture is put into water with a mass of 15 times that of the pentasodium phosphate, and after ultrasonic dispersion for 30 minutes, sodium lignin sulfonate with a mass of 2.0 times that of pentasodium phosphate and sodium alginate with a mass of 10 times are added thereto respectively, and after stirring to completely dissolve, a calcium chloride aqueous solution is added dropwise thereto while stirring, and after stirring and dispersing for 60 minutes, the mixed components are filtered and dried in turn, and the final product is a functional additive; wherein the concentration of the calcium chloride aqueous solution is 5wt%, and the dropping rate thereof is 100 drops / min; and the mass of calcium chloride in the mixed component is 60% of the sodium alginate.

[0033] Performance test: The relevant properties of the concrete samples provided in Examples 1 to 3 were tested as follows: 1. The compressive strength is tested according to GB / T 50081-2016 standard; 2. The cracking performance is tested according to GB / T 29417-2012 standard; 3. The resistance to sulfate erosion and chloride ion penetration is tested according to GB / T 50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete".

[0034] And record the test data in the following table:

[0035] By comparing and analyzing the relevant data in the table, it can be seen that the concrete produced by the present invention not only has excellent mechanical properties, but also has good corrosion resistance, which ensures the quality of the concrete and also prolongs its service life to a certain extent. This shows that the concrete based on composite mixed fibers and its production process provided by the present invention have a broader market prospect and are more suitable for promotion.

[0036] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0037] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A concrete based on composite mixed fibers, It is characterized in that The invention is composed of the following raw materials in parts by weight: 480-550 parts of silicate cement, 200-230 parts of fly ash, 800-1000 parts of crushed stone, 1000-1100 parts of sand, 200-280 parts of expanded perlite, 20-30 parts of nano titanium dioxide, 40-70 parts of wollastonite, 25-40 parts of kaolin, 15-25 parts of carbide slag powder, 30-50 parts of composite fiber, 6-10 parts of functional additives, 15-25 parts of silane coupling agent, 5-10 parts of water reducer and 260-300 parts of water; wherein the composite fiber is formed by mixing modified basalt fiber and modified polyvinyl alcohol fiber in a ratio of 1-1.5:

1.

2. A concrete based on composite mixed fibers according to claim 1, It is characterized in that The preparation method of the modified basalt fiber is: The first step is to add γ-glycidyloxypropyltrimethoxysilane at a dosage ratio of 50 to 80 g / L into a 5 to 10 g / L graphene oxide aqueous phase dispersion, adjust the pH to 4.3 to 4.8, and then keep the reaction at a temperature of 55 to 65° C. for 1 to 2 hours; after the reaction is completed, the resultant components are naturally cooled to room temperature, and after solid-liquid separation, water washing and drying treatment in sequence, the obtained pre-treated graphene oxide is stored and used; In the second step, the pretreated graphene oxide is uniformly dispersed in deionized water at a solid-liquid ratio of 20 to 50 g / L to form a pretreated graphene oxide aqueous dispersion, and then basalt fibers with a length of 8 to 12 mm are uniformly dispersed in the pretreated graphene oxide aqueous dispersion at a solid-liquid ratio of 40 to 70 g / L, and vacuum cured at a temperature of 80 to 85° C. for 3 to 4 hours; after the curing is completed, the basalt fibers are fished out and vacuum dried to obtain modified basalt fibers.

3. A concrete based on composite mixed fibers according to claim 1, It is characterized in that The preparation method of the modified polyvinyl alcohol fiber is as follows: firstly, polyvinyl alcohol fibers with a length of 10 to 15 mm are cleaned and dried, and then the fibers are put into a modification liquid with a mass 20 to 40 times that of the polyvinyl alcohol fibers, mixed and stirred evenly, and then immersed and rolled for 5 to 10 minutes at a temperature of 20 to 40° C.; after the immersion and rolling is completed, the polyvinyl alcohol fibers are fished out and vacuum dried for 5 to 10 minutes at a temperature of 80 to 100° C.; after drying, the fibers are washed and dried again, and the obtained fibers are the modified polyvinyl alcohol fibers.

4. A concrete based on composite mixed fibers according to claim 3, Features: The modified liquid is prepared by mixing and stirring deionized water, 4-6% of dimethyl silicone oil, 0.8-1.5% of nano cerium dioxide, 0.5-1.0% of 3-aminopropylmethyldiethoxysilane and 1.5-2.0% of polyethylene wax.

5. A concrete based on composite mixed fibers according to claim 1, It is characterized in that The preparation method of the functional additive comprises the following steps: Step 1: Magnesium oxide, 3-hydroxy-1,3,5-pentanetriolic acid, montmorillonite and anhydrous ethanol are put into a ball mill according to a mass ratio of 10-15:1:2-3:10-20, and the ball mill is filtered after 3-5 hours. The obtained filter material is washed and dried, and then calcined at a temperature of 450-550° C. for 30-50 minutes, and finally crushed to 150-250 meshes, and the obtained solid powder is stored and used for standby; Step 2: The solid powder is ball-milled and mixed with 8-12% of pentasodium phosphate and 150-250 mesh size for 2-3 hours, and then the obtained mixture is put into water with a mass of 10-15 times that of the solid powder, and after ultrasonic dispersion for 20-30 minutes, sodium lignin sulfonate with a mass of 1.5-2.0 times that of pentasodium phosphate and sodium alginate with a mass of 8-10 times are added thereto respectively, and after stirring to completely dissolve, a calcium chloride aqueous solution is added dropwise thereto while stirring, and after stirring and dispersing for 40-60 minutes, the mixed components are filtered and dried in turn, and the final product is a functional additive.

6. A concrete based on composite mixed fibers according to claim 5, Features: The concentration of the calcium chloride aqueous solution is 3-5wt%, and the drop rate is 70-100 drops / min; and the mass of calcium chloride in the mixed component is 40-60% of the sodium alginate.

7. A concrete based on composite mixed fibers according to claim 1, Features: The silane coupling agent is selected from any one of 3-aminopropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane and N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane.

8. A concrete based on composite mixed fibers according to claim 1, Features: The water reducing agent is selected from any one of sodium lignin sulfonate, sodium sulfite and calcium saccharide.

9. A concrete based on composite mixed fibers according to claim 1, Features: The silicate cement is 42.5R silicate cement, the fly ash is F1 grade fly ash, the crushed stone is continuously graded crushed stone with a particle size of 5 to 25 mm; the sand is river sand with a fineness modulus of 2.6 to 2.

8.

10. A production process for concrete based on composite mixed fibers according to any one of claims 1 to 9, It is characterized in that The method comprises the following steps: accurately weighing each raw material according to the formula amount, mixing and stirring each raw material except the composite fiber and water evenly, then adding water, mixing and stirring evenly, adding the remaining raw materials, and mechanically stirring for 3 to 5 minutes to obtain concrete based on composite mixed fibers.

Citation Information

Patent Citations

  • Surface treatment and modification method for high-strength high-mold polyvinyl alcohol fibers

    CN105506999A

  • High-performance fiber concrete and preparation method thereof

    CN112960949A

  • High-weather-resistance basalt fiber concrete and preparation method thereof

    CN116003065A

  • Self-compacting shrinkage-compensating concrete and preparation method thereof

    CN116143462A

  • Fiber-toughened anti-cracking cement stabilized macadam as well as preparation method and construction method thereof

    CN117645451A