Lepidolite slag water-based epoxy rapid repair mortar and preparation method thereof
By blending the modified lithium mica slag/sepiolite fiber/lithium titanate whisker composite with cement, combined with modified amine aqueous curing agent and epoxy resin, the existing aqueous epoxy emulsion repair mortar in compressive strength is solved. , problems of impermeability and rapid repairability have achieved efficient repair performance and environmentally friendly construction process.
Patent Information
- Application Number
- CN202410947489.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-16
AI Technical Summary
The existing aqueous epoxy emulsion repair mortars have poor performance in compressive strength, permeability and rapid repair, and are difficult to meet the high requirements in engineering fields such as roads and bridges.
Modified lithium mica slag/sepiolite fiber/lithium titanate whisker composite is blended with ordinary silicate/sulfur aluminate cement, combined with modified amine aqueous curing agent and epoxy resin to form a compact resin matrix With the aggregate system, reduce voids and defects, improve compressive strength and permeability, and enhance adhesion and toughness through epoxy resin curing systems.
It significantly improves the compressive strength, flexural strength, crack resistance and dimensional stability of the mortar, shortens the settling time, realizes the rapid repair function, and reduces the pollution of the environment by organic solvents.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of repair polymer mortars, and in particular to a lepidolite slag water-based epoxy rapid repair mortar and a preparation method thereof. Background Art
[0002] Concrete is subjected to environmental corrosion for a long time, and various defects are prone to appear on the surface. In order to improve the durability of concrete, its surface needs to be repaired. Polymer repair mortar is a new material widely used in the field of building maintenance, especially epoxy mortar, which has high bonding strength and good resistance to medium corrosion, and has broad application prospects. The current maintenance of special engineering fields such as roads, bridges, airports and beams has put forward high requirements for repair mortar, such as rapid repair, environmentally friendly construction, stable product size, excellent mechanical properties, and good impermeability.
[0003] The prior art discloses a water-based epoxy emulsion repair mortar and a preparation method thereof, wherein the raw materials include: 1.5% to 24% water-based epoxy emulsion, 0.15% to 4.8% curing agent, 15% to 30% cement, 33% to 66% aggregate, 4% to 8% mineral admixture, 0.01% to 0.2% chemical additives and 2% to 8% water, and the sum of the weight percentages of each component is 100%. The water-based epoxy emulsion repair mortar prepared by the patent has excellent flexural strength, corrosion resistance and workability, but the compressive strength, impermeability and rapid repairability are average. Summary of the invention
[0004] The purpose of the present invention is to solve at least one of the technical problems existing in the prior art. In order to meet the above repair requirements, the present invention provides a lithium mica slag water-based epoxy rapid repair mortar and its preparation method. The ordinary silicate / sulfoaluminate cement is blended and modified and the modified amine is used for epoxy resin curing to accelerate the mortar repair speed; the modified lithium mica slag / sepiolite fiber / lithium titanate whisker composite reduces the gap and defects between the resin matrix and the aggregate, and improves the compressive strength of the mortar; the polymer, cement gel material, lithium mica slag, sepiolite fiber, lithium titanate whisker and coarse and fine sand form a dense system, and the addition of coupling agent further enhances the compactness between lithium mica slag, sepiolite fiber, lithium titanate whisker and polymer, and improves the impermeability, crack resistance and dimensional stability of the mortar; the epoxy resin curing system improves the impermeability, adhesion and toughness of the mortar. In addition, the water-based epoxy mortar greatly reduces the pollution of organic solvents to the environment compared with the oil-soluble mortar system.
[0005] The technical solution of the present invention is as follows:
[0006] A lepidolite slag water-based epoxy quick-repair mortar, comprising the following raw materials in parts by weight:
[0007] 1100-1300 parts of aggregate, 400-600 parts of ordinary Portland cement, 200-400 parts of sulphoaluminate cement, 100-120 parts of water-based epoxy emulsion, 0.5-0.7 parts of defoamer, 0.5-0.7 parts of wetting agent, 3-5 parts of water reducer, 140-160 parts of deionized water, 30-60 parts of modified lithium mica slag / sepiolite fiber / lithium titanate whisker composite, and 50-60 parts of modified amine water-based curing agent.
[0008] Preferably, the preparation raw materials include the following parts by weight:
[0009] 1150-1250 parts of aggregate, 450-550 parts of ordinary Portland cement, 250-350 parts of sulphoaluminate cement, 105-115 parts of water-based epoxy emulsion, 0.55-0.65 parts of defoamer, 0.55-0.65 parts of wetting agent, 3.5-4.5 parts of water reducer, 145-155 parts of deionized water, 40-50 parts of modified lithium mica slag / sepiolite fiber / lithium titanate whisker composite, and 52-58 parts of modified amine water-based curing agent.
[0010] Preferably, the preparation method of the modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite comprises:
[0011] The lithium mica slag is ball-milled to obtain a specific surface area of 200-800m 2 / kg of lithium mica slag particles;
[0012] Evenly mixing the epoxy group silane coupling agent and ethanol to prepare an epoxy group silane coupling agent / ethanol mixed solution;
[0013] Adding sepiolite fiber into ethanol, ultrasonically dispersing, adding potassium titanate whisker into the mixture, ultrasonically dispersing, and drying to obtain a sepiolite fiber / potassium titanate whisker mixture;
[0014] The lepidolite slag particles are stirred, and the epoxy group silane coupling agent / ethanol mixed solution is sprayed on the surface of the lepidolite slag particles, and the sepiolite fiber and potassium titanate whisker mixture is added and stirred evenly, and then heated to 80-100° C. for 30-90 minutes to obtain a modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite.
[0015] Preferably, in the preparation method of the modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite, the mass ratio of the epoxy group silane coupling agent to ethanol is 1-2:5-10, the mass ratio of the lepidolite slag to the epoxy group silane coupling agent is 30-60:1-2, and the mass ratio of the lepidolite slag, sepiolite fiber and potassium titanate whisker is 30-60:1-5:1-5.
[0016] Preferably, the epoxy group silane coupling agent is at least one of KBM-303, KBM-403 and KBE-402.
[0017] Preferably, the preparation method of the modified amine water-based curing agent comprises:
[0018] Triethylenetetramine and bisphenol A epoxy resin are reacted at 60-70°C for 3-5h to obtain an epoxy-amine adduct intermediate;
[0019] The double-terminal epoxy polyether is reacted with the epoxy-amine adduct intermediate at 90-100° C. for 2-5 hours to obtain a modified amine water-based curing agent.
[0020] Preferably, in the preparation method of the modified amine water-based curing agent, the molar ratio of the triethylenetetramine to the bisphenol A epoxy resin is 2-3:1; and the molar ratio of the double-terminated epoxy polyether to the epoxy-amine adduct intermediate is 0.3-0.7:1.
[0021] Preferably, the preparation method of the waterborne epoxy emulsion comprises:
[0022] 1) adding epoxy resin E44 and polyethylene glycol 6000 in a molar ratio of 2:1 into a round-bottom flask respectively, and heating to 85° C. under the protection of dry nitrogen, and mixing them evenly under stirring after the two are completely melted to obtain an epoxy resin E44 / polyethylene glycol 6000 blend;
[0023] 2) The catalyst BF3 ether was diluted 10 times with acetone and then added dropwise to the epoxy resin E44 / polyethylene glycol 6000 blend, and the mixture was kept at 85°C for catalytic reaction for 4 hours, and then vacuum distilled until no solvent was removed, thereby obtaining an epoxy resin emulsifier;
[0024] 3) adding epoxy resin E44 and epoxy resin emulsifier into a stirring kettle, heating to 70° C., stirring at a high speed of 1000-1500 r / min to mix uniformly, gradually adding water into the stirring kettle, and preparing an aqueous epoxy emulsion with a solid content of 40%-60% by a phase inversion method, wherein the mass ratio of epoxy resin E44 to epoxy resin emulsifier is 1:9.
[0025] The addition amount of catalyst BF3 ether is 0.2-0.4% of the total mass of epoxy resin E44 and polyethylene glycol 6000.
[0026] Preferably, the aggregate is artificial sand or natural sand with a particle size of less than 4.75 mm and a mud content of ≤0.45wt%;
[0027] The ordinary Portland cement is at least one of P·O 42.5, 52.5, and 62.5, and the sulphoaluminate cement is fast-hardening sulphoaluminate cement.
[0028] A second aspect of the present invention provides a method for preparing a lepidolite slag water-based epoxy rapid repair mortar, comprising the following steps:
[0029] S1. Weigh the water-based epoxy emulsion, wetting agent and deionized water in proportion and stir them evenly for 0.5-2 minutes, then add the modified amine water-based curing agent and defoaming agent respectively and stir them evenly to prepare a multi-component mixture;
[0030] S2. Weigh aggregate, ordinary Portland cement, sulphoaluminate cement, modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite, and water reducer in proportion, mix and stir for 0.5-2 minutes, add the multi-component mixture in step S1, and stir together for 3-5 minutes to prepare lepidolite slag water-based epoxy quick repair mortar.
[0031] The present invention has at least one of the following beneficial effects:
[0032] On the one hand, the present invention adds a modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite, and the finely ground lepidolite slag is mostly flaky and round particles, has good reinforcement and bulk density, can reduce the gap and defects between the resin matrix and the aggregate, improve the compressive strength of the mortar, and can improve the flexural strength and tensile bonding strength of the mortar; and the present invention performs mixed modification on the lepidolite slag, sepiolite fiber, and lithium titanate whisker, can reduce the agglomeration of the sepiolite fiber and the lithium titanate whisker, and make the sepiolite fiber Stone fiber and lithium titanate whisker are evenly dispersed in lithium mica slag, and the addition of epoxy group silane coupling agent further enhances the tightness between modified lithium mica slag / sepiolite fiber / lithium titanate whisker composite and polymer, so that sepiolite fiber and lithium titanate whisker can finally be evenly dispersed in cement, and the modified sepiolite fiber, lithium titanate whisker and lithium mica slag can work together to significantly improve the mortar's impermeability, crack resistance, dimensional stability, compressive strength, flexural strength and tensile bonding strength. On the other hand, in the repair mortar of the present invention, ordinary silicate cement and sulphoaluminate cement are blended and modified in a certain proportion to shorten the setting time of the cement system, and the modified amine water-based curing agent increases the curing speed of the epoxy resin, giving the mortar a rapid repair function; the epoxy resin improves the mortar's impermeability, adhesion and toughness. In addition, the water-based epoxy mortar greatly reduces the pollution of organic solvents to the environment relative to the oil-soluble mortar system, and greatly meets the current rapid repair needs of highways, bridges, airports and beams, etc., which are environmentally friendly and quality-assured. DETAILED DESCRIPTION
[0033] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0034] One embodiment of the present invention provides a lepidolite slag water-based epoxy rapid repair mortar, comprising the following raw materials in parts by weight:
[0035] 1100-1300 parts of aggregate, 400-600 parts of ordinary Portland cement, 200-400 parts of sulphoaluminate cement, 100-120 parts of water-based epoxy emulsion, 0.5-0.7 parts of defoamer, 0.5-0.7 parts of wetting agent, 3-5 parts of water reducer, 140-160 parts of deionized water, 30-60 parts of modified lithium mica slag / sepiolite fiber / lithium titanate whisker composite, and 50-60 parts of modified amine water-based curing agent.
[0036] Preferably, the mass fractions of each preparation raw material are:
[0037] 1150-1250 parts of aggregate, 450-550 parts of ordinary Portland cement, 250-350 parts of sulphoaluminate cement, 105-115 parts of water-based epoxy emulsion, 0.55-0.65 parts of defoamer, 0.55-0.65 parts of wetting agent, 3.5-4.5 parts of water reducer, 145-155 parts of deionized water, 40-50 parts of modified lithium mica slag / sepiolite fiber / lithium titanate whisker composite, and 52-58 parts of modified amine water-based curing agent.
[0038] More preferably, the mass fractions of each preparation raw material are:
[0039] 1100 parts of aggregate, 400 parts of ordinary Portland cement, 400 parts of sulphoaluminate cement, 110 parts of water-based epoxy emulsion, 0.6 parts of defoamer, 0.6 parts of wetting agent, 4 parts of water reducer, 150 parts of deionized water, 45 parts of modified lithium mica slag / sepiolite fiber / lithium titanate whisker composite, and 50 parts of modified amine water-based curing agent.
[0040] The aggregate is artificial sand or natural sand with a particle size of less than 4.75 mm and a mud content of ≤0.45wt%;
[0041] Ordinary silicate cement is at least one of P·O 42.5, 52.5, and 62.5, and can be specifically P·O 52.5. Sulphoaluminate cement is rapid hardening sulphoaluminate cement, and can be specifically rapid hardening sulphoaluminate 52.5 cement (R·SAC 52.5).
[0042] The preparation method of the aqueous epoxy emulsion comprises:
[0043] 1) adding epoxy resin E44 and polyethylene glycol 6000 in a molar ratio of 2:1 into a round-bottom flask respectively, and heating to 85° C. under the protection of dry nitrogen, and mixing them evenly under stirring after the two are completely melted to obtain an epoxy resin E44 / polyethylene glycol 6000 blend;
[0044] 2) The catalyst BF3 ether was diluted 10 times with acetone and then added dropwise to the epoxy resin E44 / polyethylene glycol 6000 blend, and the mixture was kept at 85°C for catalytic reaction for 4 hours, and then vacuum distilled until no solvent was removed, thereby obtaining an epoxy resin emulsifier;
[0045] 3) adding epoxy resin E44 and epoxy resin emulsifier into a stirring kettle, heating to 70° C., stirring at a high speed of 1000-1500 r / min to mix uniformly, gradually adding water into the stirring kettle, and preparing an aqueous epoxy emulsion with a solid content of 40%-60% by a phase inversion method, wherein the mass ratio of epoxy resin E44 to epoxy resin emulsifier is 1:9.
[0046] The addition amount of catalyst BF3 ether is 0.2-0.4% of the total mass of epoxy resin E44 and polyethylene glycol 6000.
[0047] The preparation method of the modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite comprises:
[0048] The lithium mica slag is ball-milled to obtain a specific surface area of 200-800m 2 / kg of lithium mica slag particles;
[0049] Evenly mixing the epoxy group silane coupling agent and ethanol to prepare an epoxy group silane coupling agent / ethanol mixed solution;
[0050] Adding sepiolite fiber into ethanol, ultrasonically dispersing, adding potassium titanate whisker into the mixture, ultrasonically dispersing, and drying to obtain a sepiolite fiber / potassium titanate whisker mixture;
[0051] The lepidolite slag particles are stirred, and the epoxy group silane coupling agent / ethanol mixed solution is sprayed on the surface of the lepidolite slag particles, and the sepiolite fiber and potassium titanate whisker mixture is added and stirred evenly, and then heated to 80-100° C. for 30-90 minutes to obtain a modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite.
[0052] Among them, the mass ratio of the epoxy group silane coupling agent to ethanol is 1-2:5-10, the mass ratio of the lepidolite slag to the epoxy group silane coupling agent is 30-60:1-2, and the mass ratio of the lepidolite slag, sepiolite fiber and potassium titanate whisker is 30-60:1-5:1-5.
[0053] The epoxy group silane coupling agent is at least one of KBM-303, KBM-403 and KBE-402.
[0054] The preparation method of the modified amine water-based curing agent comprises:
[0055] Triethylenetetramine and bisphenol A epoxy resin are reacted at 60-70°C for 3-5h to obtain an epoxy-amine adduct intermediate;
[0056] The double-terminal epoxy polyether is reacted with the epoxy-amine adduct intermediate at 90-100° C. for 2-5 hours to obtain a modified amine water-based curing agent.
[0057] Wherein, the molar ratio of triethylenetetramine to bisphenol A epoxy resin is 2-3:1; preferably 2.2-2.8:1, and more preferably 2.5:1.
[0058] The molar ratio of the double-terminal epoxy polyether to the epoxy-amine adduct intermediate is 0.3-0.7:1, preferably 0.4-0.6:1, and more preferably 0.5:1.
[0059] The bisphenol A epoxy resin is specifically bisphenol A epoxy resin E51.
[0060] A second aspect of the present invention provides a method for preparing a lepidolite slag water-based epoxy rapid repair mortar, comprising:
[0061] S1. Weigh the water-based epoxy emulsion, wetting agent and deionized water in proportion and stir them evenly for 0.5-2 minutes, then add the modified amine water-based curing agent and defoaming agent respectively and stir them evenly to prepare a multi-component mixture;
[0062] S2. Weigh aggregate, ordinary Portland cement, sulphoaluminate cement, modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite, and water reducer in proportion, mix and stir for 0.5-2 minutes, add the multi-component mixture in step S1, and stir together for 3-5 minutes to prepare lepidolite slag water-based epoxy quick repair mortar.
[0063] The present invention is further described in detail below with specific examples, but the present invention is not limited to the following specific examples.
[0064] The model of the wetting agent in the following embodiments and comparative examples is 9440, the model of the water reducer is LonS-P, the model of the defoamer is AF-706, the model of the double-terminated epoxy polyether is SF-260 / 400, and the model of the bisphenol A type epoxy resin is E51 (Baling Petrochemical) and the epoxy resin E44 (Baling Petrochemical).
[0065] Example 1
[0066] 1. Preparation of modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite:
[0067] 1) Take a certain amount of lithium mica slag and put it into a ball mill for ball milling. Its specific surface area is 500m 2 / kg of granules, for future use;
[0068] 2) Mix 1 g KBM-303 and 5 g ethanol evenly to prepare a KBM-303 / ethanol mixed solution;
[0069] 3) adding 5 g of sepiolite fiber to 10 g of ethanol and dispersing by ultrasonic; further adding 3 g of potassium titanate whisker and dispersing by ultrasonic; drying to obtain a sepiolite fiber / potassium titanate whisker mixture;
[0070] 4) take 30g lepidolite slag and put it into a stirrer, carry out stirring treatment, spray 6g KBM-303 / ethanol mixed solution of step 2 on the lepidolite slag particle surface simultaneously, continue to add 5g sepiolite fiber / potassium titanate whisker mixed material to mix after the mixed solution adds, be heated to 90 DEG C of drying treatment 50min, prepare modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite.
[0071] 2. Preparation of modified amine water-based curing agent:
[0072] 1) triethylenetetramine (TETA) and bisphenol A epoxy resin E51 were weighed into a round-bottom flask at a molar ratio of 2.5:1, and the mixture was heated to 70° C. The reaction time was 3 h to prepare an epoxy-amine adduct intermediate;
[0073] 2) According to the molar ratio of 0.5:1, the double-terminal epoxy polyether and the epoxy-amine adduct intermediate were weighed into a round-bottom flask for addition reaction, heated to 90° C., and the reaction time was 3 h to prepare a modified amine water-based curing agent.
[0074] 3. The preparation method of waterborne epoxy emulsion includes:
[0075] 1) adding epoxy resin E44 and polyethylene glycol 6000 in a molar ratio of 2:1 into a round-bottom flask respectively, and heating to 85° C. under the protection of dry nitrogen, and mixing them evenly under stirring after the two are completely melted to obtain an epoxy resin E44 / polyethylene glycol 6000 blend;
[0076] 2) The catalyst BF3 ether (the amount added is 0.3% of the total mass of epoxy resin E44 and polyethylene glycol 6000) is diluted 10 times with acetone and then added dropwise to the epoxy resin E44 / polyethylene glycol 6000 blend, and the mixture is kept at 85° C. for catalytic reaction for 4 hours, and then vacuum distilled under reduced pressure until no solvent is removed, thereby obtaining an epoxy resin emulsifier;
[0077] 3) adding epoxy resin E44 and epoxy resin emulsifier into a stirring kettle, heating to 70° C., and then stirring at 1200 r / min to mix uniformly, gradually adding water into the stirring kettle, and preparing an aqueous epoxy emulsion with a solid content of 50% by a phase inversion method, wherein the mass ratio of epoxy resin E44 to epoxy resin emulsifier is 1:9.
[0078] 4. Preparation of water-based epoxy rapid repair mortar with lithium mica slag:
[0079] (1) Weigh 100 g of water-based epoxy emulsion (solid content 50%), 0.6 g of wetting agent, and 150 g of deionized water and stir evenly for 1 min, then add 50 g of modified amine water-based curing agent and 0.6 g of defoaming agent and stir evenly to prepare a multi-component mixture;
[0080] (2) Weigh 1200 g of aggregate, 600 g of P·O 52.5, 200 g of R·SAC 52.5, 30 g of modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite, and 4 g of water reducer, put them into a blender and mix them for 1 min, then add the multi-component mixture in step 1 and mix them together for 3 min. Then, form mortar specimens for relevant performance tests.
[0081] Example 2
[0082] 1. Preparation of modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite:
[0083] 1) Take a certain amount of lithium mica slag and put it into a ball mill for ball milling. Its specific surface area is 500m 2 / kg of granules, for future use;
[0084] 2) Mix 1 g KBM-303 and 5 g ethanol evenly to prepare a KBM-303 / ethanol mixed solution;
[0085] 3) adding 3 g of sepiolite fiber to 10 g of ethanol and dispersing by ultrasonic; further adding 2 g of potassium titanate whisker and dispersing by ultrasonic; drying to obtain a sepiolite fiber / potassium titanate whisker mixture;
[0086] 4) take 30g lepidolite slag and put it into a stirrer, carry out stirring treatment, spray 6g KBM-303 / ethanol mixed solution of step 2 on the lepidolite slag particle surface simultaneously, continue to add 5g sepiolite fiber / potassium titanate whisker mixed material to mix after the mixed solution adds, be heated to 90 DEG C of drying treatment 50min, prepare modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite.
[0087] 2. Preparation of modified amine water-based curing agent:
[0088] 1) triethylenetetramine (TETA) and bisphenol A epoxy resin E51 were weighed into a round-bottom flask at a molar ratio of 2.5:1, and the mixture was heated to 70° C. The reaction time was 3 h to prepare an epoxy-amine adduct intermediate;
[0089] 2) According to the molar ratio of 0.5:1, the double-terminal epoxy polyether and the epoxy-amine adduct intermediate were weighed into a round-bottom flask for addition reaction, heated to 90° C., and the reaction time was 3 h to prepare a modified amine water-based curing agent.
[0090] 3. The preparation method of waterborne epoxy emulsion includes:
[0091] 1) adding epoxy resin E44 and polyethylene glycol 6000 in a molar ratio of 2:1 into a round-bottom flask respectively, and heating to 85° C. under the protection of dry nitrogen, and mixing them evenly under stirring after the two are completely melted to obtain an epoxy resin E44 / polyethylene glycol 6000 blend;
[0092] 2) The catalyst BF3 ether (the amount added is 0.3% of the total mass of epoxy resin E44 and polyethylene glycol 6000) is diluted 10 times with acetone and then added dropwise to the epoxy resin E44 / polyethylene glycol 6000 blend, and the mixture is kept at 85° C. for catalytic reaction for 4 hours, and then vacuum distilled under reduced pressure until no solvent is removed, thereby obtaining an epoxy resin emulsifier;
[0093] 3) adding epoxy resin E44 and epoxy resin emulsifier into a stirring kettle, heating to 70° C., and then stirring at 1200 r / min to mix uniformly, gradually adding water into the stirring kettle, and preparing an aqueous epoxy emulsion with a solid content of 50% by a phase inversion method, wherein the mass ratio of epoxy resin E44 to epoxy resin emulsifier is 1:9.
[0094] 4. Preparation of Lepidolite Slag Water-based Epoxy Rapid Repair Mortar
[0095] (1) Weigh 100 g of water-based epoxy emulsion (solid content 50%), 0.6 g of wetting agent, and 150 g of deionized water and stir evenly for 1 min, then add 50 g of modified amine water-based curing agent and 0.6 g of defoaming agent and stir evenly to prepare a multi-component mixture;
[0096] (2) Weigh 1200 g of aggregate, 400 g of P·O 52.5, 400 g of R·SAC 52.5, 30 g of modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite, and 4 g of water reducer, put them into a blender and mix them for 1 min, then add the multi-component mixture in step 1 and mix them together for 3 min. Then, form mortar specimens for relevant performance tests.
[0097] Example 3
[0098] 1. Preparation of modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite:
[0099] 1) Take a certain amount of lithium mica slag and put it into a ball mill for ball milling. Its specific surface area is 500m 2 / kg of granules, for future use;
[0100] 2) Mix 2 g KBM-303 and 10 g ethanol in a certain proportion to prepare a KBM-303 / ethanol mixed solution;
[0101] 3) adding 3 g of sepiolite fiber to 10 g of ethanol and dispersing by ultrasonic; further adding 5 g of potassium titanate whisker and dispersing by ultrasonic; drying to obtain a sepiolite fiber / potassium titanate whisker mixture;
[0102] 4) take 60g lepidolite slag and put it into stirrer, carry out stirring process, spray 12g KBM-303 / ethanol mixed solution of step 2 on the lepidolite slag particle surface simultaneously, continue to add 5g sepiolite fiber / potassium titanate whisker compound to mix after mixed solution adds, be heated to 90 DEG C of drying process 50min, prepare modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite.
[0103] 2. Preparation of modified amine water-based curing agent:
[0104] 1) triethylenetetramine (TETA) and bisphenol A epoxy resin E51 were weighed into a round-bottom flask at a molar ratio of 2.5:1, and the mixture was heated to 70° C. The reaction time was 3 h to prepare an epoxy-amine adduct intermediate;
[0105] 2) According to the molar ratio of 0.5:1, the double-terminal epoxy polyether and the epoxy-amine adduct intermediate were weighed into a round-bottom flask for addition reaction, heated to 90° C., and the reaction time was 3 h to prepare a modified amine water-based curing agent.
[0106] 3. The preparation method of waterborne epoxy emulsion includes:
[0107] 1) adding epoxy resin E44 and polyethylene glycol 6000 in a molar ratio of 2:1 into a round-bottom flask respectively, and heating to 85° C. under the protection of dry nitrogen, and mixing them evenly under stirring after the two are completely melted to obtain an epoxy resin E44 / polyethylene glycol 6000 blend;
[0108] 2) The catalyst BF3 ether (the amount added is 0.3% of the total mass of epoxy resin E44 and polyethylene glycol 6000) is diluted 10 times with acetone and then added dropwise to the epoxy resin E44 / polyethylene glycol 6000 blend, and the mixture is kept at 85° C. for catalytic reaction for 4 hours, and then vacuum distilled under reduced pressure until no solvent is removed, thereby obtaining an epoxy resin emulsifier;
[0109] 3) adding epoxy resin E44 and epoxy resin emulsifier into a stirring kettle, heating to 70° C., and then stirring at 1200 r / min to mix uniformly, gradually adding water into the stirring kettle, and preparing an aqueous epoxy emulsion with a solid content of 50% by a phase inversion method, wherein the mass ratio of epoxy resin E44 to epoxy resin emulsifier is 1:9.
[0110] 4. Preparation of Lepidolite Slag Water-based Epoxy Quick Repair Mortar
[0111] (1) Weigh 100 g of water-based epoxy emulsion (solid content 50%), 0.6 g of wetting agent, and 150 g of deionized water and stir evenly for 1 min, then add 50 g of modified amine water-based curing agent and 0.6 g of defoaming agent and stir evenly to prepare a multi-component mixture;
[0112] (2) Weigh 1200 g of aggregate, 500 g of P·O 52.5, 300 g of R·SAC 52.5, 60 g of modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite, and 4 g of water reducer, put them into a blender and mix them for 1 min, then add the multi-component mixture in step 1 and mix them together for 3 min. Then, form mortar specimens for relevant performance tests.
[0113] Comparative Example 1
[0114] 1. Preparation of modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite:
[0115] 1) Take a certain amount of lithium mica slag and put it into a ball mill for ball milling. Its specific surface area is 500m 2 / kg of granules, for future use;
[0116] 2) Mix 1 g KBM-303 and 5 g ethanol evenly to prepare a KBM-303 / ethanol mixed solution;
[0117] 3) adding 1 g of sepiolite fiber to 10 g of ethanol and dispersing by ultrasonic; then adding 4 g of potassium titanate whisker and dispersing by ultrasonic; and drying to obtain a sepiolite fiber / potassium titanate whisker mixture;
[0118] 4) take 30g lepidolite slag and put it into a stirrer, carry out stirring treatment, spray 6g KBM-303 / ethanol mixed solution of step 2 on the lepidolite slag particle surface simultaneously, continue to add 5g sepiolite fiber / potassium titanate whisker mixed material to mix after the mixed solution adds, be heated to 90 DEG C of drying treatment 50min, prepare modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite.
[0119] 2. Preparation of modified amine water-based curing agent:
[0120] 1) triethylenetetramine (TETA) and bisphenol A epoxy resin E51 were weighed into a round-bottom flask at a molar ratio of 2.5:1, and the mixture was heated to 70° C. for 3 h to prepare an epoxy-amine adduct intermediate;
[0121] 2) According to the molar ratio of 0.5:1, the double-terminal epoxy polyether and the epoxy-amine adduct intermediate were weighed into a round-bottom flask for addition reaction, heated to 90° C., and the reaction time was 3 h to prepare a modified amine water-based curing agent.
[0122] 3. The preparation method of waterborne epoxy emulsion includes:
[0123] 1) adding epoxy resin E44 and polyethylene glycol 6000 in a molar ratio of 2:1 into a round-bottom flask respectively, and heating to 85° C. under the protection of dry nitrogen, and mixing them evenly under stirring after the two are completely melted to obtain an epoxy resin E44 / polyethylene glycol 6000 blend;
[0124] 2) The catalyst BF3 ether (the amount added is 0.3% of the total mass of epoxy resin E44 and polyethylene glycol 6000) is diluted 10 times with acetone and then added dropwise to the epoxy resin E44 / polyethylene glycol 6000 blend, and the mixture is kept at 85° C. for catalytic reaction for 4 hours, and then vacuum distilled under reduced pressure until no solvent is removed, thereby obtaining an epoxy resin emulsifier;
[0125] 3) adding epoxy resin E44 and epoxy resin emulsifier into a stirring kettle, heating to 70° C., and then stirring at 1200 r / min to mix uniformly, gradually adding water into the stirring kettle, and preparing an aqueous epoxy emulsion with a solid content of 50% by a phase inversion method, wherein the mass ratio of epoxy resin E44 to epoxy resin emulsifier is 1:9.
[0126] 4. Preparation of Lepidolite Slag Water-based Epoxy Rapid Repair Mortar
[0127] (1) Weigh 100 g of water-based epoxy emulsion (solid content 50%), 0.6 g of wetting agent, and 150 g of deionized water and stir them evenly for 1 min, then add 50 g of modified amine water-based curing agent and 0.6 g of defoaming agent and stir them evenly to prepare a multi-component mixture;
[0128] (2) Weigh 1200 g of aggregate, 800 g of P·O 52.5, 30 g of modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite, and 4 g of water reducer, put them into a blender and mix them for 1 min, then add the multi-component mixture in step 1 and mix them together for 3 min. Then, form mortar specimens for relevant performance tests.
[0129] Comparative Example 2
[0130] 1. Preparation of modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite:
[0131] 1) Take a certain amount of lithium mica slag and put it into a ball mill for ball milling. Its specific surface area is 500m 2 / kg of granules, for future use;
[0132] 2) Mix 2 g KBM-303 and 10 g ethanol to prepare a KBM-303 / ethanol mixture;
[0133] 3) adding 2 g of sepiolite fiber to 10 g of ethanol and dispersing by ultrasonic; further adding 3 g of potassium titanate whisker and dispersing by ultrasonic; drying to obtain a sepiolite fiber / potassium titanate whisker mixture;
[0134] 4) take 30g lepidolite slag and put it into stirrer, carry out stirring process, spray 12g KBM-303 / ethanol mixed solution of step 2 to the lepidolite slag particle surface simultaneously, continue to add 5g sepiolite fiber / potassium titanate whisker compound to mix after mixed solution adds, be heated to 90 DEG C of drying process 50min, prepare modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite.
[0135] 2. Preparation of modified amine water-based curing agent:
[0136] 1) triethylenetetramine (TETA) and bisphenol A epoxy resin E51 were weighed into a round-bottom flask at a molar ratio of 2.5:1, and the mixture was heated to 70° C. The reaction time was 3 h to prepare an epoxy-amine adduct intermediate;
[0137] 2) According to the molar ratio of 0.5:1, the double-terminal epoxy polyether and the epoxy-amine adduct intermediate were weighed into a round-bottom flask for addition reaction, heated to 90° C., and the reaction time was 3 h to prepare a modified amine water-based curing agent.
[0138] 3. The preparation method of waterborne epoxy emulsion includes:
[0139] 1) adding epoxy resin E44 and polyethylene glycol 6000 in a molar ratio of 2:1 into a round-bottom flask respectively, and heating to 85° C. under the protection of dry nitrogen, and mixing them evenly under stirring after the two are completely melted to obtain an epoxy resin E44 / polyethylene glycol 6000 blend;
[0140] 2) The catalyst BF3 ether (the amount added is 0.3% of the total mass of epoxy resin E44 and polyethylene glycol 6000) is diluted 10 times with acetone and then added dropwise to the epoxy resin E44 / polyethylene glycol 6000 blend, and the mixture is kept at 85° C. for catalytic reaction for 4 hours, and then vacuum distilled under reduced pressure until no solvent is removed, thereby obtaining an epoxy resin emulsifier;
[0141] 3) adding epoxy resin E44 and epoxy resin emulsifier into a stirring kettle, heating to 70° C., and then stirring at 1200 r / min to mix uniformly, gradually adding water into the stirring kettle, and preparing an aqueous epoxy emulsion with a solid content of 50% by a phase inversion method, wherein the mass ratio of epoxy resin E44 to epoxy resin emulsifier is 1:9.
[0142] 4. Preparation of Lepidolite Slag Water-based Epoxy Rapid Repair Mortar
[0143] (1) Weigh 100 g of water-based epoxy emulsion (solid content 50%), 0.6 g of wetting agent, and 150 g of deionized water and stir them evenly for 1 min, then add 50 g of modified amine water-based curing agent and 0.6 g of defoaming agent and stir them evenly to prepare a multi-component mixture;
[0144] (2) Weigh 1200 g of aggregate, 800 g of P·O 52.5, 30 g of modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite, and 4 g of water reducer, put them into a blender and mix them for 1 min, then add the multi-component mixture in step 1 and mix them together for 3 min. Then, form mortar specimens for relevant performance tests.
[0145] Comparative Example 3
[0146] 1. Preparation of modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite:
[0147] 1) Take a certain amount of lithium mica slag and put it into a ball mill for ball milling. Its specific surface area is 500m 2 / kg of granules, for future use;
[0148] 2) Mix 2 g KBM-303 / ethanol and 10 g ethanol evenly to prepare a KBM-303 / ethanol mixed solution;
[0149] 3) adding 3 g of sepiolite fiber to 10 g of ethanol and dispersing by ultrasonic; further adding 5 g of potassium titanate whisker and dispersing by ultrasonic; drying to obtain a sepiolite fiber / potassium titanate whisker mixture;
[0150] 4) take 60g lepidolite slag and put it into stirrer, carry out stirring process, spray 12g KBM-303 / ethanol mixed solution of step 2 on the lepidolite slag particle surface simultaneously, continue to add 5g sepiolite fiber / potassium titanate whisker compound to mix after mixed solution adds, be heated to 90 DEG C of drying process 50min, prepare modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite.
[0151] 2. Preparation of modified amine water-based curing agent:
[0152] 1) triethylenetetramine (TETA) and bisphenol A epoxy resin E51 were weighed into a round-bottom flask at a molar ratio of 2.5:1, and the mixture was heated to 70° C. The reaction time was 3 h to prepare an epoxy-amine adduct intermediate;
[0153] 2) According to the molar ratio of 0.5:1, the double-terminal epoxy polyether and the epoxy-amine adduct intermediate were weighed into a round-bottom flask for addition reaction, heated to 90° C., and the reaction time was 3 h to prepare a modified amine water-based curing agent.
[0154] 3. The preparation method of waterborne epoxy emulsion includes:
[0155] 1) adding epoxy resin E44 and polyethylene glycol 6000 in a molar ratio of 2:1 into a round-bottom flask respectively, and heating to 85° C. under the protection of dry nitrogen, and mixing them evenly under stirring after the two are completely melted to obtain an epoxy resin E44 / polyethylene glycol 6000 blend;
[0156] 2) The catalyst BF3 ether (the amount added is 0.3% of the total mass of epoxy resin E44 and polyethylene glycol 6000) is diluted 10 times with acetone and then added dropwise to the epoxy resin E44 / polyethylene glycol 6000 blend, and the mixture is kept at 85° C. for catalytic reaction for 4 hours, and then vacuum distilled under reduced pressure until no solvent is removed, thereby obtaining an epoxy resin emulsifier;
[0157] 3) adding epoxy resin E44 and epoxy resin emulsifier into a stirring kettle, heating to 70° C., and then stirring at 1200 r / min to mix uniformly, gradually adding water into the stirring kettle, and preparing an aqueous epoxy emulsion with a solid content of 50% by a phase inversion method, wherein the mass ratio of epoxy resin E44 to epoxy resin emulsifier is 1:9.
[0158] 4. Preparation of Lepidolite Slag Water-based Epoxy Rapid Repair Mortar
[0159] (1) Weigh 100 g of water-based epoxy emulsion (solid content 50%), 0.6 g of wetting agent, and 150 g of deionized water and stir them evenly for 1 min, then add 50 g of modified amine water-based curing agent and 0.6 g of defoaming agent and stir them evenly to prepare a multi-component mixture;
[0160] (2) Weigh 1200 g of aggregate, 800 g of P·O 52.5, 60 g of modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite, and 4 g of water reducer, put them into a blender and mix them for 1 min, then add the multi-component mixture in step 1 and mix them together for 3 min. Then, form mortar specimens for relevant performance tests.
[0161] Comparative Example 4
[0162] 1. Preparation of modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite:
[0163] 1) Take a certain amount of lithium mica slag and put it into a ball mill for ball milling. Its specific surface area is 500m 2 / kg of granules, for future use;
[0164] 2) Mix 1 g KBM-303 and 5 g ethanol evenly to prepare a KBM-303 / ethanol mixed solution;
[0165] 3) adding 4 g of sepiolite fiber to 10 g of ethanol and dispersing by ultrasonic; further adding 1 g of potassium titanate whisker and dispersing by ultrasonic; drying to obtain a sepiolite fiber / potassium titanate whisker mixture;
[0166] 4) take 30g lepidolite slag and put it into a stirrer, carry out stirring treatment, spray 6g KBM-303 / ethanol mixed solution of step 2 on the lepidolite slag particle surface simultaneously, continue to add 5g sepiolite fiber / potassium titanate whisker mixed material to mix after the mixed solution adds, be heated to 90 DEG C of drying treatment 50min, prepare modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite.
[0167] 2. Preparation of modified amine water-based curing agent:
[0168] 1) triethylenetetramine (TETA) and bisphenol A epoxy resin E51 were weighed into a round-bottom flask at a molar ratio of 2.5:1, and the mixture was heated to 70° C. The reaction time was 3 h to prepare an epoxy-amine adduct intermediate;
[0169] 2) According to the molar ratio of 0.5:1, the double-terminal epoxy polyether and the epoxy-amine adduct intermediate were weighed into a round-bottom flask for addition reaction, heated to 90° C., and the reaction time was 3 h to prepare a modified amine water-based curing agent.
[0170] 3. The preparation method of waterborne epoxy emulsion includes:
[0171] 1) adding epoxy resin E44 and polyethylene glycol 6000 in a molar ratio of 2:1 into a round-bottom flask respectively, and heating to 85° C. under the protection of dry nitrogen, and mixing them evenly under stirring after the two are completely melted to obtain an epoxy resin E44 / polyethylene glycol 6000 blend;
[0172] 2) The catalyst BF3 ether (the amount added is 0.3% of the total mass of epoxy resin E44 and polyethylene glycol 6000) is diluted 10 times with acetone and then added dropwise to the epoxy resin E44 / polyethylene glycol 6000 blend, and the mixture is kept at 85° C. for catalytic reaction for 4 hours, and then vacuum distilled under reduced pressure until no solvent is removed, thereby obtaining an epoxy resin emulsifier;
[0173] 3) adding epoxy resin E44 and epoxy resin emulsifier into a stirring kettle, heating to 70° C., and then stirring at 1200 r / min to mix uniformly, gradually adding water into the stirring kettle, and preparing an aqueous epoxy emulsion with a solid content of 50% by a phase inversion method, wherein the mass ratio of epoxy resin E44 to epoxy resin emulsifier is 1:9.
[0174] 4. Preparation of Lepidolite Slag Water-based Epoxy Rapid Repair Mortar
[0175] (1) Weigh 120 g of water-based epoxy emulsion (solid content 50%), 0.6 g of wetting agent, and 140 g of deionized water and stir evenly for 1 min, then add 60 g of modified amine water-based curing agent and 0.6 g of defoaming agent and stir evenly to prepare a multi-component mixture;
[0176] (2) Weigh 1200 g of aggregate, 800 g of P·O 52.5, 30 g of modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite, and 4 g of water reducer, put them into a blender and mix them for 1 min, then add the multi-component mixture in step 1 and mix them together for 3 min. Then, form mortar specimens for relevant performance tests.
[0177] Comparative Example 5
[0178] The difference from Example 1 is that the "modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite" is removed, and the rest is the same as Example 1.
[0179] Comparative Example 6
[0180] The difference from Example 1 is that the "modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite" is changed to "modified lepidolite slag", that is, sepiolite fiber and lithium titanate whisker are not added, and the rest is the same as Example 1.
[0181] Comparative Example 7
[0182] The difference from Example 1 is that the "modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite" is changed to "unmodified lepidolite slag, sepiolite fiber, lithium titanate whisker", and the preparation method is modified to:
[0183] 1) Take a certain amount of lithium mica slag and put it into a ball mill for ball milling. Its specific surface area is 400m 2 / kg of granules, for future use;
[0184] 2) adding 3 g of sepiolite fiber to 10 g of ethanol and dispersing by ultrasonic; further adding 2 g of potassium titanate whisker and dispersing by ultrasonic; drying to obtain a sepiolite fiber / potassium titanate whisker mixture;
[0185] 4) 30 g of lepidolite slag was put into a blender for stirring, and 5 g of sepiolite fiber / potassium titanate whisker mixture was added and mixed evenly to obtain a mixture of non-modified lepidolite slag, sepiolite fiber and lithium titanate whisker.
[0186] The rest is the same as Example 1.
[0187] Comparative Example 8
[0188] The difference from Example 1 is that the modified amine water-based curing agent is replaced with a commercially available amine curing agent, and the rest is the same as Example 1.
[0189] The specific addition amounts of each raw material in Examples 1 to 3 and Comparative Examples 1 to 8 are shown in Table 1.
[0190] Table 1 Specific addition amount of each raw material in Examples 1 to 3 and Comparative Examples 1 to 8
[0191]
[0192]
[0193] The performance tests of the lithium mica slag water-based epoxy quick repair mortars of Examples 1-3 and Comparative Examples 1-8 and commercially available ordinary mortars were carried out, and the performance tests were carried out according to the following standards: (1) the setting time was tested according to Chapter 5 of DL / T 5126-2001 "Test Procedure for Polymer Modified Cement Mortar"; (2) the compressive strength and flexural strength were tested according to Chapter 9 of GB / T17671-1999 "Test Method for Strength of Cement Mortar"; (3) the tensile bond strength was tested according to Chapter 5 of JC / T907-2002 "Concrete Interface Treatment Agent"; (4) the shrinkage rate was tested according to Chapter 12 of JCJ 70-2009 "Test Method for Basic Performance of Building Mortar".
[0194] Table 2 Performance test of lithium mica slag water-based epoxy rapid repair mortar of Examples 1-3 and Comparative Examples 1 to 4
[0195]
[0196]
[0197] Table 3 Performance test of lithium mica slag water-based epoxy rapid repair mortar of comparative examples 5 to 8
[0198]
[0199] It can be seen from Tables 2 to 3 that, compared with commercially available ordinary epoxy mortar, the compressive strength, flexural strength and tensile bond strength of the repair mortar prepared in Examples 1 to 3 of the present invention are significantly better than those of commercially available ordinary epoxy mortar, and the setting time is shorter than that of commercially available ordinary epoxy mortar, which can achieve rapid repair.
[0200] Compared with comparative examples 1 to 4 (all without adding sulphoaluminate cement), it can be seen that the setting time of the repair mortar prepared in Examples 1 to 3 of the present invention is shorter than that of comparative examples 1 to 4, which indicates that the present invention adopts the common silicate / sulphoaluminate cement blending modification to accelerate the mortar repair speed.
[0201] Compared with Comparative Examples 5 to 7, it can be seen that the compressive strength, flexural strength and tensile bond strength of the repair mortar prepared in Examples 1 to 3 are significantly better than those in Comparative Example 5 (modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite not added), Comparative Example 6 (no sepiolite fiber and lithium titanate whisker added), and Comparative Example 7 (using non-modified lepidolite slag, sepiolite fiber, lithium titanate whisker). This shows that whether to add modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite, the amount of modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite, whether to add sepiolite fiber and lithium titanate whisker, and whether to modify lepidolite slag, sepiolite fiber, and lithium titanate whisker will affect the compressive strength, flexural strength and tensile bond strength of the prepared repair mortar.
[0202] Compared with Comparative Example 8, it can be seen that the setting time of the repair mortar prepared in Examples 1 to 3 is significantly shorter than that in Comparative Example 8, which indicates that whether the curing agent is modified will affect the setting time of the repair mortar.
[0203] Therefore, the present invention can improve the performance of the mortar by adding the modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite. Specifically, the finely ground lepidolite slag is mostly flaky and round particles, has good reinforcement and bulk density, can reduce the gaps and defects between the resin matrix and the aggregate, improve the compressive strength of the mortar, and can improve the flexural strength and tensile bonding strength of the mortar; and the present invention performs mixed modification on the lepidolite slag, sepiolite fiber, and lithium titanate whisker, which can reduce the sepiolite fiber and lithium titanate whisker. The reunion of whiskers makes sepiolite fiber and lithium titanate whisker evenly dispersed in the lithium mica slag, and the addition of epoxy group silane coupling agent further enhances the compactness between the modified lithium mica slag / sepiolite fiber / lithium titanate whisker composite and the polymer, so that sepiolite fiber and lithium titanate whisker can finally be evenly dispersed in cement, and the modified sepiolite fiber, lithium titanate whisker and lithium mica slag can work together to significantly improve the impermeability, crack resistance, dimensional stability, compressive strength, flexural strength and tensile bond strength of the mortar. On the other hand, the present invention modifies the curing agent, which can accelerate the repair speed of the mortar. And the present invention also modifies the ordinary silicate and sulphoaluminate cement blending and can also accelerate the mortar repair speed.
[0204] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A lithium mica slag water-based epoxy quick repair mortar, characterized in that: The preparation comprises the following raw materials in parts by weight: 1100-1300 parts of aggregate, 400-600 parts of ordinary Portland cement, 200-400 parts of sulphoaluminate cement, 100-120 parts of water-based epoxy emulsion, 0.5-0.7 parts of defoamer, 0.5-0.7 parts of wetting agent, 3-5 parts of water reducer, 140-160 parts of deionized water, 30-60 parts of modified lithium mica slag / sepiolite fiber / lithium titanate whisker composite, and 50-60 parts of modified amine water-based curing agent.
2. A lithium mica slag water-based epoxy rapid repair mortar according to claim 1, characterized in that: The preparation comprises the following raw materials in parts by weight: 1150-1250 parts of aggregate, 450-550 parts of ordinary Portland cement, 250-350 parts of sulphoaluminate cement, 105-115 parts of water-based epoxy emulsion, 0.55-0.65 parts of defoamer, 0.55-0.65 parts of wetting agent, 3.5-4.5 parts of water reducer, 145-155 parts of deionized water, 40-50 parts of modified lithium mica slag / sepiolite fiber / lithium titanate whisker composite, and 52-58 parts of modified amine water-based curing agent.
3. A lithium mica slag water-based epoxy rapid repair mortar according to claim 1, characterized in that: The preparation method of the modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite comprises: The lithium mica slag is ball-milled to obtain a specific surface area of 200-800m 2 / kg of lithium mica slag particles; Evenly mixing the epoxy group silane coupling agent and ethanol to prepare an epoxy group silane coupling agent / ethanol mixed solution; Adding sepiolite fiber into ethanol, ultrasonically dispersing, adding potassium titanate whisker, ultrasonically dispersing, and drying to obtain a sepiolite fiber / potassium titanate whisker mixture; The lepidolite slag particles are stirred, and the epoxy group silane coupling agent / ethanol mixed solution is sprayed on the surface of the lepidolite slag particles, and the sepiolite fiber and potassium titanate whisker mixture is added and stirred evenly, and then heated to 80-100° C. for 30-90 minutes to obtain a modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite.
4. A lithium mica slag water-based epoxy rapid repair mortar according to claim 3, characterized in that: In the preparation method of the modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite, the mass ratio of the epoxy group silane coupling agent to ethanol is 1-2:5-10, the mass ratio of the lepidolite slag to the epoxy group silane coupling agent is 30-60:1-2, and the mass ratio of the lepidolite slag, sepiolite fiber, and potassium titanate whisker is 30-60:1-5:1-5.
5. A lithium mica slag water-based epoxy rapid repair mortar according to claim 3, characterized in that: The epoxy group silane coupling agent is at least one of KBM-303, KBM-403 and KBE-402.
6. A lithium mica slag water-based epoxy rapid repair mortar according to claim 1, characterized in that: The preparation method of the modified amine water-based curing agent comprises: Triethylenetetramine and bisphenol A epoxy resin are reacted at 60-70°C for 3-5h to obtain an epoxy-amine adduct intermediate; The double-terminal epoxy polyether is reacted with the epoxy-amine adduct intermediate at 90-100° C. for 2-5 hours to obtain a modified amine water-based curing agent.
7. A lithium mica slag water-based epoxy rapid repair mortar according to claim 6, characterized in that: In the preparation method of the modified amine water-based curing agent, the molar ratio of the triethylenetetramine to the bisphenol A epoxy resin is 2-3:1; the molar ratio of the double-terminal epoxy polyether to the epoxy-amine adduct intermediate is 0.3-0.7:
1.
8. A lithium mica slag water-based epoxy rapid repair mortar according to claim 1, characterized in that: The preparation method of the aqueous epoxy emulsion comprises: 1) adding epoxy resin E44 and polyethylene glycol 6000 in a molar ratio of 2:1 into a round-bottom flask respectively, and heating to 85° C. under the protection of dry nitrogen, and mixing them evenly under stirring after the two are completely melted to obtain an epoxy resin E44 / polyethylene glycol 6000 blend; 2) The catalyst BF3 ether was diluted 10 times with acetone and then added dropwise to the epoxy resin E44 / polyethylene glycol 6000 blend, and the mixture was kept at 85°C for catalytic reaction for 4 hours, and then vacuum distilled until no solvent was removed, thereby obtaining an epoxy resin emulsifier; 3) adding epoxy resin E44 and epoxy resin emulsifier into a stirring kettle, heating to 70° C., stirring and mixing at 1000-1500 r / min, gradually adding water into the stirring kettle, and preparing an aqueous epoxy emulsion with a solid content of 40%-60% by a phase inversion method, wherein the mass ratio of epoxy resin E44 to epoxy resin emulsifier is 1:
9.
9. A lithium mica slag water-based epoxy rapid repair mortar according to claim 1, characterized in that: The aggregate is artificial sand or natural sand with a particle size of less than 4.75 mm and a mud content of ≤0.45wt%; The ordinary Portland cement is at least one of P·O 42.5, 52.5, and 62.5, and the sulphoaluminate cement is fast-hardening sulphoaluminate cement.
10. A method for preparing the lepidolite slag water-based epoxy rapid repair mortar according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Weigh the water-based epoxy emulsion, wetting agent and deionized water in proportion and stir them evenly for 0.5-2 minutes, then add the modified amine water-based curing agent and defoaming agent respectively and stir them evenly to prepare a multi-component mixture; S2. Weigh aggregate, ordinary Portland cement, sulphoaluminate cement, modified lepidolite slag / sepiolite fiber / lithium titanate whisker composite, and water reducer in proportion, mix and stir for 0.5-2 minutes, add the multi-component mixture in step S1, and stir together for 3-5 minutes to prepare lepidolite slag water-based epoxy quick repair mortar.
Citation Information
Patent Citations
Repairing mortar for polymer rapid reinforcement
CN112551995A
Waterproof coating for wall surface and preparation method thereof
CN114133824A
Preparation method and application of collapsible loess curing agent
CN114573305A
Lipidolite slag concrete
CN115872695A