Yttrium aluminum oxide continuous ceramic fiber and preparation method thereof
The preparation of yttrium aluminum oxide fibers by polymer melt spinning method solves the problems of high energy consumption and environmental protection in the preparation of existing YAG fibers, improves the tensile strength and grain density of the fibers, and is suitable for high-temperature insulation and structural reinforcement materials.
Patent Information
- Application Number
- CN202310507804.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-08
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-05-08
AI Technical Summary
The existing preparation methods for yttrium aluminum garnet (YAG) fibers have problems such as high energy consumption, high cost, complex process, environmental protection and poor performance, especially in the process of spinning additives and high-temperature sintering, which lead to an increase in grain size. Problems with mechanical properties.
The polymer melt spinning method is used to prepare yttrium aluminum oxide continuous ceramic fibers. Through melt spinning, steam crosslinking, glue removal treatment and ceramicization treatment of yttrium aluminum oxide ceramic precursor, pure YAG phase or YAG phase is obtained. The fibers mixed with α-Al2O3, γ-Al2O3 and YAM have an average diameter of 5-15μm and a tensile strength up to 1.5GPa.
It realizes an environmentally friendly preparation process, improves the tensile strength of the fiber and the denseness of the grain size, reduces production costs, and is suitable for high-temperature insulation and structural reinforcement materials.
Smart Images

Figure CN118908697A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite fiber materials and relates to a yttrium aluminum oxide continuous ceramic fiber and a preparation method thereof. Background Art
[0002] In the 1960s, the commercial application of non-oxide ceramic fibers represented by SiC fibers played a key role in promoting the development of ceramic-based composites. However, non-oxide ceramic fibers are affected by oxidation problems at high temperatures, which limits their application in specific environments. Oxide ceramic fibers can be used in high-temperature aerobic environments due to their excellent oxidation resistance. At the same time, they have good flexibility, so that they can be woven and used as structural reinforcement materials in ceramic-based composites. Oxide short fibers were initially produced and used as refractory insulation materials, and then the SiO2-containing continuous Al2O3 fibers that were born can be used as reinforcement materials for lightweight alloys. Oxide continuous ceramic fibers are widely used in aerospace, military industry, automobiles and other fields due to their high strength, high modulus and excellent oxidation resistance. Their excellent mechanical properties mainly rely on dense nanocrystalline structures. Many studies have shown that the tensile strength of oxide continuous ceramic fibers at high temperatures will decrease due to the increase in grain size. Therefore, selecting oxide components with good high-temperature stability and refining the grain size of the fibers are crucial for the preparation of high-performance oxide continuous ceramic fibers.
[0003] Yttrium aluminum garnet (YAG) fiber is a new type of inorganic ceramic fiber developed in the 1990s. YAG is the only binary compound in the Y2O3-Al2O3 system that can exist stably at high temperatures (chemical formula is Y3A15O 12 ), belongs to the cubic system, has a garnet structure, has a melting point of 1942°C, and a density of 4.55g / cm 3 , isotropy, good chemical stability, excellent high temperature creep resistance and good water vapor corrosion resistance. Fiberization is an effective way to realize the application of YAG in lightweight high temperature thermal protection materials and structural reinforcement materials. Compared with other oxide ceramic fibers, YAG fiber has better creep resistance, which is one order of magnitude higher than alumina fiber. Therefore, YAG fiber is a very promising reinforcement material that can be used in high temperature aerobic environments.
[0004] At present, there are two main methods for preparing YAG fibers, namely the melting method and the sol-gel method. The melting method is mostly used to prepare single-crystal YAG fibers. The process requires a high temperature, generally above 1500°C. Due to its high energy consumption, high cost and complex preparation process, its further development is limited; the sol-gel method is mostly used to prepare polycrystalline YAG fibers. Due to its simple process, mild reaction conditions and controllable nature, it is currently reported in the literature as a commonly used method for preparing YAG fibers.
[0005] Patent CN106927808 B uses Al 13 Alumina sol of colloidal particles, γ-AlOOH nano-dispersion, and yttrium oxide sol are used as raw materials, and a spinning aid is added to the acidic solution. Dry spinning can produce continuous gel fiber precursors with a length of up to three kilometers, and after further heat treatment, yttrium aluminum garnet long fibers with a diameter of 6-12μm are obtained. This method combines the characteristics of the slurry method and the sol-gel method for preparing oxide fibers, and the tensile strength of the prepared fiber single filament is close to 1.0GPa. However, since the spinning raw materials contain Cl elements and spinning aids are added, it is not conducive to environmental protection and the preparation of high-performance fibers. And because the spinning raw materials contain γ-AlOOH nanoparticles, phase separation is easy to occur between the nanoparticles and the bulk oxide during the sintering process, which is not conducive to densification sintering. It must be sintered at a higher temperature, but high-temperature sintering will cause the grain size to increase, thereby affecting the mechanical properties of the fiber.
[0006] Patent CN 111978550 A uses an organic polymer precursor method to prepare yttrium aluminum garnet long fibers with high purity and flexibility. Although no spinning aid is used, chlorine-containing aluminum chloride, yttrium chloride and other raw materials are used in the preparation process. During the synthesis process and the later sintering process, acidic substances such as HCl will be produced, which will have an adverse effect on the environment and equipment. In addition, too much organic solvent is used in the dissolution, extraction, filtration and concentration process, and a large amount of organic solvent waste liquid will inevitably be generated during the industrial preparation process. In addition, the yttrium aluminum garnet fiber prepared by this method has a relatively thick diameter, which is not conducive to the preparation of high-strength yttrium aluminum garnet long fibers. Summary of the invention
[0007] The purpose of the present invention is to provide a yttrium aluminum oxide continuous ceramic fiber and a preparation method thereof.
[0008] The yttrium aluminum oxide continuous ceramic fiber provided by the present invention is composed of Al2O3 and Y2O3, and the molar ratio of Al to Y elements in the fiber is 5:3.5-0.5; specifically, it can be 5:3.5, 5:3, 5:2, 5:1, 5:0.5;
[0009] The crystalline phase composition of the yttrium aluminum oxide continuous ceramic fiber is: pure YAG (Y3A15O 12 ) phase or a mixture of a YAG phase and at least one of an α-Al2O3, γ-Al2O3 and a YAM (Y4A12O9) phase;
[0010] The yttrium aluminum oxide continuous ceramic fiber has an average diameter of 5-15 μm, specifically 10 μm, and a tensile strength of up to 1.5 GPa.
[0011] The yttrium aluminum oxide continuous ceramic fiber of the present invention is prepared by a polymer melt spinning method, and the process flow is environmentally friendly; the obtained yttrium aluminum oxide continuous ceramic fiber is composed of pure YAG (Y3A15O 12 ) phase or YAG phase with α-Al2O3, γ-Al2O3, YAG (Y3A15O 12 ) and YAM (Y4A12O9) phases, and the ratio can be adjusted when multiple phases are mixed.
[0012] The method for preparing yttrium aluminum oxide continuous ceramic fiber provided by the present invention comprises:
[0013] 1) melt spinning a yttrium aluminum oxide ceramic precursor to obtain a fiber precursor;
[0014] 2) subjecting the fiber precursor to steam crosslinking and binder removal treatment or high-temperature steam crosslinking and binder removal integrated treatment to obtain inorganic fiber;
[0015] 3) The inorganic fiber is subjected to a ceramic treatment to obtain the yttrium aluminum oxide continuous ceramic fiber.
[0016] In step 1) of the above method, in the melt spinning step, the softening point of the yttrium aluminum oxide ceramic precursor is 110-180° C., specifically 120° C.;
[0017] The yttrium aluminum oxide ceramic precursor is prepared by the following method:
[0018] An aluminum source and a yttrium source are added to a solvent, and the mixture is stirred and refluxed for 0.5-3 hours at a heating temperature of 60-110°C; a complexing agent is added at a heating temperature of 60-90°C, and the mixture is refluxed for 0.5-2 hours; a mixed solution of water and n-propanol in a mass ratio of 1:4 is then dripped at a dripping rate of 1 drop / s, and the mixture is refluxed for 2 hours; distillation is performed at a heating temperature of 180-270°C (specifically 260°C) for 0.5-6 hours, and the mixture is cooled to room temperature after being kept warm for 2 hours to obtain a yttrium aluminum oxide ceramic precursor.
[0019] Wherein, the molar ratio of the aluminum source and the yttrium source converted into Al and Y elements is 5:3.5-0.5; specifically, it can be 5:3.5-1, 5:1-0.5, 5:3.5, 5:3, 5:2, 5:1 or 5:0.5;
[0020] The aluminum source is aluminum isopropoxide;
[0021] The yttrium source is yttrium acetylacetonate;
[0022] The solvent is n-propanol;
[0023] The complexing agent is acetylacetone;
[0024] Acetylacetone is 0.6 times the molar fraction of the total amount of aluminum isopropoxide and yttrium acetylacetonate;
[0025] The molar ratio of the total amount of aluminum source, yttrium source and water is 1:0.6;
[0026] The temperature of the melt spinning is 20-60°C higher than the softening point of the precursor; specifically, it can be 45°C;
[0027] In the melt spinning, the diameter of the outlet hole is 0.1-1 mm, specifically 0.2 mm;
[0028] The screw extrusion pressure is 5-30MPa; specifically, it can be 20MPa;
[0029] The winding frequency is 15-40Hz; specifically 35Hz.
[0030] In step 2) of the above method, when the molar ratio of Al and Y elements used to prepare the yttrium aluminum oxide ceramic precursor is less than 5:1, such as 5:3.5-1 (excluding endpoint 1), the fiber precursor is subjected to high-temperature steam cross-linking and debinding integrated treatment to obtain inorganic fiber;
[0031] The operation of the high-temperature steam cross-linking and debinding integrated treatment is as follows: placing the fiber precursor in a honeypot steam furnace, continuously introducing water vapor during the debinding and sintering process, with a steam intake of 80-200 L / h (the end point of 200 L / h is not desirable, such as 80-120 L / h or 80 L / h), heating to 600° C. at a heating rate of 0.5-2° C. / min (such as 0.5° C. / min), keeping the temperature at the target temperature of 600° C. for 1 hour, closing the steam intake, and then cooling to room temperature;
[0032] In step 2) of the above method, when the molar ratio of Al and Y elements used to prepare the yttrium aluminum oxide ceramic precursor is greater than or equal to 5:1, such as 5:1-0.5, the fiber precursor is subjected to steam crosslinking and debinding treatment or the high-temperature steam crosslinking and debinding integrated treatment to obtain inorganic fiber, preferably the steam crosslinking and debinding treatment is performed;
[0033] The operation of the steam crosslinking and debinding treatment is as follows: placing the fiber raw yarn in a constant temperature and humidity chamber, heating it to 75-90°C (such as 85°C), keeping it warm at a relative humidity of 75-95% (such as 80%) for 0-60min (such as 0, 20, 40, 60min), cooling it to room temperature, and then placing the steam crosslinked fiber in a debinding and sintering integrated furnace for debinding to prepare inorganic fiber, heating it to 600°C at a speed of 1°C / min, keeping it warm at the target temperature of 600°C for 1h, and then cooling it to room temperature.
[0034] In the ceramicizing step of step 3) of the above method, the rate of increasing from room temperature to the ceramicizing temperature is 10-30°C / min; specifically 10°C / min;
[0035] The temperature of ceramicization is 1100-1500°C; specifically 1200°C;
[0036] The ceramicization time is 30min-2h; specifically 1h;
[0037] The ceramicizing atmosphere is air.
[0038] In addition, the yttrium aluminum oxide continuous ceramic fiber prepared by the above method and the use of the yttrium aluminum oxide continuous ceramic fiber in the preparation of a material having at least one of structural reinforcement and high-temperature thermal insulation properties also fall within the protection scope of the present invention.
[0039] The present invention has the following beneficial effects:
[0040] 1) In the preparation method of yttrium aluminum oxide continuous ceramic fiber provided by the present invention, melt spinning is adopted to form fibers, which has simple process, is environmentally friendly, and is easy to scale up production.
[0041] 2) The yttrium aluminum oxide continuous ceramic fiber provided by the present invention has a crystal composition of pure YAG (Y3A15O 12 ) phase or a mixture of YAG phase and at least one of α-Al2O3, γ-Al2O3 and YAM (Y4A12O9) phases, and the ratio can be adjusted when multiple phases are mixed.
[0042] 3) The average diameter of the yttrium aluminum oxide continuous ceramic fiber provided by the present invention is 5-15 μm, and the maximum tensile strength can reach 1.5 GPa. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 is the XRD pattern of the fiber prepared at different temperatures in Example 2.
[0044] Figure 2 is the SEM image of the fiber in Example 3.
[0045] Figure 3 is the XRD pattern of the fiber prepared at different temperatures in Example 3.
[0046] Figure 4 This is the TG diagram of the precursor in Comparative Example 1.
[0047] Figure 5 This is the SEM image of the fiber precursor in Comparative Example 2. DETAILED DESCRIPTION
[0048] The present invention is further described in detail below in conjunction with specific embodiments, and the examples provided are only for illustrating the present invention, rather than for limiting the scope of the present invention. The examples provided below can be used as a guide for further improvements by those of ordinary skill in the art, and do not constitute a limitation of the present invention in any way.
[0049] The experimental methods in the following examples, unless otherwise specified, are all conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial channels.
[0050] Example 1
[0051] Preparation of Yttrium Aluminum Oxide Continuous Ceramic Fibers
[0052] 1) Precursor synthesis: Aluminum isopropoxide and yttrium acetylacetonate are added to n-propanol, wherein the amount of aluminum isopropoxide:yttrium acetylacetonate is converted into a molar ratio of Al and Y elements of 5:1, and the mixture is stirred and refluxed at a heating temperature of 90°C for 3 hours; then, acetylacetone with a molar fraction of 0.6 times the total amount of aluminum isopropoxide and yttrium acetylacetonate is added at a heating temperature of 80°C, and the mixture is heated and refluxed for 1.5 hours; then, a mixed solution of water and n-propanol with a mass ratio of 1:4 is added dropwise at a dropping rate of 1 drop / s, wherein the molar ratio of the total amount of aluminum isopropoxide, yttrium acetylacetonate and water is 1:0.6, and the mixture is refluxed for 2 hours; atmospheric distillation is carried out at a heating temperature of 230°C for 5 hours, and the mixture is cooled to room temperature after being kept warm for 2 hours to obtain a yttrium aluminum oxide ceramic precursor with a softening point of 120°C and a ceramic yield of 36.2%.
[0053] 2) Melt spinning: a yttrium aluminum oxide ceramic precursor with a softening point of 120°C and a molar ratio of Al to Y elements of 5:1 is heated to 165°C, and after it is melted into a uniform melt and residual bubbles are removed, melt spinning is performed at a temperature of 165°C, the diameter of the filament outlet hole is 0.2mm, the screw extrusion pressure is 20MPa, and the filament is collected at a rate of 35Hz to obtain a fiber precursor;
[0054] 3) Steam crosslinking and debinding treatment: Steam crosslinking and debinding treatment: The obtained fiber raw silk is placed in a constant temperature and humidity chamber, heated to 85°C, kept at 80% relative humidity for 60 minutes, and cooled to room temperature. Subsequently, the steam crosslinked fiber is placed in a debinding and sintering integrated furnace for debinding to prepare inorganic fiber, and the temperature is raised to 600°C at 1°C / min, kept at the target temperature of 600°C for 1 hour, and then cooled to room temperature to obtain inorganic fiber;
[0055] 4) Ceramicization: The obtained inorganic fiber is placed in an alumina fiber fast-firing furnace with air atmosphere, and the temperature is raised to 1200°C at 10°C / min. After being kept warm for 1 hour, the temperature is lowered to room temperature to obtain yttrium aluminum oxide continuous ceramic fiber.
[0056] The average diameter of the obtained fiber is 10 μm, the average tensile strength is 1.16 GPa, the crystal phase composition is YAG phase and α-Al2O3 phase, and the average grain size is 66.2 nm.
[0057] Example 2
[0058] Preparation of Yttrium Aluminum Oxide Continuous Ceramic Fibers
[0059] 1) Precursor synthesis: Aluminum isopropoxide and yttrium acetylacetonate are added to n-propanol, wherein the amount of aluminum isopropoxide:yttrium acetylacetonate is converted into a molar ratio of Al and Y elements of 5:0.5, and the mixture is stirred and refluxed at a heating temperature of 90°C for 3 hours; then, acetylacetone with a molar fraction of 0.6 times the total amount of aluminum isopropoxide and yttrium acetylacetonate is added at a heating temperature of 80°C, and the mixture is heated and refluxed for 1.5 hours; then, a mixed solution of water and n-propanol with a mass ratio of 1:4 is added dropwise at a dropping rate of 1 drop / s, wherein the molar ratio of the total amount of aluminum isopropoxide, yttrium acetylacetonate and water is 1:0.6, and the mixture is refluxed for 2 hours; atmospheric distillation is carried out at a heating temperature of 230°C for 6 hours, and the mixture is cooled to room temperature after being kept warm for 2 hours to obtain a yttrium aluminum oxide ceramic precursor with a softening point of 120°C and a ceramic yield of 34.5%.
[0060] 2) Melt spinning: a yttrium aluminum oxide ceramic precursor with a softening point of 120°C and a molar ratio of Al to Y elements of 5:0.5 is heated to 165°C, and after it is melted into a uniform melt and residual bubbles are removed, melt spinning is performed at a temperature of 165°C, the diameter of the filament outlet hole is 0.2 mm, the screw extrusion pressure is 20 MPa, and the filament is collected at a rate of 35 Hz to obtain a fiber precursor;
[0061] 3) Steam cross-linking and debonding treatment: same as in Example 1;
[0062] 4) Ceramics: Same as in Example 1.
[0063] The average diameter of the obtained fiber is 10 μm, the average tensile strength is 1.35 GPa, the crystal phase composition is YAG phase and γ-Al2O3 phase, and the average grain size is 5.2 nm.
[0064] The XRD patterns of fibers prepared at different temperatures are shown in the attached Figure 1. As can be seen from the figure, at 950°C and below, the fiber crystal phase composition is amorphous. When the temperature rises to 1000°C, the γ-Al2O3 phase begins to appear. At 1150°C, several sharp diffraction peaks appear, which belong to the YAG phase and YAlO3 phase. When the temperature rises to 1250°C, the characteristic diffraction peaks of the γ-Al2O3 phase and the YAlO3 phase disappear, indicating that these two crystal phases appear as intermediate phases, and the characteristic peaks of the α-Al2O3 phase begin to appear. The final crystal phase composition of the fiber is the YAG phase and the α-Al2O3 phase. With the increase of temperature, the characteristic peaks of the two crystal phases gradually increase and the peak width narrows, indicating that the grain size of the two crystal phases gradually increases and the lattice structure gradually becomes complete.
[0065] Example 3
[0066] Preparation of Yttrium Aluminum Oxide Continuous Ceramic Fibers
[0067] 1) Precursor synthesis: Aluminum isopropoxide and yttrium acetylacetonate are added to n-propanol, wherein the amount of aluminum isopropoxide:yttrium acetylacetonate is converted into a molar ratio of Al and Y elements of 5:3, and the mixture is stirred and refluxed at a heating temperature of 90°C for 3 hours; then, acetylacetone with a molar fraction of 0.6 times the total amount of aluminum isopropoxide and yttrium acetylacetonate is added at a heating temperature of 80°C, and the mixture is heated and refluxed for 1.5 hours; then, a mixed solution of water and n-propanol with a mass ratio of 1:4 is dripped at a dripping rate of 1 drop / s, wherein the molar ratio of the total amount of aluminum isopropoxide, yttrium acetylacetonate and water is 1:0.6, and the mixture is refluxed for 2 hours; atmospheric distillation is performed at a heating temperature of 260°C for 4 hours, and the mixture is cooled to room temperature after being kept warm for 2 hours to obtain a yttrium aluminum oxide ceramic precursor with a softening point of 120°C and a ceramic yield of 38.7%;
[0068] 2) Melt spinning: a yttrium aluminum oxide ceramic precursor with a softening point of 120°C and a molar ratio of Al to Y elements of 5:3 is heated to 165°C, and after it is melted into a uniform melt and residual bubbles are removed, melt spinning is performed at a temperature of 165°C, the diameter of the filament outlet hole is 0.2mm, the screw extrusion pressure is 20MPa, and the filament is collected at a rate of 35Hz to obtain a fiber precursor;
[0069] 3) High-temperature steam cross-linking and debinding integrated treatment: The obtained fiber precursor is placed in a honeypot steam furnace, and water vapor is continuously introduced during the debinding and sintering process. The steam intake is 80L / h, and the temperature is increased to 600°C at a rate of 0.5°C / min. The temperature is kept at the target temperature of 600°C for 1h, the steam intake is turned off, and then the temperature is cooled to room temperature to obtain inorganic fiber;
[0070] 4) Ceramics: Same as in Example 1.
[0071] The obtained ceramic fibers have an average diameter of 10 μm, an average tensile strength of 1.56 GPa, a crystal phase composition of YAG phase, and an average grain size of 23.4 nm.
[0072] The SEM image of the fiber is attached. Figure 2 .
[0073] The XRD patterns of fibers prepared at different temperatures are shown in the attached Figure 3 . As can be seen from the figure, when the temperature rises to 900°C, the YAG fiber is basically amorphous, but there is a diffraction peak near 2θ=33°. Compared with the standard diffraction card of YAG (PDF#72-1315), it can be seen that the diffraction peak here is the characteristic peak of YAG, indicating that a small amount of YAG crystal phase has begun to form at 900°C. With the increase of temperature, the intensity of the YAG characteristic peak gradually increases and the peak width narrows, indicating that the grain size of the YAG fiber gradually increases and the lattice structure gradually completes. During the heating process, there is no intermediate phase YAP (YAlO3) and YAM (Y4Al2O9) in the crystal phase of the YAG fiber, indicating that a single-phase YAG fiber can be prepared by the polymer precursor method.
[0074] Example 4
[0075] Preparation of Yttrium Aluminum Oxide Continuous Ceramic Fibers
[0076] 1) Precursor synthesis: Aluminum isopropoxide and yttrium acetylacetonate are added to n-propanol, wherein the amount of aluminum isopropoxide:yttrium acetylacetonate is converted into a molar ratio of Al and Y elements of 5:2, and the mixture is stirred and refluxed at a heating temperature of 90°C for 3 hours; then, acetylacetone with a molar fraction of 0.6 times the total amount of aluminum isopropoxide and yttrium acetylacetonate is added at a heating temperature of 80°C, and the mixture is heated and refluxed for 1.5 hours; then, a mixed solution of water and n-propanol with a mass ratio of 1:4 is dripped at a dripping rate of 1 drop / s, wherein the molar ratio of the total amount of aluminum isopropoxide, yttrium acetylacetonate and water is 1:0.6, and the mixture is refluxed for 2 hours; atmospheric distillation is performed at a heating temperature of 240°C for 4.5 hours, and the mixture is kept warm for 2 hours and then cooled to room temperature to obtain a yttrium aluminum oxide ceramic precursor with a softening point of 120°C and a ceramic yield of 37.6%;
[0077] 2) Melt spinning: The yttrium aluminum oxide ceramic precursor with a softening point of 120°C and a molar ratio of Al to Y elements of 5:2 is heated to 165°C, and after it is melted into a uniform melt and the residual bubbles are removed, melt spinning is performed at a temperature of 165°C, the diameter of the wire outlet hole is 0.2mm, the screw extrusion pressure is 20MPa, and the wire is collected at a rate of 35Hz to obtain fiber precursor;
[0078] 3) High-temperature steam cross-linking and debinding integrated treatment: same as in Example 3;
[0079] 4) Ceramics: Same as in Example 1.
[0080] The obtained ceramic fibers have an average diameter of 10 μm, an average tensile strength of 0.98 GPa, a crystal phase composition of YAG phase and α-Al2O3 phase, and an average grain size of 72.8 nm.
[0081] Example 5
[0082] Preparation of Yttrium Aluminum Oxide Continuous Ceramic Fibers
[0083] 1) Precursor synthesis: same as in Example 1;
[0084] 2) Melt spinning: same as in Example 1;
[0085] 3) High-temperature steam cross-linking and debinding integrated treatment: same as in Example 3;
[0086] 4) Ceramics: Same as Example 3.
[0087] The obtained ceramic fibers have an average diameter of 10 μm, an average tensile strength of 1.06 GPa, a crystal phase composition of YAG phase and α-Al2O3 phase, and an average grain size of 66.2 nm.
[0088] Example 6
[0089] Preparation of Yttrium Aluminum Oxide Continuous Ceramic Fibers
[0090] 1) Precursor synthesis: same as in Example 2;
[0091] 2) Melt spinning: same as in Example 2;
[0092] 3) High-temperature steam cross-linking and debinding integrated treatment: same as in Example 3;
[0093] 4) Ceramics: Same as in Example 1.
[0094] The obtained ceramic fibers have an average diameter of 10 μm, an average tensile strength of 1.27 GPa, a crystal phase composition of YAG phase and γ-Al2O3 phase, and an average grain size of 5.2 nm.
[0095] Example 7
[0096] Preparation of Yttrium Aluminum Oxide Continuous Ceramic Fibers
[0097] 1) Precursor synthesis: Aluminum isopropoxide and yttrium acetylacetonate are added to n-propanol, wherein the amount of aluminum isopropoxide:yttrium acetylacetonate is converted into a molar ratio of Al and Y elements of 5:3.5, and the mixture is stirred and refluxed at a heating temperature of 90°C for 3 hours; then, acetylacetone with a molar fraction of 0.6 times the total amount of aluminum isopropoxide and yttrium acetylacetonate is added at a heating temperature of 80°C, and the mixture is heated and refluxed for 1.5 hours; then, a mixed solution of water and n-propanol with a mass ratio of 1:4 is dripped at a dripping rate of 1 drop / s, wherein the molar ratio of the total amount of aluminum isopropoxide, yttrium acetylacetonate and water is 1:0.6, and the mixture is refluxed for 2 hours; atmospheric distillation is performed at a heating temperature of 270°C for 3.5 hours, and the mixture is kept warm for 2 hours and then cooled to room temperature to obtain a yttrium aluminum oxide ceramic precursor with a softening point of 120°C and a ceramic yield of 39.4%;
[0098] 2) Melt spinning: The yttrium aluminum oxide ceramic precursor with a softening point of 120°C and a molar ratio of Al to Y elements of 5:3.5 is heated to 165°C, and after it is melted into a uniform melt and the residual bubbles are removed, melt spinning is performed at a temperature of 165°C, the diameter of the wire outlet hole is 0.2mm, the screw extrusion pressure is 20MPa, and the wire is collected at a rate of 35Hz to obtain fiber precursor;
[0099] 3) High-temperature steam cross-linking and debinding integrated treatment: same as in Example 3;
[0100] 4) Ceramics: Same as in Example 1.
[0101] The obtained ceramic fibers have an average diameter of 10 μm, an average tensile strength of 1.30 GPa, a crystal phase composition of YAG phase and YAM phase, and an average grain size of 43.1 nm.
[0102] Example 8
[0103] Preparation of Yttrium Aluminum Oxide Continuous Ceramic Fibers
[0104] 1) Aluminum isopropoxide and yttrium acetylacetonate are added to n-propanol, wherein the amount of aluminum isopropoxide:yttrium acetylacetonate is converted into a molar ratio of Al and Y elements of 5:3, and the mixture is stirred and refluxed at a heating temperature of 90°C for 3 hours; then, acetylacetone with a molar fraction of 0.6 times the total amount of aluminum isopropoxide and yttrium acetylacetonate is added at a heating temperature of 80°C, and the mixture is heated and refluxed for 1.5 hours; then, a mixed solution of water and n-propanol with a mass ratio of 1:4 is added dropwise at a dropping rate of 1 drop / s, wherein the molar ratio of the total amount of aluminum isopropoxide, yttrium acetylacetonate and water is 1:0.6, and the mixture is refluxed for 2 hours; atmospheric distillation is performed at a heating temperature of 260°C for 4 hours, and the mixture is cooled to room temperature after being kept warm for 2 hours to obtain a yttrium aluminum oxide ceramic precursor with a softening point of 120°C and a ceramic yield of 38.7%.
[0105] 2) Melt spinning: a yttrium aluminum oxide ceramic precursor with a softening point of 120°C and a molar ratio of Al to Y elements of 5:3 is heated to 165°C, and after it is melted into a uniform melt and residual bubbles are removed, melt spinning is performed at a temperature of 165°C, the diameter of the filament outlet hole is 0.2mm, the screw extrusion pressure is 20MPa, and the filament is collected at a rate of 35Hz to obtain a fiber precursor;
[0106] 3) High-temperature steam cross-linking and debinding integrated treatment: the obtained fiber precursor is placed in a honeypot steam furnace, and water vapor is continuously introduced during the debinding and sintering process. The steam intake is 80L / h, and the temperature is increased to 600°C at a rate of 1°C / min. The temperature is kept at the target temperature of 600°C for 1h, and the steam intake is turned off, and then the temperature is cooled to room temperature and then cooled to room temperature to obtain inorganic fiber;
[0107] 4) Ceramics: Same as in Example 1.
[0108] The obtained ceramic fibers have an average diameter of 10 μm, an average tensile strength of 1.47 GPa, a crystal phase composition of YAG phase, and an average grain size of 23.4 nm.
[0109] Example 9
[0110] Preparation of Yttrium Aluminum Oxide Continuous Ceramic Fibers
[0111] 1) Precursor synthesis: same as Example 8;
[0112] 2) Melt spinning: same as in Example 8;
[0113] 3) High-temperature steam cross-linking and debinding integrated treatment: the obtained fiber precursor is placed in a honeypot steam furnace, and water vapor is continuously introduced during the debinding and sintering process. The steam intake is 80L / h, and the temperature is increased to 600°C at a rate of 2°C / min. The temperature is kept at the target temperature of 600°C for 1h, and the steam intake is turned off, and then the temperature is cooled to room temperature and then cooled to room temperature to obtain inorganic fiber;
[0114] 4) Ceramics: Same as in Example 1.
[0115] The obtained ceramic fibers have an average diameter of 10 μm, an average tensile strength of 1.34 GPa, a crystal phase composition of YAG phase, and an average grain size of 23.4 nm.
[0116] Compared with Examples 3, 8 and 9, the heating rate in the high-temperature steam cross-linking and binder removal integrated treatment has no effect on the crystal form and grain size, but affects the tensile strength.
[0117] Example 10
[0118] Preparation of Yttrium Aluminum Oxide Continuous Ceramic Fibers
[0119] 1) Precursor synthesis: same as Example 8;
[0120] 2) Melt spinning: same as in Example 8;
[0121] 3) High-temperature steam cross-linking and debinding integrated treatment: the obtained fiber precursor is placed in a honeypot steam furnace, and water vapor is continuously introduced during the debinding and sintering process. The steam intake is 120L / h, and the temperature is raised to 600°C at a rate of 0.5°C / min. The temperature is kept at the target temperature of 600°C for 1h, and the steam intake is turned off, and then the temperature is cooled to room temperature and then cooled to room temperature to obtain inorganic fiber;
[0122] 4) Ceramics: Same as in Example 1.
[0123] The obtained ceramic fibers have an average diameter of 10 μm, an average tensile strength of 0.93 GPa, a crystal phase composition of YAG phase, and an average grain size of 23.4 nm.
[0124] Compared with Example 10 and 3, fibers can also be obtained when the steam intake is 120 L / h, but the average stretching decreases as the intake increases.
[0125] Comparative Example 1
[0126] 1) Precursor synthesis: Aluminum isopropoxide and yttrium acetylacetonate are added to n-propanol, wherein the amount of aluminum isopropoxide:yttrium acetylacetonate is converted into a molar ratio of Al and Y elements of 5:3, and the mixture is stirred and refluxed at a heating temperature of 90°C for 3 hours; then, acetylacetone with a molar fraction of 0.6 times the total amount of aluminum isopropoxide and yttrium acetylacetonate is added at a heating temperature of 80°C, and the mixture is heated and refluxed for 1.5 hours; then, a mixed solution of water and n-propanol with a mass ratio of 1:4 is added dropwise at a dropping rate of 1 drop / s, wherein the molar ratio of the total amount of aluminum isopropoxide, yttrium acetylacetonate and water is 1:0.6, and the mixture is refluxed for 2 hours; atmospheric distillation is carried out at a heating temperature of 260°C for 4 hours, and the mixture is cooled to room temperature after being kept warm for 2 hours to obtain a yttrium aluminum oxide ceramic precursor with a softening point of 120°C and a ceramic yield of 38.7%.
[0127] 2) Melt spinning: a yttrium aluminum oxide ceramic precursor with a softening point of 120°C and a molar ratio of Al to Y elements of 5:3 is heated to 165°C, and after it is melted into a uniform melt and residual bubbles are removed, melt spinning is performed at a temperature of 165°C, the diameter of the filament outlet hole is 0.2mm, the screw extrusion pressure is 20MPa, and the filament is collected at a rate of 35Hz to obtain a fiber precursor;
[0128] 3) Steam crosslinking and debinding treatment: The obtained fiber raw silk was placed in a constant temperature and humidity chamber, heated to 85°C, kept at 80% relative humidity for 60 minutes, and cooled to room temperature. Subsequently, the steam crosslinked fiber was placed in a debinding and sintering integrated furnace for debinding to prepare inorganic fiber, and the temperature was raised to 600°C at 1°C / min, kept at the target temperature of 600°C for 1 hour, and then cooled to room temperature to obtain inorganic fiber;
[0129] The inorganic fiber obtained is black and has a rough surface, is brittle and has no strength.
[0130] The TGA curve of the precursor in air atmosphere is attached. Figure 4 As can be seen from the figure, the weight loss of the YAG precursor from room temperature to 1350℃ can be divided into four stages. The weight loss rate from room temperature to 600℃ is about 50.6%, and the weight loss in this stage is mainly caused by the decomposition and departure of organic groups in the YAG precursor; the weight loss rate from 600℃ to 1050℃ is about 1%, and the weight loss curve in this stage tends to be flat; the weight loss rate from 1050℃ to 1250℃ is about 9.7%, and the weight loss in this stage is mainly caused by the removal of residual carbon in the YAG precursor; the weight loss rate from 1250℃ to 1350℃ is 0%, and the weight loss curve in this stage is flat, indicating that at 600℃, the inorganic process of the precursor has been basically completed, but due to the high thermal decomposition temperature of yttrium acetylacetonate contained in the YAG precursor, some residual carbon is still not removed after 600℃, and the residual weight rate of the precursor at 1350℃ is 38.7%.
[0131] Comparative Example 2
[0132] 1) Precursor synthesis: Aluminum isopropoxide and yttrium acetylacetonate are added to n-propanol, wherein the amount of aluminum isopropoxide:yttrium acetylacetonate is converted into a molar ratio of Al and Y elements of 5:2, and the mixture is stirred and refluxed at a heating temperature of 90°C for 3 hours; then, acetylacetone with a molar fraction of 0.6 times the total amount of aluminum isopropoxide and yttrium acetylacetonate is added at a heating temperature of 80°C, and the mixture is heated and refluxed for 1.5 hours; then, a mixed solution of water and n-propanol with a mass ratio of 1:4 is added dropwise at a dropping rate of 1 drop / s, wherein the molar ratio of the total amount of aluminum isopropoxide, yttrium acetylacetonate and water is 1:0.6, and the mixture is refluxed for 2 hours; atmospheric distillation is performed at a heating temperature of 240°C for 4.5 hours, and the mixture is cooled to room temperature after being kept warm for 2 hours to obtain a yttrium aluminum oxide ceramic precursor with a softening point of 120°C and a ceramic yield of 37.6%.
[0133] 2) Melt spinning: The yttrium aluminum oxide ceramic precursor with a softening point of 120°C and a molar ratio of Al to Y elements of 5:2 is heated to 165°C, and after it is melted into a uniform melt and the residual bubbles are removed, melt spinning is performed at a temperature of 165°C, the diameter of the wire outlet hole is 0.2mm, the screw extrusion pressure is 20MPa, and the wire is collected at a rate of 35Hz to obtain fiber precursor;
[0134] See the attached SEM image of the fiber precursor. Figure 5 .
[0135] 3) Steam cross-linking and debonding treatment: same as Comparative Example 1.
[0136] The inorganic fiber obtained is black and has a rough surface, is brittle and has no strength.
[0137] Comparative Example 3
[0138] 1) Precursor synthesis: Aluminum isopropoxide and yttrium acetylacetonate are added to n-propanol, wherein the amount of aluminum isopropoxide:yttrium acetylacetonate is converted into a molar ratio of Al and Y elements of 5:3.5, and the mixture is stirred and refluxed at a heating temperature of 90°C for 3 hours; then, acetylacetone with a molar fraction of 0.6 times the total amount of aluminum isopropoxide and yttrium acetylacetonate is added at a heating temperature of 80°C, and the mixture is heated and refluxed for 1.5 hours; then, a mixed solution of water and n-propanol with a mass ratio of 1:4 is dripped at a dripping rate of 1 drop / s, wherein the molar ratio of the total amount of aluminum isopropoxide, yttrium acetylacetonate and water is 1:0.6, and the mixture is refluxed for 2 hours; atmospheric distillation is carried out at a heating temperature of 270°C for 3.5 hours, and the mixture is cooled to room temperature after being kept warm for 2 hours to obtain a yttrium aluminum oxide ceramic precursor with a softening point of 120°C and a ceramic yield of 39.4%.
[0139] 2) Melt spinning: The yttrium aluminum oxide ceramic precursor with a softening point of 120°C and a molar ratio of Al to Y elements of 5:3.5 is heated to 165°C, and after it is melted into a uniform melt and the residual bubbles are removed, melt spinning is performed at a temperature of 165°C, the diameter of the wire outlet hole is 0.2mm, the screw extrusion pressure is 20MPa, and the wire is collected at a rate of 35Hz to obtain fiber precursor;
[0140] 3) Steam cross-linking and debonding treatment: same as Comparative Example 1.
[0141] The inorganic fiber obtained is black and has a rough surface, is brittle and has no strength.
[0142] Comparative Example 4
[0143] 1) Precursor synthesis: same as Comparative Example 1;
[0144] 2) Melt spinning: same as Comparative Example 1;
[0145] 3) Steam crosslinking and debinding treatment: the obtained fiber precursor is placed in a honeypot steam furnace, and water vapor is continuously introduced during the debinding and sintering process. The steam intake is 200 L / h, and the temperature is increased to 600°C at a rate of 0.5°C / min. The temperature is kept at the target temperature of 600°C for 1 hour, and the steam intake is turned off, and then the temperature is cooled to room temperature and then cooled to room temperature to obtain inorganic fiber;
[0146] 4) Ceramics: Same as in Example 1.
[0147] The inorganic fiber obtained was white, rough, brittle and weak in strength. This may be because the steam intake used in the steam crosslinking and debinding treatment was too large, resulting in a violent reaction during the debinding process, which destroyed the fiber structure.
[0148] The present invention has been described in detail above. For those skilled in the art, without departing from the purpose and scope of the present invention, and without the need to carry out unnecessary experimental conditions, the present invention can be implemented in a wide range under equivalent parameters, concentrations and conditions. Although the present invention provides specific embodiments, it should be understood that the present invention can be further improved. In a word, according to the principles of the present invention, the application is intended to include any changes, uses or improvements to the present invention, including departure from the disclosed scope in the application, and changes made with conventional techniques known in the art.
Claims
1. Yttrium aluminum oxide continuous ceramic fiber, composed of Al2O3 and Y2O3, wherein the molar ratio of Al to Y in the fiber is 5:3.5-0.5; The crystalline phase composition of the yttrium aluminum oxide continuous ceramic fiber is: a pure YAG phase or a mixture of a YAG phase and at least one of α-Al2O3, γ-Al2O3 and YAM phase; The yttrium aluminum oxide continuous ceramic fiber has an average diameter of 5-15 μm and a maximum tensile strength of 1.5 GPa.
2. A method for preparing yttrium aluminum oxide continuous ceramic fibers, comprising: 1) melt spinning a yttrium aluminum oxide ceramic precursor to obtain a fiber precursor; 2) subjecting the fiber precursor to steam crosslinking and binder removal treatment or high-temperature steam crosslinking and binder removal integrated treatment to obtain inorganic fiber; 3) The inorganic fiber is subjected to a ceramic treatment to obtain the yttrium aluminum oxide continuous ceramic fiber.
3. The method according to claim 2, characterized in that: In step 1), the yttrium aluminum oxide ceramic precursor is prepared by the following method: Aluminum source and yttrium source are added to a solvent, and stirred and refluxed for 0.5-3 hours at a heating temperature of 60-110°C; a complexing agent is added at a heating temperature of 60-90°C, and refluxed for 0.5-2 hours; a mixed solution of water and n-propanol with a mass ratio of 1:4 is then dripped at a drip rate of 1 drop / s, and refluxed for 2 hours after dripping; distilled at a heating temperature of 180-270°C for 0.5-6 hours, kept warm for 2 hours, and then cooled to room temperature to obtain a yttrium aluminum oxide ceramic precursor; In the melt spinning step, the softening point of the yttrium aluminum oxide ceramic precursor is 110-180°C.
4. The method according to claim 3, characterized in that: The amounts of the aluminum source and the yttrium source are converted into a molar ratio of Al to Y element of 5:3.5-0.5; The aluminum source is aluminum isopropoxide; The yttrium source is yttrium acetylacetonate; The solvent is n-propanol; The complexing agent is acetylacetone; Acetylacetone is 0.6 times the molar fraction of the total amount of aluminum isopropoxide and yttrium acetylacetonate; The molar ratio of the total amount of aluminum source, yttrium source and water is 1:0.6; The temperature of the melt spinning is 20-60°C higher than the softening point of the precursor; In the melt spinning, the diameter of the outlet hole is 0.1-1 mm; The screw extrusion force is 5-30MPa; The winding frequency is 15-40Hz.
5. The method according to claim 2, characterized in that: In step 2), when the molar ratio of Al and Y elements used to prepare the yttrium aluminum oxide ceramic precursor is less than 5:1, the fiber precursor is subjected to high-temperature steam cross-linking and debinding integrated treatment to obtain inorganic fiber; The operation of the high-temperature steam cross-linking and debinding integrated treatment is as follows: placing the fiber precursor in a honeypot steam furnace, continuously introducing water vapor during the debinding and sintering process, with a steam intake of 80-200 L / h, heating to 600°C at a heating rate of 0.5-2°C / min, keeping the temperature at the target temperature of 600°C for 1 hour, closing the steam intake, and then cooling to room temperature.
6. The method according to claim 2, characterized in that: In step 2), when the molar ratio of Al and Y elements used to prepare the yttrium aluminum oxide ceramic precursor is greater than or equal to 5:1, the fiber precursor is subjected to steam crosslinking and debinding treatment or high-temperature steam crosslinking and debinding integrated treatment to obtain inorganic fiber, The steam cross-linking and debinding treatment is performed as follows: placing the fiber precursor in a constant temperature and humidity chamber, heating it to 75-90°C, keeping it warm at a relative humidity of 75-95% for 0-60 minutes, cooling it to room temperature, and then placing the steam cross-linked fiber in a debinding and sintering integrated furnace for debinding to prepare inorganic fiber, heating it to 600°C at a rate of 1°C / min, keeping it warm at the target temperature of 600°C for 1 hour, and then cooling it to room temperature.
7. The method according to claim 2, characterized in that: Step 3) In the ceramicizing step, the rate of increasing from room temperature to the ceramicizing temperature is 10-30°C / min; The temperature of ceramicization is 1100-1500℃; The ceramicization time is 30min-2h; The ceramicizing atmosphere is air.
8. Yttrium aluminum oxide continuous ceramic fiber obtained by the method according to any one of claims 2 to 7.
9. Use of the yttrium aluminum oxide continuous ceramic fiber according to claim 1 or 8 in preparing a material having at least one of the properties of structural reinforcement and high-temperature thermal insulation.
10. A material having at least one of the properties of structural reinforcement and high-temperature thermal insulation, the material comprising the yttrium aluminum oxide continuous ceramic fiber according to claim 1 or 8.
Citation Information
Patent Citations
A method for preparing yttrium aluminum garnet continuous fibers
CN106927808B
Yttrium / aluminum-organic polymer precursor, yttrium aluminum garnet continuous fiber and preparation method
CN111978550A
Chemical gas-phase crosslinking method of polycarbosilane fibers
CN103046166A
Al-Si complex phase oxide continuous ceramic fiber and preparation method thereof
CN111733484A
Al-Zr multiphase oxide continuous ceramic fiber and preparation method thereof