Refractory material, heat-resistant part, preparation method of heat-resistant part and thermotechnical kiln

By adjusting the mass proportion of hollow alumina spheres, corundum powder, alumina powder and silicon powder, and using resin and explosion-proof fibers to form high-efficiency refractory materials, the structural instability and high thermal conductivity of traditional refractory materials at high temperatures is solved. The problem has achieved the improvement of high fire resistance and thermal insulation performance.

CN118908700APending Publication Date: 2024-11-08NINGDE XICHENG TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310502601.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-06
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional refractory materials are difficult to meet the high requirements for refractory resistance, strength and thermal insulation performance in graphitization processes, especially when sintering is used at high temperatures, there are problems of structural instability and high thermal conductivity.

Method used

The bone meal components are used, including hollow alumina spheres, corundum powder, alumina powder and silicon powder. By adjusting their mass proportion and coordination, combining resin as a binding agent, reducing cement content and adding explosion-proof during the preparation process fibers form efficient refractory materials.

Benefits of technology

It achieves good fire resistance, strength and structural stability at high temperatures, reduces thermal conductivity, improves thermal insulation performance, and extends the service life of graphitization furnace.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004215338510000201
    Figure BDA0004215338510000201
  • Figure BDA0004215338510000202
    Figure BDA0004215338510000202
  • Figure BDA0004215338510000211
    Figure BDA0004215338510000211
Patent Text Reader

Abstract

The invention relates to a refractory material, a heat-resistant workpiece, a preparation method of the heat-resistant workpiece and a thermotechnical kiln, the refractory material comprises the following components: bone meal, and the bone meal comprises alumina hollow spheres, corundum powder, alumina powder and silicon powder; in the bone powder, the mass ratio of the aluminum oxide hollow balls is greater than that of the corundum powder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of functional materials, and in particular to a refractory material, a heat-resistant product and a preparation method thereof, and a thermal kiln. Background Art

[0002] Industrial kilns are thermal equipment that utilizes heat to achieve various processing techniques such as melting, heating, drying, sintering and distillation of workpieces or materials. They have a relatively high operating temperature. For example, graphitization furnaces are mainly used for sintering and graphitization of carbon materials, graphitization of thermal conductive materials, sintering of carbon fiber ropes, sintering and graphitization of carbon fiber filaments, purification of graphite powder, and other high-temperature treatments of materials that can be graphitized under carbon environments. They have a very high operating temperature of 1600°C or above, and are currently the thermal kilns with the highest temperatures used in industrial production.

[0003] The furnace walls of industrial furnaces are generally made of refractory prefabricated parts made of refractory materials such as casting materials. They need to have high refractoriness and strength, and maintain a stable operating temperature during continuous production. Therefore, the refractory materials are also required to have good thermal insulation properties.

[0004] However, with the development of graphitization technology, the requirements for the refractoriness, strength and thermal insulation performance of graphitization furnaces are becoming increasingly higher. Traditional refractory materials are difficult to meet the demand and need further improvement. Summary of the invention

[0005] Based on this, it is necessary to provide a refractory material, a heat-resistant product and a preparation method thereof, and a thermal kiln, aiming to provide a refractory material having excellent refractory properties, mechanical strength and thermal insulation properties.

[0006] The present application is implemented through the following technical solutions.

[0007] In a first aspect of the present application, a refractory material is provided, wherein the components of the refractory material include bone powder, and the bone powder includes hollow alumina balls, corundum powder, alumina powder and silicon powder;

[0008] In the bone powder, the mass proportion of the hollow alumina spheres is greater than the mass proportion of the corundum powder.

[0009] The components of the above-mentioned refractory materials include bone powder of specific components, among which hollow alumina balls are used as aggregates, combined with specific types of powders: corundum powder, alumina powder and silicon powder, and the mass proportion of hollow alumina balls and corundum powder is controlled so that the components can work together. When used to prepare heat-resistant parts, it has excellent thermal insulation performance, high refractoriness, high strength and a small linear change rate. Even when sintered at high temperatures, it can maintain good refractoriness, strength and excellent structural stability.

[0010] In some embodiments, the bone powder includes, by weight: 47 to 75 parts of hollow alumina balls, 15 to 28 parts of corundum powder, 6 to 20 parts of alumina powder and 0.3 to 0.8 parts of silicon powder;

[0011] Optionally, the mass fraction of the corundum powder is 15 to 25 parts;

[0012] Optionally, the mass fraction of the alumina powder is 15 to 20 parts.

[0013] The specific mass ratio of the bone powder in the above-mentioned refractory material is further adjusted, with hollow alumina ball aggregate as the main material, combined with corundum powder, alumina powder and silicon powder in a specific mass ratio. When used to prepare heat-resistant parts, it has excellent thermal insulation performance, high refractoriness, high strength and a small linear change rate. Even when sintered at high temperatures, it can maintain good refractoriness, strength and excellent structural stability.

[0014] Furthermore, compared with traditional refractory materials with cement as the main ingredient, the cement content in the refractory materials of the present application is greatly reduced, which can reduce the liquid low-melting products generated during high-temperature sintering, further improve the refractoriness and strength of the refractory materials, while reducing the thermal conductivity and improving the thermal insulation performance.

[0015] In some embodiments, based on the total mass of the bone powder, the mass of the hollow alumina spheres accounts for 53% to 66%, the mass of the corundum powder accounts for 15% to 28%, the mass of the alumina powder accounts for 6% to 25%, and the mass of the silicon powder accounts for 0.25% to 0.7%;

[0016] Optionally, the mass proportion of the alumina powder is 13% to 25%;

[0017] Optionally, the mass proportion of the corundum powder is 15% to 27%;

[0018] Optionally, the mass proportion of the hollow alumina spheres is 53% to 65%.

[0019] The mass proportion of hollow alumina balls in refractory materials is adjusted to further improve the compatibility between aggregate and powder, and further improve the refractoriness, strength and thermal insulation properties.

[0020] In some embodiments, the mass ratio of the corundum powder to the alumina powder is 1:(0.7-1.6);

[0021] Optionally, the mass ratio of the corundum powder to the alumina powder is 1:(0.7-1.4).

[0022] The main component of corundum powder is alumina, which is the same as the main component of alumina powder. The two have similar functions, but also have differences. Both have high temperature resistance, and corundum powder also has higher density. By adjusting the mass ratio of corundum powder and alumina powder, on the one hand, the proportion of alumina in the refractory material can be adjusted, and on the other hand, the synergistic effect of the two can be enhanced to further improve the refractoriness, strength and thermal insulation performance.

[0023] In some embodiments, the refractory material further comprises a binder, and the binder comprises a resin;

[0024] Optionally, the resin includes a bonding resin;

[0025] More optionally, the resin includes one or more of linear phenolic resin, resol phenolic resin, polyurethane resin and epoxy resin.

[0026] The study found that when constructing traditional refractory materials for graphitizing furnaces, a large amount of water needs to be added as a binding agent. During the baking and heating process, a large amount of water vapor is generated. The construction, pouring or sintering of refractory materials are generally carried out in a relatively closed space, and the exhaust effect is not good. For example, when constructing parts in the gap between corundum bricks and lightweight bricks, a large amount of water vapor cannot be discharged in time. On the one hand, it returns to the refractory material, which will have an adverse effect on the performance of the parts at the least, and the masonry of the parts will burst at the worst. On the other hand, high-temperature water vapor that is not discharged in time will form high-pressure gas, which will impact the parts and destroy the structure of the parts, thereby adversely affecting the performance of the parts.

[0027] Therefore, the present application adopts resin as a binder, which can fully bond the bone powder without adding water. Compared with the amount of water vapor generated by traditional refractory materials due to high temperature during construction, the resin is used as a binder. During the manufacturing process and subsequent sintering process, the gas generated by the coking and decomposition of the resin is small. After coking, it mainly forms carbides, and the shrinkage rate of the carbides is small, which further reduces the linear change rate, thereby improving the structural stability of the material.

[0028] In some embodiments, the binder further comprises an organic solvent, and the mass proportion of the organic solvent in the binder is ≤5%;

[0029] The viscosity of the resin is relatively high, and a certain proportion of organic solvent is added to dilute it, while at the same time not introducing too much solvent to reduce the amount of vaporization during the production of the part.

[0030] Optionally, the organic solvent includes a small molecule alcohol solvent;

[0031] More optionally, the organic solvent includes an alcohol compound having 1 to 5 carbon atoms.

[0032] In some of the embodiments, the mass ratio of the bone powder to the binder is 100:(5-10).

[0033] The mass ratio of bone powder and binder is adjusted to ensure that the components are fully bonded and tightly combined.

[0034] In some embodiments, the bone powder satisfies at least one of the following conditions (1) to (3):

[0035] (1) The bone powder also includes explosion-proof fibers;

[0036] Optionally, the mass proportion of the explosion-proof fiber is 0.03% to 0.06%;

[0037] Optionally, under normal pressure, the melting point of the explosion-proof fiber is ≤110°C.

[0038] On the one hand, explosion-proof fibers can reduce the probability of refractory materials bursting during high-temperature use. On the other hand, in the process of preparing refractory materials into refractory parts, the explosion-proof fibers melt to leave space and form pores on the refractory parts, allowing the remaining small amount of gas to be discharged, reducing the probability of structural collapse and improving structural stability.

[0039] Further control the type of explosion-proof fiber and select explosion-proof fiber with a lower melting point so that the refractory material can melt at a lower temperature stage during the manufacturing process to form pores to act as exhaust channels, so that the small amount of gas remaining in the refractory material can be discharged from the material in time.

[0040] (2) The bone powder also includes calcium aluminate cement;

[0041] Optionally, the mass percentage of the calcium aluminate cement is 0.26% to 0.8%;

[0042] (3) The bone powder also includes a dispersant as a component;

[0043] Optionally, the mass percentage of the dispersant is 0.04% to 0.09%;

[0044] Optionally, the dispersant includes at least one of sodium tripolyphosphate and sodium hexametaphosphate.

[0045] In some embodiments, the hollow alumina sphere includes a first hollow alumina sphere, a second hollow alumina sphere, and a third hollow alumina sphere;

[0046] Wherein, the particle size range T1 of the first hollow alumina sphere satisfies: 3mm<T1≤5mm;

[0047] The particle size range T2 of the second hollow alumina sphere satisfies: 1mm≤T2≤3mm;

[0048] The particle size range T3 of the third hollow alumina sphere satisfies: 0.2 mm ≤ T3 < 1 mm.

[0049] In some embodiments, the mass ratio of the first alumina hollow sphere, the second alumina hollow sphere and the third alumina hollow sphere is (15-25):(20-30):(12-20).

[0050] The combination of alumina hollow balls of various particle sizes and powder can further improve the packing density, thereby improving the volume stability of the refractory material and making the material structure strength of the refractory material greater after high-temperature sintering.

[0051] In some embodiments, the bone powder satisfies at least one of the following conditions (4) to (6):

[0052] (4) The upper limit of the particle size range of the corundum powder is 45 μm;

[0053] Optionally, the particle size of the corundum powder is in the range of 35 μm to 45 μm;

[0054] (5) The upper limit of the particle size range of the alumina powder is 2 μm;

[0055] (6) The silicon powder is silicon micropowder;

[0056] Optionally, the upper limit of the particle size range of the silicon powder is 38 μm.

[0057] The particle size of each powder is further adjusted to form a better particle size match with the hollow alumina spheres, further improving the material structure strength of the refractory material when used in high-temperature sintering.

[0058] In some embodiments, the bone powder satisfies at least one of the following conditions (7) to (8):

[0059] (7) The corundum powder comprises white corundum powder;

[0060] Compared with other types of corundum, white corundum powder has less impurities, higher purity and better mechanical properties.

[0061] (8) The alumina powder includes α-alumina powder.

[0062] α-Alumina is the most stable phase of alumina and can further improve the structural stability of refractory materials.

[0063] According to a second aspect of the present application, a heat-resistant article is provided, wherein the raw material of the heat-resistant article comprises the refractory material according to the first aspect.

[0064] Furthermore, even when sintered at 1600°C or above, it can maintain good refractoriness, strength and structural stability.

[0065] In some embodiments, the heat-resistant article satisfies at least one of the following conditions (9) to (12);

[0066] (9) The fixed carbon content of the heat-resistant article is ≥ 3.5%;

[0067] (10) The aluminum oxide content in the heat-resistant article is ≥ 94%;

[0068] (11) The porosity of the heat-resistant article is 55% to 68%;

[0069] (12) The refractoriness of the heat-resistant article is ≥ 1780°C;

[0070] Optionally, the refractoriness of the heat-resistant article is greater than 1800°C.

[0071] In a third aspect of the present application, a method for preparing a heat-resistant article is provided, comprising the following steps:

[0072] The raw material of the heat-resistant article is baked and formed to prepare the heat-resistant article; wherein the raw material includes the refractory material of the first aspect.

[0073] According to a fourth aspect of the present application, a thermal kiln is provided, wherein the thermal kiln comprises the heat-resistant article according to the second aspect or the heat-resistant article produced by the method for producing the heat-resistant article according to the third aspect.

[0074] In some embodiments, the thermal furnace is a graphitization furnace.

[0075] The above-mentioned heat-resistant parts have high refractoriness and good high temperature resistance, which can meet the use requirements of the graphitization furnace under high temperature conditions. At the same time, they have low thermal conductivity and good heat insulation effect. On the one hand, they can reduce heat loss and improve the thermal efficiency of the continuous graphitization furnace. On the other hand, they can reduce the speed of heat conduction to other parts to increase the service life of the graphitization furnace. At the same time, they have excellent compressive strength and can meet the harsh conditions of graphitization treatment. DETAILED DESCRIPTION

[0076] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0077] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0078] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0079] The "range" disclosed in this application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range.

[0080] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0081] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0082] Unless otherwise specified, the terms "include", "contain" and "comprise" mentioned in this application may be open-ended or closed-ended. For open-ended situations, for example, the terms "include", "contain" and "comprise" may mean that other members, elements or method steps not listed may also be included or comprised, or may only include or comprise the listed members, elements or method steps.

[0083] The terms "combination thereof", "any combination thereof", "any combination thereof" and the like used in this application include all suitable combinations of any two or more of the listed items.

[0084] In the present application, the “suitable” mentioned in “suitable combination”, “suitable method”, “any suitable method”, etc. shall be based on the technical solution that can implement the present application.

[0085] In this application, "preferred", "better", "more preferred", and "suitable" are only used to describe implementation methods or examples with better effects, and it should be understood that they do not constitute a limitation on the scope of protection of this application. If multiple "preferred" items appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "preferred" item is independent.

[0086] In this application, "optionally", "optional", and "optional" mean optional or dispensable, that is, any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.

[0087] In the present application, "further", "further", "particularly" and the like are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present application.

[0088] In the present application, the terms "first", "second", "third", "fourth", etc. in "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0089] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Furthermore, the weight described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0090] An embodiment of the present application provides a refractory material, the components of which include bone powder, the bone powder including hollow alumina balls, corundum powder, alumina powder and silicon powder;

[0091] In the bone powder, the mass proportion of alumina hollow spheres is greater than that of corundum powder.

[0092] The components of the above-mentioned refractory materials include bone powder of specific components, among which hollow alumina balls are used as aggregates, combined with specific types of powders: corundum powder, alumina powder and silicon powder, and the mass proportion of hollow alumina balls and corundum powder is controlled so that the components can work together. When used to prepare heat-resistant parts, it has excellent thermal insulation performance, high refractoriness and high strength. Even when sintered at high temperatures, it can maintain good refractoriness, strength and structural stability.

[0093] In some of the embodiments, the bone powder includes, by weight: 47 to 75 parts of hollow alumina spheres, 15 to 28 parts of corundum powder, 6 to 20 parts of alumina powder and 0.3 to 0.8 parts of silicon powder.

[0094] The components of the above-mentioned refractory materials include bone powder with a specific mass ratio, among which alumina hollow balls are used as aggregates, and are matched with corundum powder, alumina powder and silicon powder with a specific mass ratio. When used to prepare heat-resistant parts, it has excellent thermal insulation performance, high refractoriness, high strength and a small linear change rate. Even when sintered at high temperatures, it can maintain good refractoriness, strength and excellent structural stability.

[0095] The specific components of the above-mentioned refractory materials work together to make the refractory materials have higher refractoriness and lower thermal conductivity. Among them, alumina powder and silicon powder have extremely large specific surface area and high surface activity. They can generate corundum-mullite phase during high-temperature sintering and have greater high-temperature compressive strength. The specific components can be stacked tightly, so that the refractory materials can form a stronger structure when used during high-temperature sintering, and have excellent refractoriness, strength and thermal insulation properties.

[0096] Furthermore, compared with traditional refractory materials with cement as the main ingredient, the cement content in the refractory materials of the present application is greatly reduced, which can reduce the liquid low-melting products generated during high-temperature sintering, further improve the refractoriness and strength of the refractory materials, while reducing the thermal conductivity and improving the thermal insulation performance.

[0097] In some of the embodiments, the mass fraction of the corundum powder is 15 to 25 parts.

[0098] In some embodiments, the mass fraction of the alumina powder is 15 to 20. The mass fraction of the corundum powder or the mass fraction of the alumina powder is further adjusted to further improve the refractoriness and strength of the refractory material.

[0099] In the above “47 to 75 parts of hollow alumina spheres”, the mass fraction of the hollow alumina spheres includes the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: “47 parts, 48 ​​parts, 49 parts, 50 parts, 51 parts, 52 parts, 53 parts, 54 parts, 55 parts, 56 parts, 57 parts, 58 parts, 59 parts, 60 parts, 61 parts, 62 parts, 63 parts, 64 parts, 65 parts, 66 parts, 67 parts, 68 parts, 69 parts , 70, 71, 72, 73, 74 or 75 parts; or a range consisting of any two numerical values, including but not limited to: 47 to 70, 47 to 65, 47 to 60, 47 to 55, 47 to 50, 50 to 75, 50 to 70, 50 to 65, 50 to 60, 50 to 55, 55 to 75, 55 to 70, 55 to 65, 55 to 60, 60 to 75, 60 to 70, 60 to 65 parts.

[0100] In the above-mentioned "15 to 28 parts of corundum powder", the mass fraction of corundum powder includes the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: "15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts; or a range consisting of any two numerical values, including but not limited to: 15 to 24 parts, 15 to 23 parts, 15 to 22 parts, 15 to 21 parts, 15 to 20 parts, 15 to 19 parts, 18 to 24 parts, 18 to 23 parts, 18 to 22 parts, 18 to 21 parts, 18 to 20 parts, or 20 to 25 parts.

[0101] In the above-mentioned "6 to 20 parts of alumina powder", the mass fraction of alumina powder includes the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: "6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts; or a range consisting of any two values, including but not limited to: 11 to 20 parts, 12 to 20 parts, 13 to 20 parts, 14 to 20 parts, 15 to 20 parts, 16 to 20 parts, 17 to 20 parts, 11 to 18 parts, 12 to 18 parts, 13 to 18 parts, 14 to 18 parts, 15 to 18 parts, 16 to 18 parts.

[0102] In the above-mentioned "0.03 parts to 0.06 parts of explosion-proof fiber", the mass fraction of the explosion-proof fiber includes the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: 0.03 parts, 0.04 parts, 0.05 parts or 0.06 parts.

[0103] In the above-mentioned "0.3 parts to 0.8 parts of silicon powder", the mass fraction of silicon powder includes the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: 0.3 parts, 0.4 parts, 0.5 parts, 0.6 parts, 0.7 parts or 0.8 parts.

[0104] In the above-mentioned "0.3 parts to 0.8 parts of calcium aluminate cement", the mass fraction of calcium aluminate cement includes the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: 0.3 parts, 0.4 parts, 0.5 parts, 0.6 parts, 0.7 parts or 0.8 parts.

[0105] In some of the embodiments, based on the total mass of bone powder, the mass of hollow alumina spheres accounts for 53% to 66%, the mass of corundum powder accounts for 15% to 28%, the mass of alumina powder accounts for 6% to 25%, and the mass of silicon powder accounts for 0.25% to 0.7%.

[0106] In the above "53%~66%", the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%; or a range consisting of any two values.

[0107] In the above "15%~28%", the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%; or a range consisting of any two values.

[0108] In the above "6% to 25%", the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%; or a range consisting of any two values.

[0109] In the above “0.25% to 0.7%”, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: “0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, 0.6%, 0.65%, 0.7%.

[0110] Optionally, the mass proportion of alumina powder is 13% to 25%.

[0111] Optionally, the mass proportion of corundum powder is 15% to 27%.

[0112] Optionally, the mass proportion of the hollow alumina spheres is 53% to 65%.

[0113] The mass ratio of hollow alumina balls in the refractory material is regulated to further improve the compatibility between aggregate and powder, and further improve the refractoriness, strength and thermal insulation performance. In some embodiments, the mass ratio of corundum powder to alumina powder is 1:(0.7-1.6).

[0114] In some of the embodiments, the mass ratio of corundum powder to alumina powder is 1:(0.7-1.4).

[0115] The main component of corundum powder is alumina, which is the same as the main component of alumina powder. The two have similar functions, but also have differences. Both have high temperature resistance, and corundum powder also has higher density. By adjusting the mass ratio of corundum powder and alumina powder, on the one hand, the proportion of alumina in the refractory material can be adjusted, and on the other hand, the synergistic effect of the two can be enhanced to further improve the refractoriness, strength and thermal insulation performance.

[0116] In the above "1:(0.7~1.4)", the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.2, 1:1.3, 1:1.4.

[0117] In some of the embodiments, the components of the refractory material further include a binder, and the components of the binder include a resin;

[0118] Optionally, the resin comprises a bonding resin.

[0119] Optionally, the resin includes one or more of linear phenolic resin, resol phenolic resin, polyurethane resin and epoxy resin.

[0120] The study found that when constructing traditional refractory materials for graphitizing furnaces, a large amount of water needs to be added as a binding agent. During the baking and heating process, a large amount of water vapor is generated. The construction, pouring or sintering of refractory materials are generally carried out in a relatively closed space, and the exhaust effect is not good. For example, when constructing parts in the gap between corundum bricks and lightweight bricks, a large amount of water vapor cannot be discharged in time. On the one hand, it returns to the refractory material, which will have an adverse effect on the performance of the parts at the least, and the masonry of the parts will burst at the worst. On the other hand, high-temperature water vapor that is not discharged in time will form high-pressure gas, which will impact the parts and destroy the structure of the parts, thereby adversely affecting the performance of the parts.

[0121] Therefore, the present application adopts resin as a binder, which can fully bond the bone powder without adding water. Compared with the amount of water vapor generated by traditional refractory materials due to high temperature during construction, the resin is used as a binder. During the manufacturing process and subsequent sintering process, the gas generated by the coking and decomposition of the resin is small. After coking, it mainly forms carbides, and the shrinkage rate of the carbides is small, which further reduces the linear change rate, thereby improving the structural stability of the material.

[0122] In some embodiments, the binder further comprises an organic solvent, and the mass proportion of the organic solvent in the binder is ≤5%.

[0123] The viscosity of the resin is relatively high, and a certain proportion of organic solvent is added to dilute it, while at the same time not introducing too much solvent to reduce the amount of vaporization during the production of the part.

[0124] Optionally, the organic solvent includes a small molecule alcohol solvent.

[0125] More optionally, the organic solvent includes an alcohol compound having 1 to 5 carbon atoms.

[0126] In some embodiments thereof, the organic solvent includes a monoalcohol compound or a polyol compound having 1 to 5 carbon atoms; further specific examples include but are not limited to: at least one of methanol, ethanol, ethylene glycol, butanol, propanol and propylene glycol.

[0127] In some of the embodiments, the mass ratio of bone powder to binder is 100:(5-10).

[0128] The mass ratio of bone powder and binder is adjusted to ensure that the components are fully bonded and tightly combined.

[0129] In the above "100:(5~10)", the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: 100:5, 100:6, 100:7, 100:8, 100:9, 100:10.

[0130] In some of these embodiments, the components of the bone meal further include a dispersant;

[0131] Dispersants can act as lubricants and further promote the bonding between the components.

[0132] In some of the embodiments, the bone powder also includes explosion-proof fibers.

[0133] On the one hand, explosion-proof fibers can reduce the probability of refractory materials bursting during high-temperature use. On the other hand, in the process of preparing refractory materials into refractory parts, the explosion-proof fibers melt to leave space and form pores on the refractory parts, allowing the remaining small amount of gas to be discharged, reducing the probability of structural collapse and improving structural stability.

[0134] In some of the embodiments, the mass percentage of the explosion-proof fiber is 0.03% to 0.06%.

[0135] Optionally, under normal pressure, the melting point of the explosion-proof fiber is ≤110°C.

[0136] Further control the type of explosion-proof fiber and select explosion-proof fiber with a lower melting point so that the refractory material can melt at a lower temperature stage during the manufacturing process to form pores to act as exhaust channels, so that the small amount of gas remaining in the refractory material can be discharged from the material in time.

[0137] In some embodiments, the bone powder component also includes calcium aluminate cement.

[0138] Optionally, the mass proportion of calcium aluminate cement is 0.26% to 0.8%.

[0139] In the above “0.26%~0.8%”, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: “0.26%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%.

[0140] According to the mass proportion of Al2O3 in calcium aluminate cement, calcium aluminate cement can be divided into ordinary calcium aluminate cement and pure calcium aluminate cement. The mass proportion of Al2O3 in ordinary calcium aluminate cement is less than 72%, generally between 53% and 72%, while the mass proportion of Al2O3 in pure calcium aluminate cement is ≥72%, generally between 72% and 82%.

[0141] In some of these embodiments, the calcium aluminate cement comprises pure calcium aluminate cement.

[0142] In some embodiments, the bone meal composition further includes a dispersant.

[0143] Optionally, the mass fraction of the explosion-proof fiber is 0.03 parts to 0.06 parts by mass.

[0144] Optionally, the mass percentage of the dispersant is 0.04% to 0.09%.

[0145] In the above-mentioned "0.04% to 0.09%", the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%.

[0146] Optionally, the mass fraction of calcium aluminate cement is 0.3 to 0.8 parts by mass.

[0147] In some of the embodiments, the mass fraction of the dispersant is 0.03 parts to 0.1 parts by mass.

[0148] In the above "0.03 parts to 0.1 parts", the value of the dispersant includes the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: 0.03 parts, 0.04 parts, 0.05 parts, 0.06 parts, 0.07 parts, 0.08 parts, 0.09 parts or, 0.1 parts.

[0149] In the above "0.03 parts to 0.06 parts", the mass fraction of explosion-proof fiber includes the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: 0.03 parts, 0.04 parts, 0.05 parts or 0.06 parts.

[0150] In the above-mentioned "0.3 parts to 0.8 parts of calcium aluminate cement", the mass fraction of calcium aluminate cement includes the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: 0.3 parts, 0.4 parts, 0.5 parts, 0.6 parts, 0.7 parts or 0.8 parts.

[0151] In some embodiments, the dispersant includes at least one of sodium tripolyphosphate and sodium hexametaphosphate.

[0152] In some embodiments, the dispersant includes at least one of sodium tripolyphosphate and sodium hexametaphosphate.

[0153] In some of the embodiments, the mass ratio of sodium tripolyphosphate to the sodium hexametaphosphate is 1:(0.8-1.2).

[0154] The mixture of sodium tripolyphosphate and sodium hexametaphosphate can improve the dispersion performance of the base fabric.

[0155] In some of the embodiments, based on the total mass of the refractory material, the mass of the hollow alumina spheres accounts for 50% to 63%.

[0156] In some of the embodiments, based on the total mass of the refractory material, the mass of the hollow alumina spheres accounts for 50% to 62%.

[0157] In the above-mentioned "50% to 63%", the mass proportion of the alumina hollow spheres includes the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: 50%, 50.5%, 51%, 51.5%, 52%, 52.5%, 53%, 53.5%, 54%, 54.5%, 55%, 55.5%, 56%, 56.5%, 57%, 57.5%, 58%, 58.5%, 59%, 59.5%, 60%, 60.5%, 61%, 61.5%, 62%, 62.5%, 63%.

[0158] In some of the embodiments, the alumina hollow spheres include first alumina hollow spheres, second alumina hollow spheres and third alumina hollow spheres; wherein, the particle size range T1 of the first alumina hollow spheres satisfies: 3mm<T1≤5mm; the particle size range T2 of the second alumina hollow spheres satisfies: 1mm≤T2≤3mm; the particle size range T3 of the third alumina hollow spheres satisfies: 0.2mm≤T3<1mm.

[0159] It should be noted that the hollow alumina sphere has a cavity structure inside, and the cavity structure is surrounded by a shell layer. The shell layer includes an inner layer in contact with the cavity structure and an outer layer away from the cavity structure. The particle size of the hollow alumina sphere calculated based on the outer layer is the outer particle size. T1, T2 and T3 all refer to the outer particle size range of the hollow alumina sphere.

[0160] In some of the embodiments, the mass ratio of the first alumina hollow sphere, the second alumina hollow sphere and the third alumina hollow sphere is (15-25):(20-30):(12-20).

[0161] The combination of alumina hollow balls of various particle sizes and powder can further improve the packing density, thereby improving the volume stability of the refractory material and making the material structure strength of the refractory material greater after high-temperature sintering.

[0162] In some of the embodiments, the mass fraction of the first hollow alumina sphere is (15-25) parts.

[0163] In some of the embodiments, the mass fraction of the second hollow alumina spheres is (20-30) parts.

[0164] In some of the embodiments, the mass fraction of the third hollow alumina sphere is (12-20) parts.

[0165] In the above "(15-25) parts", the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, and 25 parts.

[0166] In the above "(20-30) parts", the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts or 30 parts.

[0167] In the above "(12 to 20) parts", the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and the following point values: 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts or 20 parts.

[0168] In some embodiments, the upper limit of the particle size range of the corundum powder is 45 μm.

[0169] Optionally, the particle size of the corundum powder is in the range of 35 μm to 45 μm.

[0170] In some embodiments, the upper limit of the particle size range of the alumina powder is 2 μm.

[0171] In some embodiments, the silicon powder is silicon micropowder.

[0172] Optionally, the upper limit of the particle size range of the silicon powder is 38 μm.

[0173] The particle size of each powder is further adjusted to form a better particle size match with the hollow alumina spheres, further improving the material structure strength of the refractory material when used in high-temperature sintering.

[0174] It can be understood that in the present application, the particle size range of the material can be understood as the particle size of the material falling within this range; further, the particle size range of the material can be tested using the particle size measurement methods commonly used in the art, including but not limited to: microscopy, Coulter counting, sedimentation, screening and laser diffraction analysis of particle size.

[0175] Specifically, the sieving method is used: the sieving method is one of the most traditional particle size testing methods, which is to test the particle size by passing the particles through sieve holes of different sizes; specifically, sieves of different mesh numbers correspond to different ranges of particle sizes. Generally speaking, mesh number × aperture (micrometer number) = 15000.

[0176] In some embodiments, the corundum powder includes white corundum powder.

[0177] Compared with other types of corundum, white corundum powder has less impurities, higher purity and better mechanical properties.

[0178] In some embodiments, the alumina powder includes α-alumina powder.

[0179] α-Alumina is the most stable phase of alumina and can further improve the structural stability of refractory materials.

[0180] In some of the embodiments, the melting point of the explosion-proof fiber is ≤110° C. under normal pressure.

[0181] Optionally, under normal pressure, the melting point of the explosion-proof fiber is ≤100°C.

[0182] By adjusting the type of explosion-proof fiber and selecting explosion-proof fiber with a lower melting point, the refractory material can be melted at a lower temperature stage during the manufacturing process to form pores to serve as exhaust channels, so that the small amount of gas remaining in the refractory material can be discharged from the material in time.

[0183] According to a second aspect of the present application, a heat-resistant article is provided, wherein the raw material of the heat-resistant article comprises the refractory material according to the first aspect.

[0184] The components of the above-mentioned refractory materials include bone powder of specific components, among which hollow alumina balls are used as aggregates, combined with specific types of powders: corundum powder, alumina powder and silicon powder, and the mass proportion of hollow alumina balls and corundum powder is controlled so that the components can work together. When used to prepare heat-resistant parts, it has excellent thermal insulation performance, high refractoriness and high strength. Even when sintered at high temperatures, it can maintain good refractoriness, strength and structural stability.

[0185] Furthermore, even when sintered at 1600°C or above, it can maintain good refractoriness, strength and structural stability.

[0186] In some of the embodiments, the fixed carbon content in the heat-resistant article is ≥ 3.5%.

[0187] In some of the embodiments, the aluminum oxide content in the heat-resistant article is ≥ 94%.

[0188] In some embodiments, the porosity of the heat-resistant article is 55% to 68%.

[0189] In some of the embodiments, the refractoriness of the heat-resistant article is ≥ 1780°C.

[0190] In some of the embodiments, the refractoriness of the heat-resistant article is greater than 1800°C.

[0191] A third aspect of the present application provides a method for preparing a heat-resistant part, comprising the following step S10.

[0192] Step S10, baking and molding the raw materials of the heat-resistant article to prepare the heat-resistant article; wherein the raw materials include the refractory material of the first aspect.

[0193] In some of the embodiments, the baking temperature is 100°C to 120°C; further, the baking time is based on removing the solvent in the raw material components; specifically, the baking time is 12h to 24h.

[0194] The heat-resistant article of the present application has no specific restrictions on shape, and the specific shape can be determined according to the application scenario; specifically, the baking molding is carried out in a mold, and the shape of the heat-resistant article is controlled by the shape of these molds.

[0195] In a fourth aspect of the present application, a thermal kiln is provided, wherein the thermal kiln comprises the heat-resistant article according to the second aspect or the heat-resistant article produced by the method for producing the heat-resistant article according to the third aspect.

[0196] In some embodiments, the thermal furnace is a graphitization furnace.

[0197] The above-mentioned heat-resistant parts have high refractoriness and good high temperature resistance, which can meet the use requirements of the graphitization furnace under high temperature conditions. At the same time, they have low thermal conductivity and good heat insulation effect. On the one hand, they can reduce heat loss and improve the thermal efficiency of the continuous graphitization furnace. On the other hand, they can reduce the speed of heat conduction to other parts to increase the service life of the graphitization furnace. At the same time, they have excellent compressive strength and can meet the harsh conditions of graphitization treatment.

[0198] The present invention will be described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments. It should be understood that the attached claims summarize the scope of the present invention. Under the guidance of the concept of the present invention, those skilled in the art should realize that certain changes made to the various embodiments of the present invention will be covered by the spirit and scope of the claims of the present invention.

[0199] The following are specific embodiments. Specific embodiments

[0201] Example 1

[0202] (1) Preparation of refractory materials:

[0203] S1: Provide the following bone powder materials in the following mass proportions: 20 parts of first alumina hollow spheres with a particle size range of T1, 25 parts of first alumina hollow spheres with a particle size range of T2, 20 parts of first alumina hollow spheres with a particle size range of T3, 20 parts of white corundum fine powder with a particle size of 35μm to 45μm, 14 parts of α-alumina micropowder with a particle size of 2μm, 0.05 parts of explosion-proof fiber, 0.4 parts of silica micropowder (U951 type) with a particle size of 400 mesh, 0.5 parts of CA-80 pure calcium aluminate cement and 0.05 parts of dispersant;

[0204] A binder is provided, which includes linear phenolic resin (2130 resin) and 95% industrial alcohol, the mass ratio of the resin to the industrial alcohol is 100:5, and the added amount of the binder is 5.5% of the weight of the bone powder.

[0205] Among them, 3mm<T1≤5mm, 1mm≤T2≤3mm, 0.2mm≤T<1mm, where T1, T2 and T3 all refer to the actual outer diameter of the hollow alumina sphere, which can be tested by screening with sieves of different mesh sizes.

[0206] The explosion-proof fiber (model LXDR-100) has a melting point of 100° C. at normal pressure; the dispersant includes sodium tripolyphosphate (P3) and sodium hexametaphosphate (P6) in a mass ratio of 1:1.

[0207] S2: Mix the above-mentioned bone powder, binder and dispersant to prepare a refractory material.

[0208] (2) Preparation of heat-resistant parts:

[0209] S1, pour the above refractory material into a mold to make a piece of The sample was left to stand for 24 hours and then baked at 110°C for 24 hours to form a dry heat-resistant product.

[0210] S2. The heat-resistant parts were prepared by the fused glass sheet method, and the mass proportion of alumina and the fixed carbon content in the prepared heat-resistant parts were tested by X-ray fluorescence spectrometer (XRF) and reference standard process: GB / T21114-2019. Please see Table 1 for details.

[0211] (3) Performance testing of heat-resistant parts.

[0212] S1: Thermal conductivity test: Place the prepared heat-resistant parts into a high-temperature thermal conductivity tester (DRS-3), set the hot surface temperature to 1000°C for testing, refer to the standard process: GB / T 4130-2005, and see Table 3 for specific results.

[0213] S2. Place the obtained heat-resistant product in an oxygen environment, slowly raise the temperature to 1600°C within 8 hours, and sinter at this temperature for 3 hours to obtain a sintered refractory product.

[0214] Specific test process: weigh the dry mass of the sample, determine the sample volume by liquid static weighing method, calculate the apparent porosity, and refer to YB / T 5200-93 for specific steps. Test the porosity of the heat-resistant parts prepared and the heat-resistant parts after sintering, see Table 1 for details.

[0215] S3: The bulk density of the heat-resistant article prepared and the heat-resistant article after sintering is tested respectively. The specific steps refer to GB / T 2997-2015, including the following steps:

[0216] Specific test process: weigh the mass m1 of the sample after drying, the mass m2 suspended in the immersion liquid after saturated immersion, and the mass m3 of the sample in the air after immersion. According to the formula, volume density = m1 / (m3-m2)×volume density of the immersion liquid.

[0217] Required equipment: water absorption vacuum device (CZ-0.5), electronic balance, electric drying oven.

[0218] S4: The compressive strength of the heat-resistant parts prepared and the heat-resistant parts after sintering are tested respectively. The specific steps refer to GB / T 3001-2017 and are carried out using a microcomputer-controlled electro-hydraulic servo pressure testing machine (YAW-2000D).

[0219] S4: Test the linear change rate of the heat-resistant parts obtained and the heat-resistant parts after sintering respectively: refer to the standard process: GB / T 5988-2007, the main steps are as follows:

[0220] Six 160mm×40mm×40mm strips were prepared for length measurement, placed in a test furnace, heated to the test temperature at a specified heating rate, and maintained for a certain time. After cooling to room temperature, their lengths were measured again, and their linear change rates were calculated. The smaller the absolute value of the linear change rate, the smaller the probability of structural expansion or collapse of the sample to be tested, and the better the structural stability.

[0221] Required equipment: Vernier caliper, high temperature test furnace (CSL-1700).

[0222] S5. The refractoriness of the heat-resistant parts was tested according to GB / T 7322. The specific results are shown in Table 3.

[0223] Embodiments 2 to 12

[0224] Examples 2 to 12 are substantially the same as Example 1, except that in step (1), the components and proportions of the refractory materials are different from those in Example 1. For details, please see Tables 1 and 2.

[0225] The other step conditions are the same as those in Example 1. Please see Table 3 for specific parameters and test results.

[0226] Comparative Examples 1-2

[0227] The only difference is that in step (1), the components and proportions of the refractory materials are different from those in Example 1, as shown in Tables 1 and 2 for details.

[0228] The other step conditions are the same as those in Example 1. Please see Table 3 for specific parameters and test results.

[0229] The mass fraction ratio of the refractory materials in each embodiment and comparative example is shown in Table 1.

[0230] Table 1

[0231]

[0232] Note: “ / ” means not adding the material.

[0233] The proportions of the refractory components in the embodiments and comparative examples in terms of mass percentage are shown in Table 2, wherein the amount of binder added accounts for Y1 of the weight of the bone powder, based on the total mass of the bone powder, the mass proportion of the hollow alumina spheres is Y2, and based on the total mass of the bone powder, the mass proportions of the hollow alumina spheres, corundum powder, alumina powder, explosion-proof fiber, silica powder, calcium aluminate cement and dispersant are recorded as X1, X2, X3, X4, X5, X6 and X7 respectively.

[0234] Table 2

[0235]

[0236]

[0237] The properties and parameters of the heat-resistant parts made of the refractory materials of the embodiments and comparative examples are shown in Table 3, wherein the mass proportion of aluminum oxide in the heat-resistant parts is W1, and the fixed carbon content is W2.

[0238] Table 3

[0239]

[0240] It should be noted that the maximum test temperature of the refractoriness test furnace of the National Testing Center is 1800°C. The refractoriness > 1800°C in the above Table 2 means that the object to be tested can remain stable and not melt at the maximum test temperature of 1800°C in the test furnace, which means that the refractoriness of the object to be tested exceeds 1800°C; and the temperature during the test changes in units of tens or twenty. Referring to GB / T7322, the Testing Center will correct the tens digit of the tested refractoriness value to tens.

[0241] Analysis of the data in Table 3: By comparing and analyzing the embodiment and comparative example 1, it can be seen that the refractory material in the present application has excellent thermal insulation performance, high refractoriness and high strength.

[0242] Moreover, the absolute value of the linear change rate of the product made of the refractory material in the embodiment of the present application is small, indicating that the probability of structural expansion or collapse of the product after heating is smaller, and the structural stability is better. Therefore, when the heat-resistant product of the present application is applied to thermal kilns such as graphitization furnaces, it can meet the use requirements of graphitization furnaces under high temperature conditions, and can still maintain high strength and good structural stability even when used for high-temperature sintering.

[0243] Furthermore, by comparing and analyzing the performance data of Example 4, Examples 1 to 3, and Example 5, it can be seen that adjusting the composition ratio of the refractory materials can further improve the fire resistance, strength, and structural stability of the product.

[0244] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0245] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims, and the description can be used to interpret the content of the claims.

Claims

1. A refractory material, wherein the components of the refractory material include bone powder, and the bone powder includes hollow alumina balls, corundum powder, alumina powder and silicon powder; In the bone powder, the mass proportion of the hollow alumina spheres is greater than the mass proportion of the corundum powder.

2. The refractory material according to claim 1, characterized in that The bone powder comprises, by weight: 47 to 75 parts of hollow alumina balls, 15 to 28 parts of corundum powder, 6 to 20 parts of alumina powder and 0.3 to 0.8 parts of silicon powder; Optionally, the mass fraction of the corundum powder is 15 to 25 parts; Optionally, the mass fraction of the alumina powder is 15 to 20 parts.

3. The refractory material according to any one of claims 1 to 2, characterized in that: Based on the total mass of the bone powder, the mass of the hollow alumina spheres accounts for 53% to 66%, the mass of the corundum powder accounts for 15% to 28%, the mass of the alumina powder accounts for 6% to 25%, and the mass of the silicon powder accounts for 0.25% to 0.7%; Optionally, the mass proportion of the alumina powder is 13% to 25%; Optionally, the mass proportion of the corundum powder is 15% to 27%; Optionally, the mass proportion of the hollow alumina spheres is 53% to 65%.

4. The refractory material according to any one of claims 1 to 2, characterized in that: The mass ratio of the corundum powder to the alumina powder is 1:(0.7-1.6); Optionally, the mass ratio of the corundum powder to the alumina powder is 1:(0.7-1.4).

5. The refractory material according to any one of claims 1 to 2, characterized in that: The components of the refractory material also include a binder, and the components of the binder include resin; Optionally, the resin includes a bonding resin; Optionally, the resin includes one or more of linear phenolic resin, resol phenolic resin, polyurethane resin and epoxy resin.

6. The refractory material according to claim 5, characterized in that The mass ratio of the bone powder to the binder is 100:(5-10).

7. The refractory material according to claim 5, characterized in that The binder further comprises an organic solvent, and the mass proportion of the organic solvent in the binder is ≤5%; Optionally, the organic solvent includes a small molecule alcohol solvent; More optionally, the organic solvent includes an alcohol compound having 1 to 5 carbon atoms.

8. The refractory material according to any one of claims 1 to 2, characterized in that: The bone powder meets at least one of the following conditions (1) to (3): (1) The bone powder also includes explosion-proof fibers; Optionally, the mass proportion of the explosion-proof fiber is 0.03% to 0.06%; Optionally, under normal pressure, the melting point of the explosion-proof fiber is ≤110°C; (2) The bone powder also includes calcium aluminate cement; Optionally, the mass percentage of the calcium aluminate cement is 0.26% to 0.8%; (3) The bone powder also includes a dispersant as a component; Optionally, the mass percentage of the dispersant is 0.04% to 0.09%; More optionally, the dispersant includes at least one of sodium tripolyphosphate and sodium hexametaphosphate.

9. The refractory material according to any one of claims 1 to 2, characterized in that: The alumina hollow spheres include a first alumina hollow sphere, a second alumina hollow sphere and a third alumina hollow sphere; Wherein, the particle size range T1 of the first hollow alumina sphere satisfies: 3mm<T1≤5mm; The particle size range T2 of the second hollow alumina sphere satisfies: 1mm≤T2≤3mm; The particle size range T3 of the third hollow alumina sphere satisfies: 0.2 mm ≤ T3 < 1 mm.

10. The refractory material according to claim 9, characterized in that The mass ratio of the first alumina hollow sphere, the second alumina hollow sphere and the third alumina hollow sphere is (15-25):(20-30):(12-20).

11. The refractory material according to any one of claims 1 to 2, characterized in that: The bone powder meets at least one of the following conditions (4) to (6): (4) The upper limit of the particle size range of the corundum powder is 45 μm; Optionally, the particle size of the corundum powder is in the range of 35 μm to 45 μm; (5) The upper limit of the particle size range of the alumina powder is 2 μm; (6) The silicon powder is silicon micropowder; Optionally, the upper limit of the particle size range of the silicon powder is 38 μm.

12. The refractory material according to any one of claims 1 to 2, characterized in that: The bone powder meets at least one of the following conditions (7) to (8): (7) The corundum powder comprises white corundum powder; (8) The alumina powder includes α-alumina powder.

13. A heat-resistant article, characterized in that: The raw material of the heat-resistant article comprises the refractory material according to any one of claims 1 to 12.

14. The heat-resistant article according to claim 13, characterized in that: The heat-resistant article satisfies at least one of the following conditions (9) to (12); (9) The fixed carbon content of the heat-resistant article is ≥ 3.5%; (10) The aluminum oxide content in the heat-resistant article is ≥ 94%; (11) The porosity of the heat-resistant article is 55% to 68%; (12) The refractoriness of the heat-resistant article is ≥ 1780°C; Optionally, the refractoriness of the heat-resistant article is greater than 1800°C.

15. A method for preparing a heat-resistant article, characterized in that: The steps include: The raw material of the heat-resistant article is baked and formed to prepare the heat-resistant article; wherein the raw material comprises the refractory material according to any one of claims 1 to 12.

16. A thermal kiln, characterized in that: The thermal kiln comprises the heat-resistant article according to any one of claims 13 to 14 or the heat-resistant article produced by the method for producing the heat-resistant article according to claim 15.

17. The thermal furnace according to claim 16, characterized in that: The thermal kiln is a graphitization furnace.

Citation Information

Patent Citations

  • Composite combining corundum based refractory materials

    CN101423401A

  • Refractory castable composition with heat insulation and wear resistance and application thereof

    CN101555146A

  • Alumina bubble lightweight insulating refractory casting material

    CN101723687A

  • Casting material with thermal insulation function

    CN103613394A

  • High-purity hollow alumina sphere brick applied to coal water slurry gasifier and preparation process thereof