K / Ba / Y / Cr / V / W doped CaBi2Nb2O9 high-temperature piezoelectric ceramic material and preparation method thereof
By doping CaBi2Nb2O9 ceramic material with K+/Ba2+/Y3+ and Cr2+/V5+/W6+ and combining it with spark plasma sintering technology, a high-temperature piezoelectric ceramic material was prepared, which solved the problems of low Curie temperature and insufficient piezoelectric performance, and achieved high-temperature stability and environmentally friendly applications.
Patent Information
- Application Number
- CN202410975897.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-19
AI Technical Summary
Existing piezoelectric ceramic materials suffer from low Curie temperature, insufficient piezoelectric properties, and lead content, which is harmful to the environment, making it difficult to meet the application requirements in high-temperature environments.
High-temperature piezoelectric ceramic materials were prepared by using K+/Ba2+/Y3+ and Cr2+/V5+/W6+ composite high-valence ions to dope CaBi2Nb2O9 ceramic materials at A and B sites, combined with spark plasma sintering technology.
The Curie temperature and piezoelectric properties of the material have been improved, resulting in a piezoelectric ceramic material that is stable at high temperatures and environmentally friendly, suitable for sensors, transducers and other components in high-temperature environments.
Smart Images

Figure CN118908714A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of piezoelectric ceramic materials, and in particular to a method for preparing a doped bismuth layered structure calcium bismuth niobate high-temperature piezoelectric ceramic material. Background Art
[0002] At present, the most widely used piezoelectric ceramic material is mainly lead zirconate titanate piezoelectric ceramics, but this type of piezoelectric ceramics contains lead, which causes harm to the environment and human body during production, use and waste disposal, and the Curie temperature of this type of piezoelectric ceramics is generally below 400℃. Due to the existence of the depolarization phenomenon of piezoelectric materials, piezoelectric materials cannot work normally above the Curie temperature. With the rapid development of aerospace, geological exploration and other work and in line with the needs of sustainable development of human society, it is necessary to seek an environmentally friendly piezoelectric material with high Curie temperature and excellent piezoelectric performance.
[0003] Bismuth layered ceramics have the characteristics of high Curie temperature, low dielectric loss, obvious anisotropy of electromechanical coupling coefficient, high resistivity, no pollution, low leakage current, excellent ferroelectric properties, etc., and are candidate materials suitable for high temperature environments. Bismuth layered ceramic materials are composed of (Bi 2 O 2 ) 2+ The layers and perovskite structure lattice layers are alternately stacked, and its chemical formula is (Bi 2 O 2 ) 2+ (A m-1 B m O 3m+1 ) 2- , among which CaBi 2 Nb 2 O 9 (CBN) is a typical bismuth layered ferroelectric material, A is a 12-coordinated Ca 2+ , B is 6-coordinated Nb 5+ , m = 2, composed of fluorite structure (Bi 2 O 2 ) 2+ Layer and perovskite structure CaNb 2 O 3 layer composition, the Curie temperature (T C ≈943℃) is the highest among bismuth layered ceramics, but the piezoelectric constant is very low (d 33 ≈6pC / N). Therefore, how to maintain a high Curie temperature while improving the piezoelectric activity and obtaining CBN piezoelectric ceramic materials with excellent comprehensive electrical properties has become an important research topic in the field of high-temperature piezoelectric ceramic materials. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a K / Ba / Y / Cr / V / W doped CaBi 2 Nb 2 O 9 High temperature piezoelectric ceramic materials, for CaBi 2 Nb 2 O 9 Ca in the A position of ceramic materials 2+ ions, using K with 12 coordination + , Ba 2+ , Y 3+ Composition of complex high-valent ions [K 0.2 Ba 0.2 Y 0.6 ] 2.4+ Doping substitution is performed for Nb at the B position 5+ ions, using Cr with 6 coordination 2+ 、V 5+ , W 6+ Composition of complex high-valent ions [Cr 0.1 V 0.2 W 0.7 ] 5.4+ Doping substitution is performed so that through the above-mentioned composite doping modification, while maintaining a high Curie temperature, its piezoelectric properties and high-temperature resistivity are improved, thereby providing a new type of piezoelectric ceramic material with excellent comprehensive electrical properties and environmental friendliness. Another object of the present invention is to provide the above-mentioned K / Ba / Y / Cr / V / W doped CaBi 2 Nb 2 O 9 Preparation method of high temperature piezoelectric ceramic material.
[0005] The purpose of the present invention is achieved through the following technical solutions:
[0006] The present invention provides a K / Ba / Y / Cr / V / W doped CaBi 2 Nb 2 O 9 High temperature piezoelectric ceramic materials, with 12-coordinated K + , Ba 2+ , Y 3+ The complex high-valent ions [K 0.2 Ba 0.2 Y 0.6 ] 2.4+ Doping substitution CaBi 2 Nb 2 O 9 Ca in the A position 2+ ions, with Cr having 6 coordination 2+ 、V 5+ , W 6+The complex high-valent ions [Cr 0.1 V 0.2 W 0.7 ] 5.4+ Doping substitution CaBi 2 Nb 2 O 9 Nb in the middle B position 5+ ions, the chemical formula is Ca 1-x [K 0.2 Ba 0.2 Y 0.6 ] x Bi 2 Nb 2-y [Cr 0.1 V 0.2 W 0.7 ] y O 9 , where 0.02≤x≤0.065, 0.015≤y≤0.04.
[0007] In the above scheme, the piezoelectric ceramic material of the present invention has a 33 ≥19pC / N, T C ≥893℃; Resistivity (ρ) ≥2.5×10 at 500℃ 8 Ω·cm, dielectric loss (tanδ) ≤ 0.35%; d after annealing at 800℃ 33 ≥16pC / N.
[0008] Another object of the present invention is achieved by the following technical solutions:
[0009] The K / Ba / Y / Cr / V / W doped CaBi 2 Nb 2 O 9 A method for preparing a high temperature piezoelectric ceramic material comprises the following steps:
[0010] (1) Preparation of pre-synthesized precursor powder
[0011] CaCO 3 , K 2 CO 3 、BaCO 3 , Y 2 O 3 、Bi 2 O 3 , Nb 2 O 5 Cr 2 O 3 、V 2 O 5 , WO 3As raw materials corresponding to Ca, K, Ba, Y, Bi, Nb, Cr, V, and W in the chemical formula; each raw material is mixed according to the stoichiometric amount in the chemical formula, and then a ball milling treatment is performed using anhydrous ethanol as a ball milling medium, and the obtained material is dried, sieved, pressed and formed, and then placed in a sealed crucible for calcination; then the calcined material is ground and sieved, and a secondary ball milling treatment is performed, and the obtained material is dried, ground and sieved to obtain a pre-synthesized precursor powder;
[0012] (2) Preparation of high temperature piezoelectric ceramic materials
[0013] The pre-synthesized precursor powder is loaded into a graphite mold, and placed in a spark plasma sintering furnace for a calcination treatment to obtain a carbon-containing sintered product; then the carbon-containing sintered product is placed in an ordinary high-temperature furnace under an air atmosphere for a secondary calcination treatment to decarbonize, thereby obtaining a decarbonized sintered product; finally, the decarbonized sintered product is polarized to obtain a high-temperature piezoelectric ceramic material.
[0014] Furthermore, in the step (1) of the preparation method of the present invention, the pressure of the pressing molding is 4-6 MPa; the calcination treatment is to increase the temperature to 830-880° C. at 5° C. / min and keep the temperature for 3-5 hours.
[0015] Furthermore, in the first calcination treatment in step (2) of the preparation method of the present invention, the spark plasma sintering furnace pressure is 40-45MPa, the DC pulse current is 600-650A, the temperature is first increased to 900°C at 100°C / min, then increased to 950-1000°C at 20°C / min, kept warm for 5-6min, cooled to 600°C at a cooling rate of 50°C / min, the DC pulse current is stopped, and then the pressure is released and the furnace is cooled to room temperature; the second calcination treatment is increased to 700-750°C at 5°C / min, kept warm for 4-4.5h, and cooled to room temperature with the furnace.
[0016] In the above scheme, the polarization treatment in step (2) of the preparation method of the present invention is to first polish the surface of the decarbonized sintered product; then perform electrode coating treatment, that is, silver electrodes are applied to the upper and lower surfaces of the decarbonized sintered product after polishing; then increase the temperature to 700-800°C at 5°C / min for calcination, keep warm for 20-30 minutes, and cool to room temperature with the furnace; finally, polarize in high-temperature silicone oil at 180-200°C with a DC voltage of 10-15kV / mm for polarization for 25-35 minutes.
[0017] Using the above K / Ba / Y / Cr / V / W doped CaBi 2 Nb 2 O 9 Products obtained by the preparation method of high-temperature piezoelectric ceramic materials.
[0018] The present invention has the following beneficial effects:
[0019] (1) In the preparation of CaBi 2 Nb 2 O 9 In the process of preparing piezoelectric ceramic materials, due to the volatilization of bismuth at high temperature, bismuth vacancies will inevitably be formed, thereby generating vacancy defects. In view of this phenomenon, the present invention adopts a valence ratio of A-site Ca 2+ Ions with high complex high valence [K 0.2 Ba 0.2 Y 0.6 ] 2.4+ Doping and substitution are performed to increase the mixing entropy of the material. 5+ Ionic high complex ions [Cr 0.1 V 0.2 W 0.7 ] 5.4+ Doping and substitution are performed to make the A and B positions both defective, making the perovskite layer (A m- 1 B m O 3m+1 ) 2- Producing electrons, thereby enhancing the bismuth oxide layer (Bi 2 O 2 ) 2+ and perovskite-like layers (A m-1 B m O 3m+1 ) 2- The interaction between them can regulate the growth behavior of the grains, causing them to produce polarized nanodomains locally, and finally obtain CaBi with excellent performance. 2 Nb 2 O 9 High temperature piezoelectric ceramic materials.
[0020] (2) The present invention adopts advanced spark plasma sintering technology, which requires low sintering temperature and short sintering time, thus low energy consumption, and high density of the sintered material, which can obtain CaBi with excellent performance. 2 Nb 2 O 9 High temperature piezoelectric ceramic materials.
[0021] (3) CaBi doped with K, Ba, Y and Cr, V, W in the present invention 2 Nb 2 O 9 Piezoelectric ceramic materials, Curie temperature above 893 ° C, piezoelectric constant d 33 ≥19pC / N, d after annealing at 800℃ 33 ≥16pC / N; resistivity ≥2.5×10 at 500℃8 Ω·cm, dielectric loss ≤0.35%. The material has good high temperature stability and can fully meet the application requirements of piezoelectric ceramic sensors, transducers, brakes and other components in high temperature environments, and has broad application prospects in high temperature electronic equipment.
[0022] (4) The preparation method of the present invention adopts advanced ceramic preparation technology, has low firing temperature, low preparation cost, simple and easy process operation, and easy control of influencing factors. It is suitable for large-scale industrial production and is conducive to promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The present invention will be further described in detail below with reference to the embodiments and accompanying drawings:
[0024] Figure 1 is the XRD crystal phase spectrum of the piezoelectric ceramic materials of the embodiments of the present invention and the comparative examples;
[0025] Figure 2 is the piezoelectric constant d of the piezoelectric ceramic materials of the embodiment of the present invention and the comparative example 33 Curves changing with temperature. DETAILED DESCRIPTION
[0026] Embodiment 1:
[0027] This embodiment is a K / Ba / Y / Cr / V / W doped CaBi 2 Nb 2 O 9 A method for preparing a high temperature piezoelectric ceramic material, wherein the piezoelectric ceramic material has a chemical formula of Ca 0.94 [K 0.2 Ba 0.2 Y 0.6 ] 0.06 Bi 2 Nb 1.985 [Cr 0.1 V 0.2 W 0.7 ] 0.015 O 9 , the preparation method has the following steps:
[0028] (1) Preparation of pre-synthesized precursor powder
[0029] With 99.9% pure CaCO 3 , K 2 CO 3 、BaCO 3 , Y 2 O 3 、Bi 2 O 3 , Nb 2 O 5 Cr2 O 3 、V 2 O 5 , WO 3 As raw materials corresponding to Ca, K, Ba, Y, Bi, Nb, Cr, V, and W in the above chemical formula, each raw material is prepared according to the stoichiometric amount in the above chemical formula, and then anhydrous ethanol is used as a ball milling medium, and a ball: material: anhydrous ethanol = 4: 1: 3 is used, and a ball milling treatment is performed on a planetary ball mill at a speed of 400 r / min for 24 hours. The obtained material is dried, passed through an 80-mesh sieve, pressed and formed at 4 MPa, and then placed in a sealed crucible, and the temperature is increased to 840° C. at 5° C. / min and calcined in an oxidizing atmosphere for 4 hours; the calcined material is ground and passed through an 80-mesh sieve, and a secondary ball milling treatment is performed using the same process as the primary ball milling treatment, and the obtained material is dried, ground, and passed through an 80-mesh sieve to obtain a pre-synthesized precursor powder;
[0030] (2) Preparation of high temperature piezoelectric ceramic materials
[0031] (2-1) 0.8 g of the above-mentioned pre-synthesized precursor powder was loaded into a cylindrical graphite mold with a diameter of 20 mm, and placed in a spark plasma sintering furnace. The pressure was set to 45 MPa and the DC pulse current was set to 600 A. The temperature was first raised to 900° C. at 100° C. / min, and then raised to 960° C. at 20° C. / min. A calcination treatment was performed. After keeping the temperature for 6 minutes, the temperature was lowered to 600° C. at a cooling rate of 50° C. / min. The DC pulse current was stopped, and then the pressure was released. The product was cooled to room temperature in the furnace to obtain a carbon-containing sintered product.
[0032] (2-2) placing the carbon-containing sintered product in a common high-temperature furnace, and performing secondary calcination treatment at a temperature of 5°C / min to 750°C in an air atmosphere to decarbonize the product, keeping the temperature for 4.5 hours, and cooling the product to room temperature to obtain a decarbonized sintered product;
[0033] (2-3) The decarburized sintered product is subjected to the following polarization treatment: first, the surface of the decarburized sintered product is polished; then, electrode coating is performed, i.e., silver electrodes are applied to the upper and lower surfaces of the decarburized sintered product after polishing; then, the temperature is raised to 800°C at a rate of 5°C / min, the temperature is kept for 25 minutes, and the product is cooled to room temperature with the furnace; finally, the product is polarized in high-temperature silicone oil at 180°C with a DC voltage of 10 to 15 kV / mm for 30 minutes, thereby obtaining a high-temperature piezoelectric ceramic material.
[0034] Embodiment 2:
[0035] This embodiment is a K / Ba / Y / Cr / V / W doped CaBi 2 Nb 2 O 9The method for preparing high temperature piezoelectric ceramic material is different from that of the first embodiment in that:
[0036] 1. The general chemical formula of this embodiment is Ca 0.955 [K 0.2 Ba 0.2 Y 0.6 ] 0.045 Bi 2 Nb 1.97 [Cr 0.1 V 0.2 W 0.7 ] 0.03 O 9 .
[0037] 2. The calcination temperature in step (1) is 880°C and the holding time is 5h.
[0038] 3. The calcination system in step (2-1) is as follows: set the pressure to 40 MPa and the DC pulse current to 620 A, first heat the temperature to 900 ° C at 100 ° C / min, then heat the temperature to 1000 ° C at 20 ° C / min, carry out a calcination treatment, keep warm for 5 minutes, then cool the temperature to 600 ° C at a rate of 50 ° C / min, stop the DC pulse current, and then release the pressure, cool to room temperature with the furnace to obtain a carbon-containing sintered product.
[0039] Embodiment three:
[0040] This embodiment is a K / Ba / Y / Cr / V / W doped CaBi 2 Nb 2 O 9 The method for preparing high temperature piezoelectric ceramic material is different from that of the first embodiment in that:
[0041] 1. The general chemical formula of this embodiment is Ca 0.975 [K 0.2 Ba 0.2 Y 0.6 ] 0.025 Bi 2 Nb 1.96 [Cr 0.1 V 0.2 W 0.7 ] 0.04 O 9 .
[0042] 2. The calcination temperature in step (1) is 880°C and the holding time is 3.5h.
[0043] 3. The calcination system in step (2-1) is as follows: the pressure is set to 40 MPa and the DC pulse current is set to 620 A. The temperature is first raised to 900 ° C at 100 ° C / min, and then raised to 980 ° C at 20 ° C / min. A calcination treatment is performed. After keeping the temperature for 5 minutes, the temperature is reduced to 600 ° C at a cooling rate of 50 ° C / min, the DC pulse current is stopped, and then the pressure is released. The product is cooled to room temperature in the furnace to obtain a carbon-containing sintered product.
[0044] Comparative Example:
[0045] Undoped, chemically CaBi 2 Nb 2 O 9 A high temperature piezoelectric ceramic material is used as a comparative example, and its preparation steps are the same as those in Example 1.
[0046] The XRD crystal phase spectra of the piezoelectric ceramic materials of the embodiments of the present invention and the comparative examples are as follows: Figure 1 As shown, from Figure 1 It can be seen that the diffraction peaks of the piezoelectric ceramic materials obtained in the embodiments and comparative examples are completely consistent with the standard spectrum PDF 00-49-0608, indicating that the obtained materials are CaBi with a single crystal phase. 2 Nb 2 O 9 Material.
[0047] Piezoelectric constant d of piezoelectric ceramic materials in the embodiments of the present invention and the comparative examples 33 The temperature change curve is as follows Figure 2 As shown. Figure 2 It can be seen that from room temperature to 600°C, the d 33 The value decreases slightly with the increase of temperature. At 800℃, d 33 The value still remains above 84% of that at room temperature, indicating that the material has good temperature stability and is conducive to its application in high temperature fields.
[0048] The performance test results of the piezoelectric ceramic materials of the embodiments of the present invention and the comparative examples are shown in Table 1.
[0049] Table 1 Properties of piezoelectric ceramic materials of the embodiments of the present invention and comparative examples
[0050]
Claims
1. A K / Ba / Y / Cr / V / W doped CaBi 2 Nb 2 O 9 High temperature piezoelectric ceramic materials, Features: With 12-coordinate K + , Ba 2+ , Y 3+ The complex high-valent ions [K 0.2 Ba 0.2 Y 0.6 ] 2.4+ Doping substitution CaBi 2 Nb 2 O 9 Ca in the A position 2+ ions, with Cr having 6 coordination 2+ 、V 5+ , W 6+ The complex high-valent ions [Cr 0.1 V 0.2 W 0.7 ] 5.4+ Doping substitution CaBi 2 Nb 2 O 9 Nb in the middle B position 5+ ions, the chemical formula is Ca 1-x [K 0.2 Ba 0.2 Y 0.6 ] x Bi 2 Nb 2-y [Cr 0.1 V 0.2 W 0.7 ] y O 9 , where 0.02≤x≤0.065, 0.015≤y≤0.
04.
2. K / Ba / Y / Cr / V / W doped CaBi according to claim 1 2 Nb 2 O 9 High temperature piezoelectric ceramic materials, Features: The d of the piezoelectric ceramic material 33 ≥19pC / N, T C ≥893℃; Resistivity (ρ) ≥2.5×10 at 500℃ 8 Ω·cm, dielectric loss (tanδ) ≤ 0.35%; d after annealing at 800℃ 33 ≥16pC / N.
3. K / Ba / Y / Cr / V / W doped CaBi according to claim 1 or 2 2 Nb 2 O 9 Preparation method of high temperature piezoelectric ceramic material, Features The following steps are involved: (1) Preparation of pre-synthesized precursor powder CaCO 3 , K 2 CO 3 、BaCO 3 , Y 2 O 3 、Bi 2 O 3 , Nb 2 O 5 Cr 2 O 3 、V 2 O 5 , WO 3 As raw materials corresponding to Ca, K, Ba, Y, Bi, Nb, Cr, V, and W in the chemical formula; each raw material is mixed according to the stoichiometric amount in the chemical formula, and then a ball milling treatment is performed using anhydrous ethanol as a ball milling medium, and the obtained material is dried, sieved, pressed and formed, and then placed in a sealed crucible for calcination; then the calcined material is ground and sieved, and a secondary ball milling treatment is performed, and the obtained material is dried, ground and sieved to obtain a pre-synthesized precursor powder; (2) Preparation of high temperature piezoelectric ceramic materials The pre-synthesized precursor powder is loaded into a graphite mold, and placed in a spark plasma sintering furnace for a calcination treatment to obtain a carbon-containing sintered product; then the carbon-containing sintered product is placed in an ordinary high-temperature furnace under an air atmosphere for a secondary calcination treatment to decarbonize, thereby obtaining a decarbonized sintered product; finally, the decarbonized sintered product is polarized to obtain a high-temperature piezoelectric ceramic material.
4. K / Ba / Y / Cr / V / W doped CaBi according to claim 3 2 Nb 2 O 9 Preparation method of high temperature piezoelectric ceramic material, Features: The pressure of the pressing molding in the step (1) is 4-6 MPa; the calcination treatment is to increase the temperature to 830-880° C. at 5° C. / min and keep the temperature for 3-5 hours.
5. K / Ba / Y / Cr / V / W doped CaBi according to claim 3 2 Nb 2 O 9 Preparation method of high temperature piezoelectric ceramic material, Features: The primary calcination treatment in step (2) is as follows: the spark plasma sintering furnace pressure is 40-45 MPa, the DC pulse current is 600-650A, the temperature is first raised to 900°C at 100°C / min, then raised to 950-1000°C at 20°C / min, kept at that temperature for 5-6 minutes, then cooled to 600°C at a cooling rate of 50°C / min, the DC pulse current is stopped, and then the pressure is released and the furnace is cooled to room temperature; the secondary calcination treatment is as follows: the temperature is raised to 700-750°C at 5°C / min, kept at that temperature for 4-4.5 hours, and then cooled to room temperature with the furnace.
6. K / Ba / Y / Cr / V / W doped CaBi according to claim 3 2 Nb 2 O 9 Preparation method of high temperature piezoelectric ceramic material, Features: The polarization treatment in step (2) is as follows: first, the surface of the decarburized sintered product is polished; then, an electrode coating treatment is performed, i.e., silver electrodes are applied to the upper and lower surfaces of the decarburized sintered product after polishing; then, the temperature is raised to 700-800°C at 5°C / min for calcination, the temperature is kept for 20-30 minutes, and the product is cooled to room temperature with the furnace; finally, the product is polarized in high-temperature silicone oil at 180-200°C with a DC voltage of 10-15 kV / mm for a polarization time of 25-35 minutes.
7. Using the K / Ba / Y / Cr / V / W doped CaBi as claimed in any one of claims 3 to 6 2 Nb 2 O 9 The product is obtained by the preparation method of high-temperature piezoelectric ceramic material.
Citation Information
Patent Citations
Doping modified bismuth calcium niobate ceramic material and preparation method thereof
CN101941841A
Calcium bismuth niobate high-temperature piezoceramic material of bismuth layer structure and preparing method of calcium bismuth niobate high-temperature piezoceramic material
CN106554203A
Ce, Cr and W co-doped CaBi4Ti4O15 high-temperature piezoelectric ceramic material and preparation method thereof
CN117263678A
Bismuth calcium niobate-based bismuth layered structure ferroelectric piezoelectric ceramic and preparation method thereof
CN117964359A