Gallium-doped zinc oxide target material and preparation method thereof
By using dispersed grinding of gallium oxide and zinc oxide powder and acid solution treatment in ZnO targets, combined with cold isostatic pressure and two-stage sintering processes, the problem of insufficient density and compressive strength of ZnO targets is solved, and high efficiency is achieved Improve conductivity and process simplification.
Patent Information
- Application Number
- CN202411096182.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-08
AI Technical Summary
The density and compressive strength of existing ZnO targets are insufficient, the grinding process requirements are high, the preparation process is complex, and it is difficult to achieve efficient electrical conductivity improvement.
Gallium oxide powder and zinc oxide powder are dispersed in deionized water, grinding and spray granulation, grinding in an acidic solution, dried and molded, and cold isostatic pressure and two-stage sintering processes are carried out to form a gallium zinc oxide target.
The dense microstructure and relatively high density of gallium-doped zinc oxide targets are realized, the process steps are simplified, the sintering temperature is reduced, and the conductivity and compressive strength are improved.
Smart Images

Figure CN118908719A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of target material preparation, and specifically discloses a gallium-doped zinc oxide target material and a preparation method thereof. Background Art
[0002] Transparent conductive oxide (TCO) is a thin film material with high transmittance and low resistivity in the visible light spectrum range (380nm<λ<780nm). This type of material combines transparency and conductivity and is a typical example of wide bandgap semiconductors or insulators that introduce carriers through element doping to achieve conductivity. TCO films mainly include oxides of In, Sb, Zn and Cd and their composite multi-element oxide thin film materials, such as indium oxide (In2O3), tin oxide (SnO2), zinc oxide (ZnO) and cadmium oxide (CdO). They have excellent optoelectronic properties such as wide bandgap, low resistivity, high light transmittance in the visible light region and high light reflectivity in the infrared spectral region. They are widely used in solar cells, flat panel displays, organic light-emitting diodes, low-emissivity glass, special functional window coatings, transparent thin film transistors and flexible electronic devices.
[0003] Among all kinds of TCO thin film materials, ZnO-based thin film materials are not only low-cost and abundant in reserves, but also non-toxic and harmless. Compared with traditional transparent conductive materials such as ITO and FTO, they are not inferior in terms of optoelectronic performance. Therefore, they have emerged in recent years and become a hot topic of research. ZnO targets are prepared by sputtering or other thin film deposition techniques to obtain ZnO transparent conductive films. In modern electronic and photovoltaic technologies, ZnO targets are the cornerstone. In order to further improve the density, compressive strength and conductivity of ZnO targets, elements such as Ga, Sn and Nb are usually added to ZnO targets. CN116041047A discloses an IZO doped target material for sputtering and a preparation method thereof, comprising: (1) mixing indium oxide powder, zinc oxide powder, doped oxide powder, water, a dispersant and a binder to prepare a slurry; (2) spraying and granulating the slurry obtained in step (1) to obtain a granulated powder; (3) subjecting the granulated powder obtained in step (2) to dry pressing and cold isostatic pressing, and then sintering at normal pressure to obtain the IZO doped target material for sputtering. Although the doped oxide powder has a wide range of selectivity, this method requires high grinding technology by mixing and grinding raw materials with large and small particle sizes to prepare a slurry. Summary of the invention
[0004] In view of the problems existing in the prior art, the object of the present invention is to provide a gallium-doped zinc oxide target and a preparation method thereof.
[0005] To achieve the above objectives, the present invention provides the following specific technical solutions.
[0006] First, the present invention provides a method for preparing a gallium-doped zinc oxide target, comprising the following steps: Gallium oxide powder and zinc oxide powder are added into deionized water containing a dispersant and a binder and dispersed to obtain slurry I; The slurry I is ground and then spray granulated to obtain granulated powder; Grinding the granulated powder in an acidic solution to obtain slurry II; After the slurry II is dried and formed, it is subjected to cold isostatic pressing to obtain a green blank; The green blank is sintered to obtain a gallium-doped zinc oxide target.
[0007] In a further preferred embodiment, the particle size D50 of the gallium oxide powder is 1-5 μm; the particle size D50 of the zinc oxide powder is 1-5 μm.
[0008] In a further preferred embodiment, based on the total amount of the gallium oxide powder and the zinc oxide powder as 100 parts by mass: the mass fraction of the gallium oxide powder is 1 to 4 parts; the mass fraction of the zinc oxide powder is 96 to 99 parts; the mass fraction of the dispersant is 0.1 to 5.5 parts; and the mass fraction of the binder is 1.5 to 8.5 parts.
[0009] In a further preferred embodiment, the dispersant is one or more of polyvinyl pyrrolidone, sodium hexaalkylbenzene sulfonate, and polyacrylic acid salt; the binder is one or more of polyvinyl alcohol, polyethylene glycol, carboxymethyl cellulose, polyacrylamide, and polyacrylic acid salt.
[0010] In a further preferred embodiment, the solid content of the slurry I is 50%-70%.
[0011] In a further preferred embodiment, the slurry I is ground in a sand mill. Further preferably, the grinding speed is 750-1500 r / min and the grinding time is 4-10 h.
[0012] In a further preferred embodiment, the temperature of the spray granulation is 180°C-240°C; the spraying speed of the spray granulation is 6kg / h-20kg / h; and the atomization pressure of the spray granulation is 20-60MPa.
[0013] In a further preferred embodiment, the concentration of the acidic solution is 0.5 mol / L-2 mol / L.
[0014] In a further preferred embodiment, the acidic solution is a solution of one of acetic acid, choline chloride and malonic acid.
[0015] In a further preferred embodiment, the molded slurry II is dried by the following process: the slurry II is transferred to a mold and a uniaxial pressure of 300-600 MPa is applied at 200-500°C.
[0016] In a further preferred embodiment, the pressure of the cold isostatic pressing treatment is 100-800 MPa, and the time is 30-200 s.
[0017] In a further preferred embodiment, the process of sintering the green blank is a two-stage sintering process; the two-stage sintering process is firstly pre-sintering at 600-850°C, and then high-temperature sintering at 1000-1550°C.
[0018] In a further preferred embodiment, the heating rate of the high temperature sintering is 0.3-2°C / min, and the holding time is 2-6h.
[0019] In a further preferred embodiment, the process further comprises: a cooling process after sintering the green blank, wherein the cooling rate is preferably 0.5-2.5°C / min.
[0020] Based on the same inventive concept, the present invention provides a gallium-doped zinc oxide target prepared by the above preparation method.
[0021] Compared with the prior art, the above one or more technical solutions of the present invention can achieve one of the following beneficial effects: The preparation method of the present invention is relatively simple and uncomplicated, and has low requirements on the operation of the process steps.
[0022] The preparation method of the present invention can significantly reduce the sintering temperature.
[0023] The gallium-doped zinc oxide target material prepared by the preparation method of the present invention has a compact microstructure and a high relative density. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a picture of the target material prepared in Example 1.
[0025] Figure 2 This is a SEM image of the cross section of the target material prepared in Example 1.
[0026] Figure 3 This is a SEM image of the cross section of the target material prepared in Comparative Example 1.
[0027] Figure 4 This is the SEM image of the cross section of the target material prepared in Comparative Example 2.
[0028] Figure 5 This is the SEM image of the cross section of the target material prepared in Example 2.
[0029] Figure 6 This is the SEM image of the cross section of the target material prepared in Example 3.
[0030] Figure 7 This is a SEM image of the cross section of the target material prepared in Example 4.
[0031] Figure 8 This is the SEM image of the cross section of the target material prepared in Example 5. DETAILED DESCRIPTION
[0032] Some embodiments of the present invention provide a method for preparing a gallium-doped zinc oxide target, comprising the following steps: Gallium oxide powder and zinc oxide powder are added into deionized water containing a dispersant and a binder and dispersed to obtain slurry I; The slurry I is ground and then spray granulated to obtain granulated powder; Grinding the granulated powder in an acidic solution to obtain slurry II; After the slurry II is dried and formed, it is subjected to cold isostatic pressing to obtain a green blank; The green blank is sintered to obtain a gallium-doped zinc oxide target.
[0033] In some preferred embodiments, the concentration of the acidic solution is 0.5 mol / L-2.0 mol / L. Further preferably, the acidic solution is a solution of one of acetic acid, choline chloride and malonic acid.
[0034] In some preferred embodiments, the molded slurry II is dried by the following process: the slurry II is transferred to a mold and a uniaxial pressure of 300-600 MPa is applied at 200-500°C.
[0035] Acidic solutions will dissolve ZnO powder, but not Ga2O3. The dissolution products of ZnO powder in acidic solutions are further decomposed into ZnO under high temperature and applied pressure. For example, acetic acid solution dissolves ZnO powder to form zinc acetate, but acetic acid and Ga2O3 do not react; zinc acetate will decompose into ZnO at high temperature. The reaction process of other acids and ZnO is similar. In this process, under the dual effects of temperature and applied pressure, the powder slides and rearranges, and the decomposition product ZnO is deposited in various parts of the blank to form crystal nuclei or is swallowed by large grains, and the ZnO grains grow around the Ga2O3 particles. After complete growth, a dense microstructure is formed, which greatly improves the density of the target material.
[0036] In some preferred embodiments, the particle size D50 of the gallium oxide powder is 1-5 μm; the particle size D50 of the zinc oxide powder is 1-5 μm.
[0037] In some preferred embodiments, based on 100 parts by weight of the total amount of the gallium oxide powder and the zinc oxide powder: the mass fraction of the gallium oxide powder is 1 to 4 parts, the mass fraction of the zinc oxide powder is 96 to 99 parts; the mass fraction of the dispersant is 0.1 to 5.5 parts; and the mass fraction of the binder is 1.5 to 8.5 parts.
[0038] In some preferred embodiments, the dispersant is one or more of polyvinyl pyrrolidone, sodium hexaalkylbenzene sulfonate, and polyacrylic acid salt; the binder is one or more of polyvinyl alcohol, polyethylene glycol, carboxymethyl cellulose, polyacrylamide, and polyacrylic acid salt.
[0039] In some preferred embodiments, the solid content of the slurry I is 50%-70%.
[0040] In some preferred embodiments, the slurry I is ground in a sand mill. It is further preferred that the grinding speed is 750-1500 r / min and the grinding time is 4-10 h. The present invention does not have excessive requirements on the grinding process and the particle size distribution of the ground slurry.
[0041] In some preferred embodiments, the temperature of the spray granulation is 180° C.-240° C.; the liquid spraying rate of the spray granulation is 6 kg / h-20 kg / h; and the atomization pressure of the spray granulation is 20 MPa-60 MPa.
[0042] In some preferred embodiments, the cold isostatic pressing treatment is performed at a pressure of 100-800 MPa and for a time of 30-200 s.
[0043] In some preferred embodiments, the process of sintering the green blank is a two-stage sintering process, first pre-sintering at 600-850° C., and then high-temperature sintering at 1000-1550° C. The present invention adopts a two-stage sintering process, firstly performing low-temperature sintering, so that the powder is easier to crystallize and grow during high-temperature sintering, and the particle size distribution is more uniform.
[0044] In some preferred embodiments, the heating rate of the high temperature sintering is 0.3-2°C / min, and the holding time is 2-6h. If the heating rate is too fast, the temperature in the furnace may be uneven, which is not conducive to exhaust and may result in low density of the target material. If the heating rate is too slow, it will take too long.
[0045] In some preferred embodiments, the process further includes: a cooling process after sintering the green blank. A further preferred cooling rate is 0.5-2.5°C / min. If the cooling rate is too fast, the target material will be greatly deformed or even broken. If the cooling rate is too slow, it will take too long.
[0046] Some embodiments of the present invention also provide a gallium-doped zinc oxide target prepared by the above preparation method.
[0047] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.
[0048] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0049] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0050] Example 1 (1) Weigh 4 parts by mass of gallium oxide powder and 96 parts by mass of zinc oxide powder for later use. The particle size D50 of the gallium oxide powder is 2 μm. The particle size D50 of the zinc oxide powder is 3 μm.
[0051] (2) Deionized water, 4 parts by mass of sodium hexaalkylbenzene sulfonate, and 7 parts by mass of polyethylene glycol were added to a mixing barrel in sequence and pre-dispersed for 45 minutes to obtain slurry 1.
[0052] (3) Add the gallium oxide and zinc oxide powders weighed in step (1) to the slurry 1 in step (2), and stir and pre-disperse for 20 minutes to obtain slurry 2. The solid content in slurry 2 is controlled to be 60%.
[0053] (4) Slurry 2 was pumped into a sand mill for grinding. The grinding speed was 1200 r / min and the grinding time was 4 h to obtain slurry 3. The D50 of slurry 3 was < 0.55 μm.
[0054] (5) The slurry 3 was sent to a spray drying tower for spray granulation. The spray granulation temperature was controlled to be 200°C, the spray rate was 11kg / h, and the atomization pressure was 25MPa to obtain granulated powder.
[0055] (6) The granulated powder was placed in a mortar, and an acetic acid solution with a concentration of 1 mol / L was added for grinding to obtain slurry 4.
[0056] (7) The slurry was transferred into a mold and a uniaxial pressure of 530 MPa was applied at 400 °C for 1.5 h, followed by natural cooling to room temperature to obtain a powder.
[0057] (8) The powder is subjected to cold isostatic pressing to obtain a green blank. The cold isostatic pressing pressure is 400 MPa and the pressure is maintained for 150 seconds.
[0058] (9) The green blank was placed in a muffle furnace for pre-sintering at a temperature of 800°C for 10 hours. It was then transferred to a sintering furnace for sintering at a temperature of 1150°C. The heating rate was 2°C / min. The holding time was 5 hours. The temperature was then cooled to room temperature at a cooling rate of 1°C / min to obtain a target.
[0059] Figure 1 This is a picture of the target material obtained in Example 1. Figure 2 This is the SEM image of the cross section of the target material obtained in Example 1. It can be seen that the interior of the target material is very dense.
[0060] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that there is no step (6) and step (7). Specifically: (1) Weigh 4 parts by mass of gallium oxide powder and 96 parts by mass of zinc oxide powder for later use. The particle size D50 of the gallium oxide powder is 2 μm. The particle size D50 of the zinc oxide powder is 3 μm.
[0061] (2) Deionized water, 4 parts by mass of sodium hexaalkylbenzene sulfonate, and 7 parts by mass of polyethylene glycol were added to a mixing barrel in sequence and pre-dispersed for 45 minutes to obtain slurry 1.
[0062] (3) Add the gallium oxide and zinc oxide powders weighed in step (1) to the slurry 1 in step (2), and stir and pre-disperse for 20 minutes to obtain slurry 2. The solid content in slurry 2 is controlled to be 60%.
[0063] (4) Slurry 2 was pumped into a sand mill for grinding. The grinding speed was 1200 r / min and the grinding time was 4 h to obtain slurry 3. The D50 of slurry 3 was < 0.55 μm.
[0064] (5) The slurry 3 was sent to a spray drying tower for spray granulation. The spray granulation temperature was controlled to be 200°C, the spray rate was 11kg / h, and the atomization pressure was 25MPa to obtain granulated powder.
[0065] (6) The granulated powder is subjected to cold isostatic pressing to obtain a green blank. The pressure during cold isostatic pressing is 400 MPa and the pressure is maintained for 150 seconds.
[0066] (7) The green blank is placed in a muffle furnace for pre-sintering at a temperature of 800°C for 10 hours. It is then transferred to a sintering furnace for sintering at a temperature of 1150°C. The heating rate is 2°C / min. The holding time is 5 hours. The temperature is then cooled to room temperature at a cooling rate of 1°C / min to obtain a target.
[0067] Figure 3 This is a SEM image of the cross section of the target material obtained in Comparative Example 1. It can be seen that the target material still has a large number of interconnected pores, and the overall target material is still in a loose state between powder and sintered body, and the density is not high.
[0068] Comparative Example 2 The difference between Comparative Example 2 and Comparative Example 1 is only that the sintering temperature is different.
[0069] The sintering temperature of Comparative Example 2 is 1550°C.
[0070] Figure 4 This is a SEM image of the cross section of the target obtained in Comparative Example 2. Increasing the sintering temperature can increase the density of the target.
[0071] Example 2 (1) Weigh 3 parts by mass of gallium oxide powder and 97 parts by mass of zinc oxide powder for later use. The particle size D50 of the gallium oxide powder is 1 μm. The particle size D50 of the zinc oxide powder is 2 μm.
[0072] (2) Deionized water, 2 parts by mass of sodium hexaalkylbenzene sulfonate, and 1.5 parts by mass of polyethylene glycol were added to a mixing barrel in sequence and pre-dispersed for 30 minutes to obtain slurry 1.
[0073] (3) Add the gallium oxide and zinc oxide powders weighed in step (1) to the slurry 1 in step (2), and stir and pre-disperse for 20 minutes to obtain slurry 2. The solid content in slurry 2 is controlled to be 60%.
[0074] (4) Slurry 2 was pumped into a sand mill for grinding. The grinding speed was 1000 r / min and the grinding time was 6 h to obtain slurry 3. The D50 of slurry 3 was < 0.55 μm.
[0075] (5) The slurry 3 was sent to a spray drying tower for spray granulation. The spray granulation temperature was controlled to be 240° C., the spray rate was 16 kg / h, and the atomization pressure was 40 MPa to obtain granulated powder.
[0076] (6) The granulated powder was placed in a mortar, and an acetic acid solution with a concentration of 1.5 mol / L was added for grinding to obtain slurry 4.
[0077] (7) The slurry was transferred into a mold and a uniaxial pressure of 600 MPa was applied at 300 °C for 2 h. The mold was then naturally cooled to room temperature to obtain a powder.
[0078] (8) The powder is subjected to cold isostatic pressing to obtain a green blank. The cold isostatic pressing pressure is 600 MPa and the pressure is maintained for 100 seconds.
[0079] (9) The green blank was placed in a muffle furnace for pre-sintering at a temperature of 700°C for 12 hours. It was then transferred to a sintering furnace for sintering at a temperature of 1250°C. The heating rate was 1.5°C / min. The holding time was 4 hours. The temperature was then cooled to room temperature at a cooling rate of 2°C / min to obtain a target.
[0080] Figure 5 This is a SEM image of the cross section of the target material obtained in Example 2.
[0081] Example 3 (1) Weigh 1 part by mass of gallium oxide powder and 99 parts by mass of zinc oxide powder for later use. The particle size D50 of the gallium oxide powder is 3 μm. The particle size D50 of the zinc oxide powder is 5 μm.
[0082] (2) Deionized water, 5.5 parts by mass of sodium hexaalkylbenzene sulfonate, and 3 parts by mass of polyethylene glycol were added to a mixing barrel in sequence and pre-dispersed for 45 minutes to obtain slurry 1.
[0083] (3) Add the gallium oxide and zinc oxide powders weighed in step (1) to the slurry 1 in step (2), and stir and pre-disperse for 20 minutes to obtain slurry 2. The solid content in slurry 2 is controlled to be 70%.
[0084] (4) Slurry 2 was pumped into a sand mill for grinding. The grinding speed was 1500 r / min and the grinding time was 4 h to obtain slurry 3. The D50 of slurry 3 was < 0.55 μm.
[0085] (5) The slurry 3 was sent to a spray drying tower for spray granulation. The spray granulation temperature was controlled to be 180°C, the spray rate was 6kg / h, and the atomization pressure was 20MPa to obtain granulated powder.
[0086] (6) The granulated powder was placed in a mortar, and an acetic acid solution with a concentration of 2 mol / L was added for grinding to obtain slurry 4.
[0087] (7) The slurry was transferred into a mold and a uniaxial pressure of 600 MPa was applied at 200 °C for 1 h. The mold was then naturally cooled to room temperature to obtain a powder.
[0088] (8) The powder is subjected to cold isostatic pressing to obtain a green blank. The cold isostatic pressing pressure is 800 MPa and the pressure is maintained for 30 seconds.
[0089] (9) The green blank was placed in a muffle furnace for pre-sintering at a temperature of 600°C for 16 hours. It was then transferred to a sintering furnace for sintering at a temperature of 1350°C. The heating rate was 2°C / min. The holding time was 3 hours. The temperature was then cooled to room temperature at a cooling rate of 2°C / min to obtain a target.
[0090] Figure 6 This is a SEM image of the cross section of the target material obtained in Example 3.
[0091] Example 4 (1) Weigh 2 parts by mass of gallium oxide powder and 98 parts by mass of zinc oxide powder for later use. The particle size D50 of the gallium oxide powder is 5 μm. The particle size D50 of the zinc oxide powder is 3 μm.
[0092] (2) Deionized water, 0.1 parts by mass of sodium hexaalkylbenzene sulfonate, and 1.5 parts by mass of polyethylene glycol were added to a mixing barrel in sequence and pre-dispersed for 45 minutes to obtain slurry 1.
[0093] (3) Add the gallium oxide and zinc oxide powders weighed in step (1) to the slurry 1 in step (2), and stir and pre-disperse for 20 minutes to obtain slurry 2. The solid content in slurry 2 is controlled to be 65%.
[0094] (4) Slurry 2 was pumped into a sand mill for grinding. The grinding speed was 1000 r / min and the grinding time was 8 h to obtain slurry 3. The D50 of slurry 3 was < 0.55 μm.
[0095] (5) The slurry 3 was sent to a spray drying tower for spray granulation. The spray granulation temperature was controlled to be 200°C, the spray rate was 20kg / h, and the atomization pressure was 60MPa to obtain granulated powder.
[0096] (6) The granulated powder was placed in a mortar, and an acetic acid solution with a concentration of 0.5 mol / L was added for grinding to obtain slurry 4.
[0097] (7) The slurry was transferred into a mold and a uniaxial pressure of 600 MPa was applied at 200 °C for 1.5 h, followed by natural cooling to room temperature to obtain a powder.
[0098] (8) The powder is subjected to cold isostatic pressing to obtain a green blank. The cold isostatic pressing pressure is 400 MPa and the pressure is maintained for 150 seconds.
[0099] (9) The green blank was placed in a muffle furnace for pre-sintering at a temperature of 850°C for 8 hours. It was then transferred to a sintering furnace for sintering at a temperature of 1000°C. The heating rate was 1°C / min. The holding time was 6 hours. The temperature was then cooled to room temperature at a cooling rate of 0.5°C / min to obtain a target.
[0100] Figure 7 This is a SEM image of the cross section of the target material obtained in Example 4.
[0101] Example 5 (1) Weigh 4 parts by mass of gallium oxide powder and 96 parts by mass of zinc oxide powder for later use. The particle size D50 of the gallium oxide powder is 2 μm. The particle size D50 of the zinc oxide powder is 1 μm.
[0102] (2) Deionized water, 3 parts by mass of sodium hexaalkylbenzene sulfonate, and 5 parts by mass of polyethylene glycol were added to a mixing barrel in sequence and pre-dispersed for 45 minutes to obtain slurry 1.
[0103] (3) Add the gallium oxide and zinc oxide powders weighed in step (1) to the slurry 1 in step (2), and stir and pre-disperse for 20 minutes to obtain slurry 2. The solid content in slurry 2 is controlled to be 55%.
[0104] (4) Slurry 2 was pumped into a sand mill for grinding. The grinding speed was 750 r / min and the grinding time was 10 h to obtain slurry 3. The D50 of slurry 3 was < 0.55 μm.
[0105] (5) The slurry 3 was sent to a spray drying tower for spray granulation. The spray granulation temperature was controlled to be 220°C, the spray rate was 15kg / h, and the atomization pressure was 35MPa to obtain granulated powder.
[0106] (6) The granulated powder was placed in a mortar, and an acetic acid solution with a concentration of 1 mol / L was added for grinding to obtain slurry 4.
[0107] (7) The slurry was transferred into a mold and a uniaxial pressure of 300 MPa was applied at 500 °C for 3 h. The mold was then naturally cooled to room temperature to obtain a powder.
[0108] (8) The powder is subjected to cold isostatic pressing to obtain a green blank. The cold isostatic pressing pressure is 100 MPa and the pressure is maintained for 200 seconds.
[0109] (9) The green blank was placed in a muffle furnace for pre-sintering at a temperature of 750°C for 12 hours. It was then transferred to a sintering furnace for sintering at a temperature of 1150°C. The heating rate was 2°C / min. The holding time was 5 hours. The temperature was then cooled to room temperature at a cooling rate of 1°C / min to obtain a target.
[0110] Figure 8 This is a SEM image of the cross section of the target material obtained in Example 5.
[0111] The relative density of the target material is tested in the following way: measured by using an Archimedes drainage method solid density detector.
[0112] The relative density results of the targets obtained from test examples 1-5, comparative example 1, and comparative example 2 are shown in Table 1.
[0113] Table 1 By comparing and analyzing the relative densities of the target materials obtained in Example 1 and Comparative Example 1, it can be seen that the relative density of the target material obtained by first grinding the granulated powder in an acidic solution, then applying uniaxial pressure at high temperature, and then cold isostatic pressing and sintering will be higher, which is higher than the relative density of the target material obtained by directly cold isostatic pressing and sintering the granulated powder.
[0114] Comparative analysis of Comparative Example 1 and Comparative Example 2 shows that increasing the sintering temperature is beneficial to increasing the relative density of the target material. Comparative analysis of Example 1, Comparative Example 1 and Comparative Example 2 shows that the relative density of the target material obtained in Example 1 is higher. That is to say, the granulated powder is first ground in an acidic solution, and then uniaxial pressure is applied at a high temperature, and then cold isostatic pressing is performed and sintered at a relatively low temperature. This is a process step that can obviously improve the relative density of the target material, and this step can significantly reduce the subsequent sintering temperature. Comparative Example 2 has no steps of grinding with an acidic solution and applying uniaxial pressure at a high temperature at a higher sintering temperature. Even if the sintering temperature is 400°C higher, the relative density of the target material obtained is still lower than that of the target material obtained in Example 1.
[0115] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a gallium-doped zinc oxide target, characterized in that: The following steps are involved: Gallium oxide powder and zinc oxide powder are added into deionized water containing a dispersant and a binder and dispersed to obtain slurry I; The slurry I is ground and then spray granulated to obtain granulated powder; Grinding the granulated powder in an acidic solution to obtain slurry II; After the slurry II is dried and formed, it is subjected to cold isostatic pressing to obtain a green blank; The green blank is sintered to obtain a gallium-doped zinc oxide target.
2. The preparation method according to claim 1, characterized in that The particle size D50 of the gallium oxide powder is 1-5 μm; the particle size D50 of the zinc oxide powder is 1-5 μm; Preferably, based on 100 parts by weight of the total amount of the gallium oxide powder and the zinc oxide powder: the mass fraction of the gallium oxide powder is 1 to 4 parts, the mass fraction of the zinc oxide powder is 96 to 99 parts; the mass fraction of the dispersant is 0.1 to 5.5 parts; the mass fraction of the binder is 1.5 to 8.5 parts; Preferably, the dispersant is one or more of polyvinyl pyrrolidone, sodium hexaalkylbenzene sulfonate, and polyacrylic acid salt; the binder is one or more of polyvinyl alcohol, polyethylene glycol, carboxymethyl cellulose, polyacrylamide, and polyacrylic acid salt.
3. The preparation method according to claim 1, characterized in that: The solid content of the slurry I is 50%-70%; preferably, the slurry I is ground in a sand mill; more preferably, the grinding speed is 750-1500 r / min, and the grinding time is 4-10 h.
4. The preparation method according to claim 1, characterized in that: The temperature of the spray granulation is 180° C.-240° C.; the liquid spraying speed of the spray granulation is 6kg / h-20kg / h; and the atomization pressure of the spray granulation is 20MPa-60MPa.
5. The preparation method according to claim 1, characterized in that: The concentration of the acidic solution is 0.5 mol / L-2 mol / L; preferably, the acidic solution is a solution of one of acetic acid, choline chloride and malonic acid.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The molded slurry II is dried by the following process: the slurry II is transferred to a mold and a uniaxial pressure of 300 to 600 MPa is applied at 200 to 500°C.
7. The preparation method according to any one of claims 1 to 5, characterized in that: The cold isostatic pressing treatment is performed at a pressure of 100-800 MPa and for a time of 30-200 s.
8. The preparation method according to any one of claims 1 to 5, characterized in that: The process for sintering the green billet is a two-stage sintering process; the two-stage sintering process is first pre-sintering at 600-850°C, and then high-temperature sintering at 1000-1550°C; preferably, the heating rate of the high-temperature sintering is 0.3-2°C / min, and the holding time is 2-6h.
9. The preparation method according to any one of claims 1 to 5, characterized in that: Also includes: The cooling process after sintering the green billet; the preferred cooling rate is 0.5~2.5℃ / min.
10. Gallium-doped zinc oxide target, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Method for preparing zinc oxide-based ceramic sputtering target material at intermediate temperature
CN101885609A
Method for preparing high-conductivity zinc oxide ceramic at ultralow temperature
CN108546110A
Multicomponent doped ZnO coating material and preparation method and application thereof
CN108947518A
Ultralow-temperature cold sintering method of ZnO-based ceramic
CN109133911A
Method for preparing anisotropic bulk ferrite permanent magnet material by low-temperature sintering
CN115831577A
Cited By
Zinc oxide doped target material preparation method, target material, film preparation method and film
CN120117889A
Method for preparing zinc oxide doped target material, target material, thin film preparation method and thin film