Rare earth doped electrical porcelain and preparation method and application thereof
By adding rare earth dopants and molding agents to the porcelain insulators to form a dense microstructure, the problem of insufficient mechanical properties of porcelain insulators in high-voltage power systems is solved, the mechanical strength and self-cleaning performance of the material are significantly improved, and the high-voltage power is met The system needs to operate safely and stably.
Patent Information
- Application Number
- CN202410849578.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-06-27
AI Technical Summary
In high-voltage power systems, pillar porcelain insulators need to withstand greater mechanical strength to ensure the safe and stable operation of the power system, but the mechanical properties of existing porcelain insulators are not sufficient to meet this requirement.
Rare earth doped electroceramic materials are used to form a dense and uniform microstructure by adding aluminum oxide, quartz, titanium dioxide, rare earth dopants and molding agents, thereby improving the mechanical strength and self-cleaning performance of the material. Yttrium dioxide and lanthanum stearate in rare earth dopants improve microstructure and thermal properties, and modified aluminum silicate and isocyanate in molding agent promote crystal nucleus formation and pore dispersion, forming a network-like structure, and improving mechanical properties .
It significantly improves the mechanical strength and bending strength of electroceramic materials, enhances its stability and self-cleaning performance at high temperatures, and meets the mechanical performance requirements of high-voltage power systems for insulators.
Smart Images

Figure BDA0004916477030000111 
Figure BDA0004916477030000121
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of electric porcelain, and in particular to a rare earth-doped electric porcelain and a preparation method and application thereof. Background Art
[0002] In order for the power system to transmit electric energy from the power plant to the distant users, two conditions must be met: one is to provide mechanical support for the conductors that transmit the current; the other is to provide sufficient insulation distance between the high-voltage end and the ground. Insulators have these two basic functions, so insulators occupy a very important position in the power system.
[0003] Porcelain insulators have always been the main players in the insulator industry, relying on their excellent mechanical and electrical properties, such as high stability, thermal stability, and chemical corrosion resistance. During operation, porcelain insulators must not only withstand the effects of conductor tension, wind force, and short-circuit current electromotive force acting on the insulator axis, but also the gravity of the electrical mechanism, the deadweight of the components, and the effects of natural environments such as earthquakes, freezing, and sudden temperature changes that may occur during operation. Moreover, as the power grid develops towards ultra-high and extra-high voltage, the greater the force that the insulator needs to withstand, the safe and stable operation of the power system places higher requirements on the mechanical strength of the pillar porcelain insulators.
[0004] Application Contents
[0005] The present application is made in view of the above-mentioned problems, and its object is to provide a rare earth-doped insulator having high mechanical strength.
[0006] Specifically, the first aspect of the present application provides a rare earth-doped insulator, comprising the following preparation raw materials:
[0007] Alumina, ceramic powder, quartz, titanium dioxide, rare earth dopants, dispersants and forming agents;
[0008] The molding agent comprises the following preparation raw materials:
[0009] Modified aluminum silicate, silicone rubber, isopropyl trioleyl titanate and isocyanate;
[0010] The rare earth dopant comprises the following preparation raw materials:
[0011] Yttrium trioxide and lanthanum stearate.
[0012] According to one of the technical solutions of this application, at least the following beneficial effects are achieved:
[0013] The raw materials prepared in the present application include alumina and quartz, etc., and rare earth dopants are also added. The rare earth dopants are used to improve the microstructure and thermal properties of the electrical porcelain, make the porcelain tougher, and thus improve the mechanical strength of the product.
[0014] The strength of electrical ceramic materials is determined not only by the strength and content of the crystalline phase itself, but also by the distribution of the crystalline phase in the material and its reasonable texture. 3+ Radius 9.3nm, La 3+ radius 10.6nm) and aluminum ions (Al 3+ The radius is 5.0nm) and the radius is very different; rare earth oxides are difficult to dissolve in Al2O3, so they work together with other grain boundary second phases to inhibit grain growth, form a dense and uniform microstructure, and improve the mechanical properties of the material. Rare earth ions play the role of fine grain strengthening, solid solution strengthening, self-toughening and strengthening in the microstructure of electrical ceramic materials. From a macroscopic point of view, adding rare earth oxides can reduce the sintering temperature of Al2O3 ceramics, improve the microstructure, and increase the mechanical strength.
[0015] At the same time, yttrium oxide in the rare earth forming agent is a network intermediate. 3+ It is a network denaturing ion. The introduction of yttrium oxide increases the active oxygen in the melt, increases O / Si, and reduces the silicon-oxygen complex anion group, which leads to a decrease in melt viscosity, thereby promoting the generation of crystal nuclei. Therefore, the tendency to produce crystalline mullite in the porcelain body increases, and the tendency to form a glass phase decreases. With the increase of mullite content, the density of the porcelain body increases, thereby improving the strength of the porcelain body.
[0016] Rare earth dopants and alumina tend to form low-melting point chemicals at high temperatures. Low-melting point compounds tend to form a liquid phase on the surface of the base particles. These liquid phase structures can wet the base particles and fill the pores between the particles, promote the discharge of gas, make the pores more evenly dispersed, increase the sintering density, and thus improve the bending strength.
[0017] The present application also controls the morphology of the pores through molding agents and lanthanum stearate, etc., so that the mullite phase is interspersed in the corundum phase to form a network structure, which significantly improves the mechanical properties of the material; thereby, an electric porcelain material with excellent mechanical properties is produced.
[0018] The preparation raw materials also contain a certain amount of titanium element. Titanium dioxide has a certain photocatalytic ability and can also improve the self-cleaning properties of electrical ceramic materials.
[0019] The microstructure of insulator materials mainly includes corundum (Al2O3) and mullite (3Al2O3·2SiO2) phases; within a certain range, the increase of mullite phase content is beneficial to enhance the mechanical properties of insulator materials.
[0020] According to some embodiments of the present application, the particle size of the yttrium oxide is 3 μm to 5 μm.
[0021] According to some embodiments of the present application, the ceramic powder is magnesium-calcium-silicon ternary ceramic powder;
[0022] According to some embodiments of the present application, the mass fraction of magnesium oxide in the ceramic powder is 10% to 20%.
[0023] According to some embodiments of the present application, the mass fraction of calcium oxide in the ceramic powder is 40% to 50%.
[0024] According to some embodiments of the present application, the mass fraction of silicon oxide in the ceramic powder is 40% to 50%.
[0025] According to some embodiments of the present application, the ceramic powder is 2CaO·MgO·2SiO2 powder.
[0026] According to some embodiments of the present application, the following raw materials are prepared in parts by weight:
[0027] 100 parts of alumina, 50 to 100 parts of ceramic powder, 20 to 30 parts of quartz, 5 to 10 parts of titanium dioxide, 1 to 2 parts of rare earth dopant, 10 to 20 parts of dispersant and 5 to 10 parts of forming agent.
[0028] According to some embodiments of the present application, the molding agent includes the following preparation raw materials in parts by weight:
[0029] 10 parts of modified aluminum silicate, 1 to 2 parts of silicone rubber, 10 to 20 parts of isopropyl trioleyl titanate and 1 to 2 parts of isocyanate.
[0030] According to some embodiments of the present application, the rare earth dopant includes the following preparation raw materials:
[0031] Yttrium trioxide, lanthanum stearate and solvent;
[0032] According to some embodiments of the present application, the rare earth dopant includes the following preparation raw materials in parts by weight:
[0033] 10 parts of yttrium trioxide, 20 to 40 parts of lanthanum stearate and 100 to 200 parts of solvent;
[0034] According to some embodiments of the present application, the solvent is ethanol.
[0035] According to some embodiments of the present application, the silicone rubber includes methyl vinyl silicone rubber.
[0036] According to some embodiments of the present application, the vinyl content of the methyl vinyl silicone rubber is 0.15% to 0.25%.
[0037] According to some embodiments of the present application, the molecular weight of the methyl vinyl silicone rubber is 600,000 to 700,000.
[0038] According to some embodiments of the present application, the vinyl silicone rubber is XIAMETER RBG-0702.
[0039] According to some embodiments of the present application, the modified aluminum silicate includes the following preparation raw materials:
[0040] Vinyltrimethoxysilane, aluminum silicate, and base.
[0041] According to some embodiments of the present application, the mass ratio of vinyltrimethoxysilane to aluminum silicate is 7 to 8:10.
[0042] The second aspect of the present application provides a method for preparing the rare earth-doped insulator according to the first aspect of the present application, comprising the following steps:
[0043] Mixing the prepared raw materials and then sintering them;
[0044] The sintering temperature is 500°C to 1300°C.
[0045] According to some embodiments of the present application, the sintering includes a first heat preservation, a second heat preservation and a third heat preservation.
[0046] According to some embodiments of the present application, the temperature of the first insulation is 500°C to 600°C.
[0047] According to some embodiments of the present application, the first insulation time is 1 hour to 3 hours.
[0048] According to some embodiments of the present application, the temperature of the second insulation is 1000°C to 1100°C.
[0049] According to some embodiments of the present application, the second insulation time is 12 hours to 16 hours.
[0050] According to some embodiments of the present application, the temperature of the third insulation is 1200°C to 1300°C.
[0051] According to some embodiments of the present application, the third insulation time is 3h to 5h.
[0052] The present application controls the insulation stage of sintering. The first insulation process is mainly to fully decompose the organic matter in the preparation raw materials. The organic matter containing metal elements will be converted into inorganic matter, such as metal oxides, during the first insulation process; and the organic matter containing metal elements and silicone rubber have good compatibility, so that the metal oxides can be fully fixed in the electrical porcelain material, thereby improving the uniformity of the phase after sintering; at the same time, the metal oxides can also be fully mixed with the preparation raw materials such as alumina, so as to fully form a network structure in which the mullite phase is interspersed in the corundum phase, further improving the mechanical properties.
[0053] The second and third heat preservation processes are mainly to promote the formation of mullite phase and increase the content of mullite phase, thereby improving the mechanical properties of the electrical ceramic material.
[0054] According to some embodiments of the present application, the method for preparing the modified aluminum silicate comprises the following steps:
[0055] mixing aluminum silicate, alkali and water to prepare pretreated aluminum silicate;
[0056] The pretreated aluminum silicate, vinyltrimethoxysilane and ethanol are mixed and refluxed.
[0057] According to some embodiments of the present application, the reflux temperature is 60°C to 70°C.
[0058] According to some embodiments of the present application, the reflux time is 5 h to 6 h.
[0059] The third aspect of the present application provides the use of the rare earth-doped electrical porcelain described in the first aspect of the present application in the preparation of insulators. DETAILED DESCRIPTION
[0060] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is described and illustrated below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. Based on the embodiments provided in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.
[0061] Obviously, the following descriptions are only some examples or embodiments of the present application. For ordinary technicians in this field, the present application can also be applied to other similar scenarios without creative work. In addition, it can also be understood that although the efforts made in this development process may be complicated and lengthy, for ordinary technicians in the field related to the content disclosed in this application, some changes in design, manufacturing or production based on the technical content disclosed in this application are just conventional technical means, and should not be understood as insufficient content disclosed in this application.
[0062] However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of substantially the same structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the following description is provided for those skilled in the art to fully understand the present application and is not intended to limit the subject matter described in the claims.
[0063] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0064] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0065] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0066] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0067] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0068] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0069] If there is no special explanation, the "include" and "comprising" mentioned in this application represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0070] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0071] Ceramic powder: 2CaO·MgO·2SiO2 powder, particle size (D50) is 5 μm.
[0072] Silicone rubber: The vinyl silicone rubber is XIAMETER RBG-0702, with a vinyl content of 0.2% and a molecular weight of 600,000 to 700,000.
[0073] The particle size (D50) of yttrium oxide (yttrium trioxide) is 4 μm.
[0074] Isocyanate: 1,3,5-tris(trimethoxysilylpropyl)polyisocyanate, Evonik Isocyanurate 88445.
[0075] The particle size (D50) of aluminum oxide was 5 μm.
[0076] The particle size (D50) of quartz is 3 μm.
[0077] The particle size (D50) of titanium dioxide is 200 nm.
[0078] The particle size (D50) of aluminum silicate was 10 μm.
[0079] Example 1
[0080] This embodiment is a rare earth doped insulator, which is composed of the following raw materials in parts by weight:
[0081] 100 parts of alumina, 60 parts of ceramic powder, 25 parts of quartz, 5 parts of titanium dioxide, 1.5 parts of rare earth dopant, 20 parts of dispersant (water) and 8 parts of forming agent.
[0082] The molding agent is composed of the following raw materials in parts by weight:
[0083] 10 parts of modified aluminum silicate, 2 parts of silicone rubber, 18 parts of isopropyl trioleyl titanate and 2 parts of isocyanate.
[0084] The rare earth dopant comprises the following raw materials in parts by weight:
[0085] 10 parts of yttrium trioxide, 30 parts of lanthanum stearate and 100 parts of solvent (ethanol);
[0086] The preparation method of the rare earth dopant comprises the following steps:
[0087] Yttrium trioxide, lanthanum stearate and a solvent were mixed and stirred (200 rpm), and evaporated to dryness at 40°C.
[0088] Modified aluminum silicate includes the following preparation raw materials:
[0089] Vinyltrimethoxysilane, aluminum silicate, and base (sodium carbonate).
[0090] The mass ratio of vinyltrimethoxysilane to aluminum silicate is 7.8:10.
[0091] The preparation method of modified aluminum silicate consists of the following steps:
[0092] Aluminum silicate, alkali (sodium carbonate, the mass ratio of sodium carbonate to aluminum silicate is 1:1) and water (the mass ratio of aluminum silicate to water is 1:10) are mixed (treated at 25°C for 2 hours), solid-liquid separation is performed, and the solid phase is collected to obtain pretreated aluminum silicate;
[0093] The pretreated aluminum silicate, vinyl trimethoxysilane and ethanol (the mass ratio of vinyl trimethoxysilane to ethanol is 1:10) are mixed and refluxed, and the solid-liquid separation is performed after reflux, and the solid phase is collected.
[0094] The reflux temperature was 65°C and the reflux time was 5 h.
[0095] The preparation method of the rare earth doped electric porcelain in this embodiment is composed of the following steps:
[0096] Alumina, ceramic powder, quartz, titanium dioxide, rare earth dopant and dispersant are mixed and spray-dried to obtain a first powder;
[0097] The first powder and the molding agent are mixed and pressed (pressing pressure is 1.2t / cm 2 ), to obtain a blank;
[0098] sintering the blank;
[0099] Sintering includes a first heating, a first heat preservation, a second heating, a second heat preservation, a third heating and a third heat preservation.
[0100] The starting temperature of the first heating was 25°C and the rate was 60°C / h;
[0101] The temperature of the first insulation is 550°C and the time of the first insulation is 2h;
[0102] The second heating rate is 120℃ / h;
[0103] The second insulation temperature is 1050°C and the second insulation time is 12h;
[0104] The rate of the third heating is 20℃ / h;
[0105] The temperature of the third insulation is 1250°C, and the time of the third insulation is 4 hours.
[0106] Example 2
[0107] This embodiment is a rare earth doped insulator, which is composed of the following raw materials in parts by weight:
[0108] 100 parts of alumina, 70 parts of ceramic powder, 27 parts of quartz, 10 parts of titanium dioxide, 1.5 parts of rare earth dopant, 20 parts of dispersant (water) and 7 parts of forming agent.
[0109] The molding agent is composed of the following raw materials in parts by weight:
[0110] 10 parts of modified aluminum silicate, 1.8 parts of silicone rubber, 12 parts of isopropyl trioleyl titanate and 1.8 parts of isocyanate.
[0111] The rare earth dopant comprises the following raw materials in parts by weight:
[0112] 10 parts of yttrium trioxide, 12 parts of lanthanum stearate and 100 parts of solvent (ethanol).
[0113] The preparation method of the rare earth dopant is carried out in accordance with Example 1.
[0114] Modified aluminum silicate includes the following preparation raw materials:
[0115] Vinyltrimethoxysilane, aluminum silicate, and base (sodium carbonate).
[0116] The mass ratio of vinyltrimethoxysilane to aluminum silicate is 7:10.
[0117] The mass ratio of sodium carbonate to aluminum silicate is 1:1.
[0118] The preparation method of modified aluminum silicate is carried out in accordance with Example 1.
[0119] The preparation method of rare earth-doped electric porcelain in the present application is carried out with reference to Example 1.
[0120] Example 3
[0121] This embodiment is a rare earth doped insulator, which is composed of the following raw materials in parts by weight:
[0122] 100 parts of alumina, 50 parts of ceramic powder, 30 parts of quartz, 8 parts of titanium dioxide, 1 part of rare earth dopant, 20 parts of dispersant (water) and 5 parts of forming agent.
[0123] The molding agent is composed of the following raw materials in parts by weight:
[0124] 10 parts of modified aluminum silicate, 1 part of silicone rubber, 20 parts of isopropyl trioleate acyloxy titanate and 1 part of isocyanate.
[0125] The rare earth dopant comprises the following raw materials in parts by weight:
[0126] 10 parts of yttrium trioxide, 40 parts of lanthanum stearate and 100 parts of solvent (ethanol);
[0127] The preparation method of the rare earth dopant is carried out in accordance with Example 1.
[0128] Modified aluminum silicate includes the following preparation raw materials:
[0129] Vinyltrimethoxysilane, aluminum silicate, and base (sodium carbonate).
[0130] The mass ratio of vinyltrimethoxysilane to aluminum silicate is 8:10.
[0131] The mass ratio of sodium carbonate to aluminum silicate is 1:1;
[0132] The preparation method of modified aluminum silicate is carried out in accordance with Example 1.
[0133] The preparation method of rare earth-doped electric porcelain in the present application is carried out with reference to Example 1.
[0134] Example 4
[0135] This embodiment is a rare earth doped insulator, which is composed of the following raw materials in parts by weight:
[0136] 100 parts of alumina, 100 parts of ceramic powder, 20 parts of quartz, 5 parts of titanium dioxide, 2 parts of rare earth dopant, 20 parts of dispersant (water) and 10 parts of forming agent.
[0137] The molding agent is composed of the following raw materials in parts by weight:
[0138] 10 parts of modified aluminum silicate, 2 parts of silicone rubber, 10 parts of isopropyl trioleate acyloxy titanate and 2 parts of isocyanate.
[0139] The rare earth dopant comprises the following raw materials in parts by weight:
[0140] 10 parts of yttrium trioxide, 20 parts of lanthanum stearate and 100 parts of solvent (ethanol);
[0141] Modified aluminum silicate includes the following preparation raw materials:
[0142] Vinyltrimethoxysilane, aluminum silicate, and base (sodium carbonate).
[0143] The mass ratio of vinyltrimethoxysilane to aluminum silicate is 7:10.
[0144] The mass ratio of sodium carbonate to aluminum silicate is 1:1.
[0145] The preparation method of modified aluminum silicate is carried out in accordance with Example 1.
[0146] The reflux temperature was 65°C and the reflux time was 5 h.
[0147] The preparation method of rare earth-doped electric porcelain in the present application is carried out with reference to Example 1.
[0148] Example 5
[0149] This embodiment is a rare earth doped insulator, which is different from the embodiment 4 in that the preparation method of the rare earth doped insulator in this embodiment is composed of the following steps:
[0150] Alumina, ceramic powder, quartz, titanium dioxide, rare earth dopant and dispersant are mixed and spray-dried to obtain a first powder;
[0151] The first powder and the molding agent are mixed and pressed (pressing pressure is 1.2t / cm 2 ), to obtain a blank;
[0152] sintering the blank;
[0153] Sintering consists of heating and heat preservation
[0154] The starting temperature of the heating is 25°C, and the rate is 80°C / h; the insulation temperature is 1250°C, and the insulation time is 16h.
[0155] Comparative Example 1
[0156] This comparative example is an insulator, and the differences from Example 5 are as follows:
[0157] The electric porcelain is composed of the following raw materials in parts by weight:
[0158] 100 parts of alumina, 100 parts of ceramic powder, 20 parts of quartz, 5 parts of titanium dioxide, 20 parts of dispersant (water) and 10 parts of forming agent.
[0159] The preparation method of the rare earth doped electric porcelain in this comparative example consists of the following steps:
[0160] Alumina, ceramic powder, quartz, titanium dioxide and a dispersant are mixed and spray-dried to obtain a first powder;
[0161] The first powder and the molding agent are mixed and pressed (pressing pressure is 1.2t / cm 2 ), to obtain a blank;
[0162] sintering the blank;
[0163] Sintering consists of heating up and keeping warm;
[0164] The starting temperature of the heating is 25°C, and the rate is 80°C / h; the insulation temperature is 1250°C, and the insulation time is 16h.
[0165] Comparative Example 2
[0166] This comparative example is an insulator, and the differences from Example 5 are as follows:
[0167] In this comparative example, aluminum silicate was not subjected to modification treatment.
[0168] That is, the molding agent is composed of the following raw materials in parts by weight:
[0169] 10 parts of aluminum silicate, 2 parts of silicone rubber, 18 parts of isopropyl trioleyl titanate and 2 parts of isocyanate.
[0170] Comparative Example 3
[0171] This comparative example is an insulator, and the difference from comparative example 2 is as follows:
[0172] In this comparative example, isopropyl trioleyl titanate is not added as the molding agent.
[0173] That is, the molding agent is composed of the following raw materials in parts by weight:
[0174] 10 parts of aluminum silicate, 2 parts of silicone rubber and 2 parts of isocyanate.
[0175] Comparative Example 4
[0176] This comparative example is an insulator, and the differences from Example 5 are as follows:
[0177] The rare earth dopant comprises the following raw materials in parts by weight:
[0178] 30 parts of lanthanum stearate and 100 parts of solvent (ethanol);
[0179] The preparation method of the rare earth dopant comprises the following steps:
[0180] Lanthanum stearate and the solvent were mixed and stirred (200 rpm), and evaporated to dryness at 40°C.
[0181] Comparative Example 5
[0182] This comparative example is an insulator, and the differences from Example 5 are as follows:
[0183] The rare earth dopant in this comparative example includes the following raw materials in parts by weight:
[0184] 10 parts of yttrium trioxide, 3.3 parts of lanthanum trioxide and 100 parts of solvent (ethanol).
[0185] The preparation method of the rare earth dopant comprises the following steps:
[0186] Yttrium trioxide, lanthanum trioxide and a solvent were mixed and stirred (200 rpm), and evaporated to dryness at 40°C.
[0187] The performance test results of the electrical ceramic materials of this application are shown in Table 1.
[0188] Table 1
[0189]
[0190]
[0191] The difference between Example 5 and Example 4 is that Example 5 is a single heat preservation treatment, and during the heating process, the organic matter cannot be fully decomposed, so during the formation of the mullite phase and the corundum phase, the residual organic matter will have a certain impact on the network structure, resulting in poor mechanical properties.
[0192] The difference between Comparative Example 1 and Example 5 is that in Comparative Example 1, there is no rare earth doping modifier, and the content of the mullite phase is greatly reduced, resulting in poor mechanical properties.
[0193] The difference between Comparative Example 2 and Example 5 is that aluminum silicate is not modified, and aluminum silicate plays a bonding role during the blank forming process, but is not modified by silane, and has poor compatibility with silicone rubber. The stability of the formed bonding network is poor, which leads to poor mechanical properties of the final electrical ceramic material.
[0194] The difference between Comparative Example 3 and Comparative Example 2 is that isopropyl trioleyl titanate is not added. Isopropyl trioleyl titanate contains organic segments, which is beneficial to improving compatibility. Failure to add this substance leads to further deterioration in the stability of the bonding network, resulting in poor mechanical properties of the final electrical ceramic material.
[0195] The difference between Comparative Example 4 and Example 5 is that yttrium oxide is not added to the rare earth dopant, resulting in a significant reduction in the content of the mullite phase, which leads to poor mechanical properties.
[0196] The difference between Comparative Example 5 and Example 5 is that lanthanum stearate is replaced by lanthanum oxide, and lanthanum stearate has good compatibility with silicone rubber and modified aluminum silicate; while lanthanum oxide has poor compatibility, which makes it more difficult to form an interlaced network structure between the mullite phase and the corundum phase, resulting in poor mechanical properties.
[0197] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A rare earth doped electric porcelain, characterized in that: The preparation includes the following raw materials: Alumina, ceramic powder, quartz, titanium dioxide, rare earth dopants, dispersants and forming agents; The molding agent comprises the following preparation raw materials: Modified aluminum silicate, silicone rubber, isopropyl trioleyl titanate and isocyanate; The rare earth dopant comprises the following preparation raw materials: Yttrium trioxide and lanthanum stearate.
2. The rare earth-doped electrical porcelain according to claim 1, characterized in that: The ceramic powder is magnesium-calcium-silicon ternary ceramic powder; And / or, the ceramic powder is 2CaO·MgO·2SiO2 powder; And / or, the mass fraction of magnesium oxide in the ceramic powder is 10% to 20%; And / or, the mass fraction of calcium oxide in the ceramic powder is 40% to 50%; And / or, the mass fraction of silicon oxide in the ceramic powder is 40% to 50%.
3. The rare earth-doped electrical porcelain according to claim 1, characterized in that: The preparation comprises the following raw materials in parts by weight: 100 parts of alumina, 50 to 100 parts of ceramic powder, 20 to 30 parts of quartz, 5 to 10 parts of titanium dioxide, 1 to 2 parts of rare earth dopant, 10 to 20 parts of dispersant and 5 to 10 parts of forming agent; And / or, the molding agent comprises the following raw materials in parts by weight: 10 parts of modified aluminum silicate, 1 to 2 parts of silicone rubber, 10 to 20 parts of isopropyl trioleate acyloxy titanate and 1 to 2 parts of isocyanate; And / or, the rare earth dopant includes the following preparation raw materials: Yttrium trioxide, lanthanum stearate and solvent; And / or, the rare earth dopant comprises the following raw materials in parts by weight: 10 parts of yttrium trioxide, 20 to 40 parts of lanthanum stearate and 100 to 200 parts of solvent; And / or, the solvent is ethanol.
4. The rare earth-doped insulator according to claim 1, characterized in that: The silicone rubber includes methyl vinyl silicone rubber; And / or, the vinyl content of the methyl vinyl silicone rubber is 0.15% to 0.25%; And / or, the molecular weight of the methyl vinyl silicone rubber is 600,000 to 700,000; And / or, the vinyl silicone rubber is XIAMETER RBG-0702.
5. The rare earth-doped electric porcelain according to claim 1, characterized in that: The modified aluminum silicate comprises the following preparation raw materials: Vinyltrimethoxysilane, aluminum silicate, and base; And / or, the mass ratio of vinyltrimethoxysilane to aluminum silicate is 7 to 8:
10.
6. The method for preparing rare earth-doped electric porcelain according to any one of claims 1 to 5, characterized in that: The following steps are involved: Mixing the prepared raw materials and then sintering them; The sintering temperature is 500°C to 1300°C.
7. The preparation method according to claim 6, characterized in that: The sintering includes a first heat preservation, a second heat preservation and a third heat preservation; And / or, the temperature of the first insulation is 500° C. to 600° C.; And / or, the first insulation time is 1h to 3h; And / or, the temperature of the second insulation is 1000° C. to 1100° C.; And / or, the second insulation time is 12h to 16h; And / or, the temperature of the third insulation is 1200° C. to 1300° C.; And / or, the third insulation time is 3h to 5h.
8. The preparation method according to claim 6, characterized in that: The preparation method of the modified aluminum silicate comprises the following steps: mixing aluminum silicate, alkali and water to prepare pretreated aluminum silicate; The pretreated aluminum silicate, vinyltrimethoxysilane and ethanol are mixed and refluxed.
9. The preparation method according to claim 8, characterized in that: The reflux temperature is 60°C to 70°C; And / or, the reflux time is 5h to 6h.
10. Use of the rare earth-doped electrical porcelain according to any one of claims 1 to 5 in the preparation of insulators.
Citation Information
Patent Citations
Efficient flame retardant cable sheath material
CN103897400A
Honeycomb type wear resistant composite material and preparation method thereof
CN105948786A
Electric porcelain insulator and preparation method thereof
CN108101526A
Electric porcelain insulator and preparation method thereof
CN110746178A
Injection molding alumina-based ceramic part composite material and preparation method thereof
CN114736009A
Cited By
Porcelain insulator for extra-high voltage direct current transmission and preparation method thereof
CN122426997A