Filling cementing material and preparation method thereof

By mixing phosphate flotation tailings, phosphogypsum and alkali slag with water glass and acrylate copolymerization emulsion, a filling gelling material with high mechanical properties is solved, and the stability of solid waste in fillers and building materials is achieved. The effective utilization of phosphogypsum, phospho ore flotation tailings and alkali slag has been reduced, and the use of cement has been improved, and the compactness and compressive flexural strength of the material have been improved.

CN118908684AActive Publication Date: 2024-11-08KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411007503.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The long-term stability of solid waste such as phosphogypsum, phospho ore flotation tailings and alkali slags in fillers and building materials is common, and the overall utilization rate is not high, so it cannot fundamentally solve the large accumulation of these solid wastes and Environmental pollution problems.

Method used

Using a preparation method of filling gelling materials, the high-quality is formed by mixing phosphate flotation tailings, phosphogypsum and alkali slag and adding water glass and acrylate copolymer emulsion as a curing accelerator. Filled gelling material with mechanical properties and compactness.

Benefits of technology

It effectively improves the doping amount of phosphate flotation tailings, phosphogypsum and alkali slag, improves the mechanical strength, toughness, impact resistance and water resistance of the filled gelling materials, and solves the accumulation problem of three kinds of solid wastes. Enhances the stability and compactness of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908684A_ABST
    Figure CN118908684A_ABST
Patent Text Reader

Abstract

The invention discloses a filling cementing material and a preparation method thereof, and belongs to the technical field of resource utilization of solid wastes. The preparation method comprises the following steps: uniformly mixing cement, phosphate tailing powder, flotation ardealite and alkaline residues to obtain a dry mixture; uniformly mixing the dry mixture, water and a curing accelerator to obtain a wet mixture; and finally, putting the wet mixture into a prefabricated mold, pressing the mold, demolding and curing to obtain the filling cementing material. According to the treated filling cementing material, the PO4 < 3-> curing effect is remarkable, and F <-> and measured heavy metal in leachate are within the range specified by the Integrated Wastewater Discharge Standard (GB8978-1996). Meanwhile, the filling cementing material has good mechanical properties, can be used as a building material and pavement infrastructure, has the characteristics of simple process flow, energy conservation, environmental protection, safety, reliability and the like, and has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of resource utilization of solid wastes, and in particular relates to a filling gelling material and a preparation method thereof. Background Art

[0002] Phosphogypsum is a byproduct of wet phosphoric acid preparation. Its main component is CaSO4·2H2O. The production of 1 ton of phosphoric acid will produce about 5 tons of phosphogypsum. It is estimated that more than 200 million to 300 million tons of phosphogypsum will be produced worldwide each year, and China will produce more than 60 million tons. At present, the main treatment method for phosphogypsum in China is stacking. The storage of large amounts of phosphogypsum not only occupies a large amount of land, but also pollutes groundwater, soil and atmosphere for a long time, and damages the surrounding ecological environment. The arbitrary stacking and discharge of phosphogypsum restricts the sustainable development of wet phosphoric acid, phosphate fertilizer and other industries. Therefore, how to promote the reduction and resource utilization of phosphogypsum has become an urgent problem to be solved.

[0003] Phosphate ore flotation tailings are produced during the flotation process of phosphate ore. They are mainly composed of dolomite (CaMg(CO3)2), fluoroapatite (Ca5(PO4)3F), CaSO4·2H2O, SiO2 and other impurities. Usually, the weight percentage of P2O5 in phosphate ore flotation tailings is less than 10%, and the weight percentage of MgO is greater than 15%. Only 7% of phosphate ore flotation tailings in the world are recycled as building materials, agricultural fertilizers, ceramsite and magnesium sulfate. 93% of phosphate ore flotation tailings are directly discarded in tailings fields without any treatment, occupying a large amount of farmland and causing serious ecological pollution.

[0004] Alkali residue is the alkaline waste residue discharged during the alkali production and alkali treatment process in industrial production, including the waste residue discharged during the ammonium alkali method and the alkaline waste residue discharged from other industrial production processes. The components of alkali residue mainly include waste residues with calcium salts such as calcium carbonate, calcium sulfate, and calcium chloride as the main components, and also contain a small amount of sulfur dioxide and other components. Alkali residue is a by-product obtained by refining and alkali washing of gasoline, diesel, liquefied gas and other products of the refinery. It mainly contains free alkali, sodium phenol, sodium cyclohexane acid, neutral oil, water and various sulfides. Alkali residue treatment has always been a bottleneck restricting the development of the soda ash industry at home and abroad. Most alkali plants have long adopted a mixed emission method, which has brought certain pollution to the environment. With the improvement of national environmental governance policies and regulations, the treatment of alkali residue generated by the soda ash industry is also imminent.

[0005] At present, there has been great progress in the research on resource utilization of the above three solid wastes at home and abroad. However, there are common problems with the long-term stability of fillers for the three solid wastes as road infrastructure materials and building materials, and the overall utilization rate of the three solid wastes is not high, which cannot fundamentally solve the problem of large-scale accumulation and storage of the above three solid wastes. Therefore, it is still of great significance to develop a curing accelerator to simultaneously solidify and stabilize the three solid wastes. Summary of the invention

[0006] In view of the above-mentioned shortcomings of the prior art, the present invention provides a filling gelling material and a preparation method thereof.

[0007] To achieve the above object, the technical solution adopted by the present invention is:

[0008] A method for preparing a filling gelling material comprises the following steps:

[0009] (1) crushing and sieving the phosphate ore flotation tailings to obtain phosphate tailings powder; then flotation treating the phosphogypsum and drying it to obtain flotation phosphogypsum;

[0010] (2) mixing cement, phosphate tailings powder, flotation phosphogypsum and alkali residue to obtain a dry mix;

[0011] (3) mixing the dry mix, water and curing accelerator to obtain a wet mix;

[0012] (4) The wet mixed material is placed in a prefabricated mold, and the mold is pressed, demoulded, and cured to obtain a filling gelling material.

[0013] As a preferred embodiment of the present invention, the flotation treatment is froth flotation.

[0014] As a preferred embodiment of the present invention, the curing accelerator comprises water glass and acrylate copolymer emulsion, and the mass ratio of water glass to acrylate copolymer emulsion is 6:5-12.

[0015] As a preferred embodiment of the present invention, the mass ratio of the cement, phosphate tailings powder, flotation phosphogypsum and alkali slag is (1-2):(2-3):(2-3):(1-2).

[0016] More preferably, the mass ratio of the cement, phosphate tailings powder, flotation phosphogypsum and alkali slag is 2:3:3:2. Under this ratio, the pH of the filling cementitious material is 7.0-9.0, at which the mechanical properties and density are optimal.

[0017] In the present invention, the addition ratio of phosphate ore flotation tailings and phosphogypsum is as close as possible, and the addition amount of alkali slag is reduced, which can ensure that the use of cement is minimized on the basis of the density and mechanical properties of the filling cementitious material. The present invention uses phosphogypsum after flotation, which can reduce PO4 3-The leaching of organic matter improves the unconfined compressive strength of the gel material.

[0018] As a preferred embodiment of the present invention, the mass ratio of the dry mix to water is 5:(1-3); the mass of the curing accelerator is 1% to 3% of the total mass of the dry mix and water.

[0019] More preferably, the mass ratio of the dry mix to water is 5:2; when the mass of the curing accelerator is 2% of the total mass of the dry mix and water, the compressive and flexural strengths of the filling cementitious material are optimal.

[0020] As a preferred embodiment of the present invention, the pressure of the compression mold is 40-60 MPa and the time is 15-25 hours.

[0021] As a preferred embodiment of the present invention, the curing temperature is 10-30° C., the time is 20-40 days, and the relative humidity is 80-90%.

[0022] More preferably, when the curing temperature is 20° C., the curing time is 30 days and the relative humidity is 85%, the compressive and flexural strengths of the filling cementitious material are optimal.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The present invention uses phosphate ore flotation tailings, phosphogypsum and alkali slag to synergize, and cooperates with a curing accelerator to increase the doping amount of phosphate ore flotation tailings, phosphogypsum and alkali slag, thereby improving the mechanical strength, toughness, impact resistance and water resistance of the filling cementitious material. In addition, water glass and acrylic copolymer emulsion synergize to increase the doping amount of phosphate ore flotation tailings, phosphogypsum and alkali slag on the one hand; on the other hand, it increases the PO4 3- and F - of solidification.

[0025] (2) The present invention solidifies and stabilizes three solid wastes, namely, phosphate ore flotation tailings, phosphogypsum and alkali slag, thereby effectively solving the current accumulation problem of the three solid wastes. At the same time, phosphate ore flotation tailings, phosphogypsum and alkali slag can interact with each other in the medium of water and cement to generate substances such as sodium silicate hydrate (CSH), calcium aluminosilicate hydrate (CASH), and calcium phosphate compounds, thereby enhancing the strength, stability, and density of the filling cementitious material. Moreover, phosphogypsum and phosphate tailing powder produce an alkali excitation effect under the action of alkali slag, which promotes the dissolution of phosphogypsum and accelerates the reaction process. Unreacted phosphate tailing powder can also fill the pores of the solidified body and increase its density. Water glass can regulate the crystal growth mode of cement gel material to form more fine and uniform crystals, thereby improving the density and mechanical properties of the solidified body. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1This is a process flow chart for preparing filling cementitious materials. DETAILED DESCRIPTION

[0027] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0028] Example 1

[0029] A method for preparing a filling gelling material comprises the following steps:

[0030] (1) crushing the phosphate ore flotation tailings through a 100-mesh sieve to obtain phosphate tailings powder; then flotating the phosphogypsum and drying it to obtain flotation phosphogypsum.

[0031] (2) Cement, phosphate tailings powder, flotation phosphogypsum and alkali slag are mixed in a mass ratio of 1:2:3:1 to obtain a dry mix.

[0032] (3) The dry mixture and water are mixed at a mass ratio of 5:1, and the mass of the curing accelerator is 1% of the total mass of the dry mixture and water to obtain a wet mixture; the curing accelerator includes water glass and acrylic copolymer emulsion, and the mass ratio of the water glass and the acrylic copolymer emulsion is 6:10.

[0033] (4) The wet mixture is placed in a prefabricated mold, subjected to compression molding, demoulding, and curing to obtain a filling gelling material; the compression molding pressure is 50 MPa, the time is 20 h; the curing temperature is 20° C., the time is 30 days, and the relative humidity is 85%.

[0034] The obtained filling gelling material was subjected to leaching test, PO4 3- 6.8mg / L, F - The measured heavy metals are all within the range specified in GB8978-1996.

[0035] Unconfined compressive strength of filling cementitious material: 7d: 6.5MPa; 28d: 8.3MPa; 90d: 12.8MPa.

[0036] Example 2

[0037] A method for preparing a filling gelling material comprises the following steps:

[0038] (1) crushing the phosphate ore flotation tailings through a 100-mesh sieve to obtain phosphate tailings powder; then flotating the phosphogypsum and drying it to obtain flotation phosphogypsum.

[0039] (2) Cement, phosphate tailings powder, flotation phosphogypsum and alkali residue are mixed in a mass ratio of 2:3:3:1 to obtain a dry mix.

[0040] (3) The dry mixture and water are mixed at a mass ratio of 5:3, and the mass of the curing accelerator is 1% of the total mass of the dry mixture and water to obtain a wet mixture; the curing accelerator includes water glass and acrylic copolymer emulsion, and the mass ratio of the water glass and the acrylic copolymer emulsion is 6:5.

[0041] (4) The wet mixture is placed in a prefabricated mold, subjected to compression molding, demoulding, and curing to obtain a filling gelling material; the compression molding pressure is 40 MPa, the time is 15 h; the curing temperature is 10° C., the time is 10 days, and the relative humidity is 90%.

[0042] The obtained filling gelling material was subjected to leaching test, PO4 3- 7.2mg / L, F - The measured heavy metals are all within the range specified in GB8978-1996.

[0043] Unconfined compressive strength of filling cementitious material: 7d: 6.2MPa; 28d: 8.2MPa; 90d: 12.5MPa.

[0044] Example 3

[0045] A method for preparing a filling gelling material comprises the following steps:

[0046] (1) crushing the phosphate ore flotation tailings through a 100-mesh sieve to obtain phosphate tailings powder; then flotating the phosphogypsum and drying it to obtain flotation phosphogypsum.

[0047] (2) Cement, phosphate tailings powder, flotation phosphogypsum and alkali slag are mixed in a mass ratio of 2:3:3:2 to obtain a dry mix.

[0048] (3) The dry mixture and water are mixed at a mass ratio of 5:2, and the mass of the curing accelerator is 2% of the total mass of the dry mixture and water to obtain a wet mixture; the curing accelerator includes water glass and acrylic copolymer emulsion, and the mass ratio of the water glass and the acrylic copolymer emulsion is 6:12.

[0049] (4) The wet mixture is placed in a prefabricated mold, subjected to compression molding, demoulding, and curing to obtain a filling gelling material; the compression molding pressure is 60 MPa, the time is 25 h; the curing temperature is 30° C., the time is 40 days, and the relative humidity is 80%.

[0050] The obtained filling gelling material was subjected to leaching test, PO4 3- 4.1mg / L, F - The measured heavy metals are all within the range specified in GB8978-1996.

[0051] Unconfined compressive strength of filling cementitious material: 7d: 6.9MPa; 28d: 9.1MPa; 90d: 13.9MPa.

[0052] Example 4

[0053] A method for preparing a filling gelling material comprises the following steps:

[0054] (1) crushing the phosphate ore flotation tailings through a 100-mesh sieve to obtain phosphate tailings powder; then flotating the phosphogypsum and drying it to obtain flotation phosphogypsum.

[0055] (2) Cement, phosphate tailings powder, flotation phosphogypsum and alkali slag are mixed in a mass ratio of 2:3:2:2 to obtain a dry mix.

[0056] (3) The dry mixture and water are mixed at a mass ratio of 5:3, and the mass of the curing accelerator is 3% of the total mass of the dry mixture and water to obtain a wet mixture; the curing accelerator includes water glass and acrylic copolymer emulsion, and the mass ratio of the water glass and the acrylic copolymer emulsion is 6:10.

[0057] (4) The wet mixture is placed in a prefabricated mold, subjected to compression molding, demoulding, and curing to obtain a filling gelling material; the compression molding pressure is 40-60 MPa, the time is 15 hours, the curing temperature is 10° C., the time is 10 days, and the relative humidity is 90%.

[0058] The obtained filling gelling material was subjected to leaching test, PO4 3- 4.9 mg / L, F - The measured heavy metals are all within the range specified in GB8978-1996.

[0059] Unconfined compressive strength of filling cementitious material: 7d: 6.8MPa; 28d: 8.8MPa; 90d: 13.3MPa.

[0060] Example 5

[0061] A method for preparing a filling gelling material comprises the following steps:

[0062] (1) crushing the phosphate ore flotation tailings through a 100-mesh sieve to obtain phosphate tailings powder; then flotating the phosphogypsum and drying it to obtain flotation phosphogypsum.

[0063] (2) Cement, phosphate tailings powder, flotation phosphogypsum and alkali slag are mixed in a mass ratio of 1:2:2:1 to obtain a dry mix.

[0064] (3) The dry mixture and water are mixed at a mass ratio of 5:2, and the mass of the curing accelerator is 2% of the total mass of the dry mixture and water to obtain a wet mixture; the curing accelerator includes water glass and acrylic copolymer emulsion, and the mass ratio of the water glass and the acrylic copolymer emulsion is 6:10.

[0065] (4) The wet mixture is placed in a prefabricated mold, subjected to compression molding, demoulding, and curing to obtain a filling gelling material; the compression molding pressure is 40-60 MPa, the time is 15 hours, the curing temperature is 10° C., the time is 10 days, and the relative humidity is 90%.

[0066] The obtained filling gelling material was subjected to leaching test, PO4 3- 4.8mg / L, F - The measured heavy metals are all within the range specified in GB8978-1996.

[0067] Unconfined compressive strength of filling cementitious material: 7d: 6.6MPa; 28d: 9.0MPa; 90d: 13.2MPa.

[0068] Comparative Example 1

[0069] A method for preparing a filling gelling material comprises the following steps:

[0070] (1) crushing the phosphate ore flotation tailings through a 100-mesh sieve to obtain phosphate tailings powder; then flotating phosphogypsum and drying it to obtain flotation phosphogypsum;

[0071] (2) mixing cement, phosphate tailings powder, flotation phosphogypsum and alkali residue in a mass ratio of 1:2:3:1 to obtain a dry mix;

[0072] (3) mixing the dry mix with water in a mass ratio of 5:1 to obtain a wet mix;

[0073] (4) The wet mixture is placed in a prefabricated mold, subjected to compression molding, demoulding, and curing to obtain a filling gelling material; the compression molding pressure is 50 MPa, the time is 20 h; the curing temperature is 20° C., the time is 30 days, and the relative humidity is 85%.

[0074] The obtained filling gelling material was subjected to leaching test, PO4 3- The measured heavy metal content is within the range specified in GB8978-1996. - Not within the scope specified in GB8978-1996.

[0075] Unconfined compressive strength of filling cementitious material: 7d: 5.2MPa; 28d: 7.1MPa; 90d: 10.3MPa.

[0076] Comparative Example 2

[0077] A method for preparing a filling gelling material comprises the following steps:

[0078] (1) crushing the phosphate ore flotation tailings through a 100-mesh sieve to obtain phosphate tailings powder; then flotating the phosphogypsum and drying it to obtain flotation phosphogypsum.

[0079] (2) Cement, phosphate tailings powder, flotation phosphogypsum and alkali slag are mixed in a mass ratio of 1:2:3:1 to obtain a dry mix.

[0080] (3) The dry mix and water are mixed at a mass ratio of 5:3 and the acrylic copolymer emulsion is mixed at a mass ratio of 1% of the total mass of the dry mix and water to obtain a wet mix.

[0081] (4) The wet mixture is placed in a prefabricated mold, subjected to compression molding, demoulding, and curing to obtain a filling gelling material; the compression molding pressure is 50 MPa, the time is 20 h; the curing temperature is 20° C., the time is 30 days, and the relative humidity is 85%.

[0082] The obtained filling gelling material was subjected to leaching test, PO4 3- The measured heavy metals are all within the range specified in GB8978-1996. - Not within the scope specified in GB8978-1996.

[0083] Unconfined compressive strength of filling cementitious material: 7d: 5.6MPa; 28d: 7.5MPa; 90d: 11.2MPa.

[0084] Comparative Example 3

[0085] A method for preparing a filling gelling material comprises the following steps:

[0086] (1) crushing the phosphate ore flotation tailings through a 100-mesh sieve to obtain phosphate tailings powder; then flotating the phosphogypsum and drying it to obtain flotation phosphogypsum.

[0087] (2) Cement, phosphate tailings powder, flotation phosphogypsum and alkali slag are mixed in a mass ratio of 1:2:3:1 to obtain a dry mix.

[0088] (3) The dry mix and water are mixed at a mass ratio of 5:3 and water glass at a mass of 1% of the total mass of the dry mix and water to obtain a wet mix.

[0089] (4) The wet mixture is placed in a prefabricated mold, subjected to compression molding, demoulding, and curing to obtain a filling gelling material; the compression molding pressure is 50 MPa, the time is 20 h; the curing temperature is 20° C., the time is 30 days, and the relative humidity is 85%.

[0090] The obtained filling gelling material was subjected to leaching test, PO4 3- It is 9.3 mg / L, F- and the measured heavy metals are all within the range specified in GB8978-1996.

[0091] Unconfined compressive strength of filling cementitious material: 7d: 6.1MPa; 28d: 7.6MPa; 90d: 11.6MPa.

[0092] According to Comparative Examples 1-3, the synergistic effect of water glass and acrylic copolymer emulsion can increase the amount of flotation phosphogypsum, phosphate tailings powder and alkali slag, and can effectively fix PO4 in phosphate tailings powder and phosphogypsum. 3- and F-. The lack of water glass will reduce the hydrolysis and hydration efficiency of the solidifying components and delay the PO4 3- The lack of acrylate copolymer emulsion will affect the bonding strength of the components in the filling gel material and reduce the overall mechanical properties. Acrylate copolymer emulsion can also form a hydrophobic film on the surface and inside of the cured body, improving the water resistance of the cured body.

[0093] Comparative Example 4

[0094] A method for preparing a filling gelling material comprises the following steps:

[0095] (1) crushing the phosphate ore flotation tailings through a 100-mesh sieve to obtain phosphate tailings powder; then flotating the phosphogypsum and drying it to obtain flotation phosphogypsum.

[0096] (2) Cement, phosphate tailings powder, and flotation phosphogypsum are mixed in a mass ratio of 1:2:3 to obtain a dry mix.

[0097] (3) The dry mixture and water are mixed at a mass ratio of 5:1, and the mass of the curing accelerator is 1% of the total mass of the dry mixture and water to obtain a wet mixture; the curing accelerator includes water glass and acrylic copolymer emulsion, and the mass ratio of the water glass and the acrylic copolymer emulsion is 6:10.

[0098] (4) The wet mixture is placed in a prefabricated mold, subjected to compression molding, demoulding, and curing to obtain a filling gelling material; the compression molding pressure is 50 MPa, the time is 20 h; the curing temperature is 20° C., the time is 30 days, and the relative humidity is 85%.

[0099] The obtained filling gelling material was subjected to leaching test, PO4 3- It is 9.9 mg / L, F- and the measured heavy metals are within the range specified in GB8978-1996.

[0100] Unconfined compressive strength of filling cementitious material: 7d: 5.7MPa; 28d: 7.8MPa; 90d: 11.9MPa.

[0101] Comparative Example 5

[0102] A method for preparing a filling gelling material comprises the following steps:

[0103] (1) The phosphogypsum is subjected to flotation treatment and then dried to obtain flotation phosphogypsum.

[0104] (2) Cement, flotation phosphogypsum and alkali residue are mixed in a mass ratio of 1:3:1 to obtain a dry mix.

[0105] (3) The dry mixture and water are mixed at a mass ratio of 5:1, and the mass of the curing accelerator is 1% of the total mass of the dry mixture and water to obtain a wet mixture; the curing accelerator includes water glass and acrylic copolymer emulsion, and the mass ratio of the water glass and the acrylic copolymer emulsion is 6:10.

[0106] (4) The wet mixture is placed in a prefabricated mold, subjected to compression molding, demoulding, and curing to obtain a filling gelling material; the compression molding pressure is 50 MPa, the time is 20 h; the curing temperature is 20° C., the time is 30 days, and the relative humidity is 85%.

[0107] The obtained filling gelling material was subjected to leaching test, PO4 3- It is 10.2 mg / L, F- and the measured heavy metals are within the range specified in GB8978-1996.

[0108] Unconfined compressive strength of filling cementitious material: 7d: 6.1MPa; 28d: 7.7MPa; 90d: 11.8MPa.

[0109] According to the comparison between Example 1 and Comparative Examples 4-5, it can be seen that there is a lack of alkali slag or phosphate tailings powder, PO4 3- and F - The curing effect and the mechanical strength of the filling gel material will be reduced. Mixing alkali slag with cement and adding water will generate hydrated calcium aluminosilicate (CASH), which improves the mechanical properties of the filling gel material. The phosphate components in the phosphate tailings can also react with calcium to generate various calcium phosphate compounds with certain gelling properties such as hydroxyapatite, further improving the strength and stability of the solidified body. In addition, the alkali slag provides an alkaline environment for the curing system. Phosphogypsum and phosphate tailings powder can produce alkali excitation in an alkaline environment, thereby promoting the dissolution of phosphogypsum and accelerating the reaction process.

[0110] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a filling gelling material, characterized in that: The steps include: (1) crushing and sieving the phosphate ore flotation tailings to obtain phosphate tailings powder; then flotation treating the phosphogypsum and drying it to obtain flotation phosphogypsum; (2) mixing cement, phosphate tailings powder, flotation phosphogypsum and alkali residue to obtain a dry mix; (3) mixing the dry mix, water and curing accelerator to obtain a wet mix; (4) The wet mixed material is placed in a prefabricated mold, and the mold is pressed, demoulded, and cured to obtain a filling gelling material.

2. The method for preparing the filling gelling material according to claim 1, characterized in that: The flotation process is a froth flotation method.

3. The method for preparing the filling gelling material according to claim 1, characterized in that: The curing accelerator comprises water glass and acrylate copolymer emulsion, and the mass ratio of the water glass to the acrylate copolymer emulsion is 6:5-12.

4. The method for preparing the filling gelling material according to claim 1, characterized in that: The mass ratio of the cement, phosphate tailings powder, flotation phosphogypsum and alkali slag is (1-2):(2-3):(2-3):(1-2).

5. The method for preparing a filling gelling material according to claim 4, characterized in that: The mass ratio of the cement, phosphate tailings powder, flotation phosphogypsum and alkali slag is 2:3:3:

2.

6. The method for preparing the filling gelling material according to claim 1, characterized in that: The mass ratio of the dry mix to water is 5:(1-3); the mass of the curing accelerator is 1% to 3% of the total mass of the dry mix and water.

7. The method for preparing a filling gelling material according to claim 1, characterized in that: The pressure of the compression mold is 40-60MPa, and the time is 15-25h.

8. The method for preparing the filling gelling material according to claim 1, characterized in that: The curing temperature is 10-30° C., the curing time is 20-40 days, and the relative humidity is 80-90%.

9. The method for preparing a filling gelling material according to claim 8, characterized in that: The curing temperature is 20° C., the time is 30 days, and the relative humidity is 85%.

10. The filling gelling material prepared by the method for preparing a filling gelling material according to any one of claims 1 to 9.